Through the composite process of laser welding, vacuum brazing and high-frequency induction welding, combined with the shaping process, the problems of poor welding strength and large deformation of thin-walled parts are solved, and the flatness and finished product quality of water-permeable structural parts are significantly improved.
Patent Information
- Application Number
- CN202410847621.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-08
AI Technical Summary
The existing thin-walled structural parts for water flow have poor welding strength and large deformation after welding, which affects the quality of the finished product.
Three composite welding processes of laser welding, vacuum brazing and high-frequency induction welding are used, combined with the shaping process to form a multi-step processing method to reduce deformation and improve flatness.
It effectively reduces the deformation of the product, significantly improves the flatness of the water-flow structural parts, and improves the quality of the finished product.
Smart Images

Figure CN118744292A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of parts processing, and in particular to a processing method for a water-passing structural part. Background Art
[0002] Reference Figure 1 to Figure 2 As shown, the water-passing structural member mainly includes a thin-wall frame 1, a thin-wall bracket 2, a pipe body 3 and a joint assembly 4. Among them, the thin-wall frame 1 and the thin-wall bracket 2 are made of stainless steel, the thickness of a single thin-wall bracket 2 is 1.5 mm, the pipe body 3 is made of copper, and the joint assembly 4 is made of stainless steel. The thin-wall bracket 2 is fixed on the thin-wall frame 1, the pipe body 3 is fixed on the thin-wall bracket 2, and the joint assembly 4 is fixed on the pipe body 3.
[0003] In the prior art, the components of the water-passing structural parts are currently connected by welding. However, since it involves welding of thin-walled parts and welding of dissimilar metals, the welding strength is poor, the deformation after welding is large, and the product flatness is poor, which affects the quality of the finished water-passing structural parts. Summary of the invention
[0004] The object of the present invention is to provide a processing method for water-passing structural parts, which adopts a variety of welding processes and cooperates with a shaping process to effectively reduce the deformation of the product and effectively improve the flatness of the product.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] A method for processing a water-passing structural member, used for processing the water-passing structural member, the water-passing structural member comprises a thin-wall frame, a thin-wall bracket, a pipe body and a joint assembly, and the method for processing the water-passing structural member comprises the following steps:
[0007] S100, cleaning the thin-wall frame, the thin-wall bracket and the tube body;
[0008] S200, placing the thin-walled bracket in the thin-walled frame and performing laser welding on the thin-walled frame to form a first semi-finished component after welding;
[0009] S300, shaping and cleaning the first semi-finished product;
[0010] S400, placing the tube body on the thin-walled support and performing vacuum brazing on the thin-walled support to form a second semi-finished part after welding;
[0011] S500, shaping the second semi-finished product;
[0012] S600, placing the joint assembly on the pipe body and performing high-frequency induction welding with the pipe body to form the water-passing structural member after welding.
[0013] Preferably, in step S100, a hydrofluoric acid solution is used to clean the thin-wall frame, the thin-wall bracket and the tube body, the concentration of the hydrofluoric acid solution is 10%-15%, and the cleaning time is 15s-30s.
[0014] Preferably, between step S100 and step S200, the step further includes: vacuum drying the thin-wall frame and the thin-wall bracket.
[0015] Preferably, in step S200, the welding speed is 0.11 mm / s-0.13 mm / s, the weld width is less than 0.05 mm, the welding gun power is 2.5 Kw-2.6 Kw, and argon is used as the shielding gas.
[0016] Preferably, in step S300, a hydraulic shaping machine is used to shape the first semi-finished component so that the flatness of the first semi-finished component is less than 0.5 mm.
[0017] Preferably, in step S300, the first semi-finished component is cleaned with a hydrofluoric acid solution, the concentration of the hydrofluoric acid solution is 10%-15%, and the cleaning time is 15s-30s.
[0018] Preferably, between step S300 and step S400, the step further includes: vacuum drying the first semi-finished component and the tube body.
