Preformed composite metal foil brazing filler metal and preparation method thereof

By using preformed composite metal foil solder in aluminum alloy connectors, the low ignition point of magnesium foil is used to stimulate thermite reaction, reduce the brazing temperature and enhance the sealing of solder joints, solving the problem of high temperature problems in the existing technology for aluminum alloy connectors. It reduces the problems of damage and air leakage and achieves brazing effect with lower energy consumption.

CN118744294AActive Publication Date: 2024-10-08SOLDERWELL MICROELECTRONIC PACKAGING MATERIALS CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410852903.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-08
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

When brazing aluminum alloy connectors with existing aluminum-based brazing materials, the high temperature causes overheating damage to heat-resistant parts, air leakage and high energy consumption, making it difficult to effectively reduce the brazing temperature and leakage rate.

Method used

Preformed composite metal foil solder is used, and magnesium foil is used as a carrier to deposit oxidized copper foil, aluminum foil and nickel foil layers. The heat with low ignition point of magnesium is used to stimulate the aluminothermic reaction, reduce the brazing temperature, and form the aluminum and copper oxide foil. Intermetallic compounds or solid solutions realize connection and enhance the strength and sealing effect of solder joints.

Benefits of technology

Effectively lowers the brazing temperature to just over 500°C, reduces leakage rate, prevents overheating damage to aluminum alloy connectors, improves the sealing effect of solder joints, and reduces brazing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004917283150000081
    Figure BDA0004917283150000081
  • Figure BDA0004917283150000091
    Figure BDA0004917283150000091
Patent Text Reader

Abstract

The invention discloses preformed composite metal foil brazing filler metal and a preparation method thereof, and relates to the technical field of brazing. The composite metal foil brazing filler metal comprises a carrier and a plurality of composite foil layers, the composite foil layers are stacked and deposited on the surface of the carrier, each composite foil layer comprises an oxidized copper foil, an aluminum foil and a nickel foil which are sequentially stacked and deposited in the direction away from the carrier, and the carrier is a magnesium foil. The adopted magnesium foil has the advantage of low ignition point, heat generated by igniting the magnesium foil can excite the oxidized copper foil and the aluminum foil to generate a thermit reaction, aluminum, the nickel foil and copper generate an intermetallic compound or a solid solution through the high temperature of the thermit reaction, brazing connection is achieved, the brazing temperature is low, and the brazing temperature is 500 DEG C; the heat-labile part of the aluminum alloy connecting piece can be prevented from being damaged due to overheating, the brazing temperature and the leakage rate are reduced, and the sealing effect is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of brazing, and in particular to a preformed composite metal foil brazing material and a preparation method thereof. Background Art

[0002] Brazing refers to a brazing method in which the solder and the connector are heated to the melting temperature of the solder at the same time, and the gap of the connector is filled with liquid solder to interconnect the connectors. Aluminum alloys have been increasingly widely used in aviation, aerospace, electricity, electronics, automobiles, and ships due to their good thermal and electrical conductivity and corrosion resistance. Therefore, the connection of aluminum alloys and their processing technology play a very important role in product manufacturing. There are many ways to connect aluminum alloys, among which brazing has many advantages such as no melting of the base material, low working temperature, smooth and beautiful joints, small welding deformation, high dimensional accuracy of welded parts, and the ability to connect different materials.

[0003] Generally speaking, the melting point of aluminum alloy is basically lower than the melting point of pure aluminum, 660°C, and is generally between 607°C and 650°C. However, the aluminum-based brazing filler metal currently used for brazing aluminum alloys, such as the commonly used aluminum silicon brazing filler metal, has a melting point of 577°C, and the brazing temperature usually needs to be 25°C higher than the melting point of the brazing filler metal, that is, the brazing temperature needs to be at least 600°C. Such a high brazing temperature, which is close to the melting point of the aluminum alloy, when the aluminum-based brazing filler metal and the aluminum alloy connector are heated at the same time to melt the aluminum-based brazing filler metal and then braze the aluminum alloy connector, the excessively high brazing temperature can easily cause the local heat-sensitive parts of the aluminum alloy connector to be overheated and damaged, resulting in air leakage, and the energy consumption of the brazing process is high. Summary of the invention

[0004] The present invention provides a preformed composite metal foil brazing filler metal and a preparation method thereof. By stimulating thermite reaction, local brazing can be initiated at a relatively low temperature, thereby reducing the brazing temperature and leakage rate, thereby solving the problem of overheating and damage of heat-sensitive parts and resulting in air leakage when brazing aluminum alloy connectors with aluminum-based brazing fillers.

[0005] In order to solve the above technical problems, one of the objectives of the present invention is to provide a preformed composite metal foil solder, including a carrier and a plurality of composite foil layers, wherein the plurality of composite foil layers are stacked and deposited on the surface of the carrier, the composite foil layers include copper oxide foil, aluminum foil and nickel foil stacked and deposited in sequence in a direction away from the carrier, and the carrier is magnesium foil.

[0006] By adopting the above scheme, the brazing material of the present invention needs to further reduce the brazing temperature under the premise of ensuring a low leakage rate. By taking advantage of the low ignition point of magnesium at 490°C, the magnesium foil is ignited at a