[0019] Preferably, in step S400, the welding vacuum degree is ≤3.0×10 -3 Pa, welding temperature is 1100℃-1150℃, applied pressure is 10MPa, welding time is 180min-200min.
[0020] Preferably, in step S500, a hydraulic shaping machine is used to shape the second semi-finished component so that the flatness of the second semi-finished component is less than 0.5 mm.
[0021] Preferably, in step S600, the operating frequency of the high frequency generator is 300kHz-450kHz, the generated current is 200A-250A, and the time is 5s-8s.
[0022] Beneficial effects:
[0023] The processing method for a water-passing structural member provided by the present invention first cleans the thin-walled frame, the thin-walled bracket and the tube body. Then, the thin-walled bracket is placed in the thin-walled frame and laser welded with the thin-walled frame. The thin-walled bracket and the thin-walled frame are welded and fixed to form a first semi-finished member. Then, the first semi-finished member is shaped and cleaned to ensure the reliable flatness of the first semi-finished member itself, and to wash away the debris during the welding process. Next, the tube body is placed on the thin-walled bracket of the first semi-finished member and vacuum brazed with the thin-walled bracket. The tube body and the first semi-finished member are welded and fixed to form a second semi-finished member. Then, the second semi-finished member is shaped to ensure the reliable flatness of the second semi-finished member itself. Next, the joint assembly is placed on the tube body and high-frequency induction welded to the tube body. Finally, the water-passing structural member is formed after welding and fixing. The above method adopts three composite welding process forms of laser welding, vacuum brazing, and high-frequency induction welding, and cooperates with the shaping process, which can effectively reduce the deformation of the product and effectively improve the flatness of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a structural schematic diagram of a water-passing structural member used in the present invention from one perspective;
[0025] Figure 2 It is a structural schematic diagram of the water-passing structural member used in the present invention from another perspective;
[0026] Figure 3 It is a schematic flow chart of the processing method for water-passing structural parts provided by the present invention.
[0027] In the figure:
[0028] 1. Thin-wall frame; 2. Thin-wall bracket; 3. Tube body; 4. Joint assembly. DETAILED DESCRIPTION
[0029] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0030] In the description of the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0031] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0032] In the description of this embodiment, the terms "upper", "lower", "right", etc., directions or positional relationships are based on the directions or positional relationships shown in the drawings, and are only for the convenience of description and simplification of operation, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used to distinguish in the description and have no special meaning.
[0033] Reference Figures 1 to 3 As shown, this embodiment provides a processing method for a water-passing structural member.
[0034] The processing method for water-passing structural parts is applied to the processing of water-passing structural parts. The water-passing structural parts include a thin-wall frame 1, a thin-wall bracket 2, a pipe body 3 and a joint assembly 4. The processing method for water-passing structural parts includes the following steps:
[0035] S100, cleaning the thin-wall frame 1, the thin-wall support 2 and the tube body 3;
[0036] S200, placing the thin-walled bracket 2 in the thin-walled frame 1 and laser welding the thin-walled frame 1 to form a first semi-finished component after welding;
[0037] S300, shaping and cleaning the first semi-finished product;
[0038] S400, placing the tube body 3 on the thin-walled support 2 and performing vacuum brazing on the thin-walled support 2 to form a second semi-finished component after welding;
[0039] S500, shaping the second half-finished product;
[0040] S600, placing the joint assembly 4 on the pipe body 3 and performing high-frequency induction welding with the pipe body 3 to form a water-permeable structural member after welding.
[0041] In this embodiment, the above-mentioned processing method for water-passing structural parts is adopted, and the thin-walled frame 1, the thin-walled bracket 2 and the tube body 3 are first cleaned. Then the thin-walled bracket 2 is placed in the thin-walled frame 1 and laser welded with the thin-walled frame 1. The thin-walled bracket 2 and the thin-walled frame 1 are welded and fixed to form a first semi-finished part. Then the first semi-finished part is shaped and cleaned to ensure the reliable flatness of the first semi-finished part itself, and to wash away the debris during the welding process. Next, the tube body 3 is placed on the thin-walled bracket 2 of the first semi-finished part and vacuum brazed with the thin-walled bracket 2. The tube body 3 and the first semi-finished part are welded and fixed to form a second semi-finished part. Then the second semi-finished part is shaped to ensure the reliable flatness of the second semi-finished part itself. Next, the joint assembly 4 is placed on the tube body 3 and high-frequency induction welded to the tube body 3, and finally welded and fixed to form a water-passing structural part. The above method adopts three composite welding process forms of laser welding, vacuum brazing, and high-frequency induction welding, and cooperates with the shaping process, which can effectively reduce the deformation of the product and effectively improve the flatness of the product.
[0042] In the present embodiment, in step S100, hydrofluoric acid solution is used to clean the thin-walled frame 1, the thin-walled support 2 and the tube body 3, the concentration of the hydrofluoric acid solution is 10%-15%, and the cleaning time is 15s-30s. Specifically, hydrofluoric acid can react with the oxide on the metal surface to generate soluble metal fluorides. These metal fluorides can be dissolved quickly, thereby removing the oxide layer on the metal surface. In addition, hydrofluoric acid is also corrosive and can dissolve impurities and pollutants on the metal surface. During the pickling process, hydrofluoric acid reacts with the impurities on the metal surface to form soluble metal fluorides or fluoride complexes, thereby effectively and comprehensively removing these impurities from the metal surface. In addition, hydrofluoric acid can also provide a certain corrosion inhibition effect during the pickling process. Thereby forming a protective film on the metal surface to prevent further corrosion of the metal surface by hydrofluoric acid.
[0043] In this embodiment, between step S100 and step S200, it also includes: vacuum drying the thin-walled frame 1 and the thin-walled bracket 2. Specifically, before laser welding, the thin-walled frame 1 and the thin-walled bracket 2 must be dried. Using vacuum drying equipment, applying the vacuum drying principle, and utilizing the low temperature environment under a vacuum state, the moisture in the thin-walled frame 1 and the thin-walled bracket 2 exists in the form of ice crystals, and then the ice crystals are directly sublimated into water vapor by heating, thereby achieving fast and reliable drying of the thin-walled frame 1 and the thin-walled bracket 2. Since the thin-walled frame 1 and the thin-walled bracket 2 are in a low temperature state during the vacuum freeze-drying process, deformation, cracking and other problems that may occur during the traditional hot air drying process can be avoided.
[0044] In this embodiment, during the laser welding process, the laser welding parameters are: welding speed is 0.11mm / s-0.13mm / s, weld width is less than 0.05mm, welding gun power is 2.5Kw-2.6Kw, and argon is used as the shielding gas.
[0045] In this embodiment, in step S300, a hydraulic shaping machine is used to shape the first semi-finished part so that the flatness of the first semi-finished part is less than 0.5 mm. Specifically, the working principle of the hydraulic shaping machine is that the hydraulic shaping machine realizes shape processing by controlling the change of oil pressure. When working, the hydraulic system will provide a certain oil pressure force to make the mold on the workbench move up and down, so as to achieve the purpose of shape processing. The hydraulic shaping machine has the advantages of high processing accuracy, high processing efficiency, and easy operation, and has strong adaptability. It can adapt to different materials and shape processing requirements and can process various types of parts.
[0046] In this embodiment, in step S300, the first semi-finished component is cleaned with a hydrofluoric acid solution, the concentration of the hydrofluoric acid solution is 10%-15%, and the cleaning time is 15s-30s.
[0047] In this embodiment, between step S300 and step S400 , the step further includes: vacuum drying the first semi-finished component and the tube body 3 .
[0048] In this embodiment, during the vacuum brazing process, the vacuum brazing parameters are: welding vacuum degree ≤ 3.0×10 -3 Pa, welding temperature is 1100℃-1150℃, applied pressure is 10MPa, welding time is 180min-200min.
[0049] In this embodiment, in step S500, a hydraulic shaping machine is used to shape the second semi-finished component so that the flatness of the second semi-finished component is less than 0.5 mm.
[0050] In this embodiment, during the high-frequency induction welding, the welding parameters are: the operating frequency of the high-frequency generator is 300kHz-450kHz, the generated current is 200A-250A, and the time is 5s-8s.
[0051] In summary, the processing method for water-passing structural parts provided in this embodiment adopts a variety of welding processes and cooperates with a shaping process, which can effectively reduce the deformation of the product and effectively improve the flatness of the product.
[0052] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, various obvious changes, readjustments and substitutions can be made without departing from the protection scope of the present invention. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for processing a water-passing structural member, for processing a water-passing structural member, wherein the water-passing structural member comprises a thin-wall frame (1), a thin-wall bracket (2), a tube body (3) and a joint assembly (4), characterized in that: The processing method for the water-passing structural member comprises the following steps: S100, cleaning the thin-wall frame (1), the thin-wall support (2) and the tube body (3); S200, placing the thin-walled bracket (2) in the thin-walled frame (1) and performing laser welding with the thin-walled frame (1), so as to form a first semi-finished component after welding; S300, shaping and cleaning the first semi-finished product; S400, placing the tube body (3) on the thin-walled support (2) and performing vacuum brazing with the thin-walled support (2), so as to form a second semi-finished component after welding; S500, shaping the second semi-finished product; S600, placing the joint assembly (4) on the pipe body (3) and performing high-frequency induction welding with the pipe body (3), so as to form the water-passing structural component after welding.
2. The processing method for water-passing structural parts according to claim 1, characterized in that: In step S100, the thin-wall frame (1), the thin-wall bracket (2) and the tube body (3) are cleaned using a hydrofluoric acid solution, the concentration of the hydrofluoric acid solution is 10%-15%, and the cleaning time is 15s-30s.
3. The processing method for a water-passing structural member according to claim 1, characterized in that: The step between step S100 and step S200 also includes: vacuum drying the thin-wall frame (1) and the thin-wall support (2).
4. The processing method for a water-passing structural member according to claim 1, characterized in that: In step S200, the welding speed is 0.11 mm / s-0.13 mm / s, the weld width is less than 0.05 mm, the welding gun power is 2.5 Kw-2.6 Kw, and argon is used as the shielding gas.
5. The processing method for water-passing structural parts according to claim 1, characterized in that: In step S300, a hydraulic shaping machine is used to shape the first semi-finished component so that the flatness of the first semi-finished component is less than 0.5 mm.
6. The processing method for a water-passing structural member according to claim 1, characterized in that: In step S300, the first semi-finished component is cleaned with a hydrofluoric acid solution, the concentration of the hydrofluoric acid solution is 10%-15%, and the cleaning time is 15s-30s.
7. The processing method for a water-passing structural member according to claim 1, characterized in that: The step between step S300 and step S400 also includes: vacuum drying the first semi-finished component and the tube body (3).
8. The processing method for a water-passing structural member according to claim 1, characterized in that: In step S400, the welding vacuum degree is ≤3.0×10 -3 Pa, welding temperature is 1100℃-1150℃, applied pressure is 10MPa, welding time is 180min-200min.
9. The processing method for a water-passing structural member according to claim 1, characterized in that: In step S500, the second semi-finished part is shaped by using a hydraulic shaping machine so that the flatness of the second semi-finished part is less than 0.5 mm.
10. The processing method for a water-passing structural member according to claim 1, characterized in that: In step S600, the operating frequency of the high frequency generator is 300kHz-450kHz, the generated current is 200A-250A, and the time is 5s-8s.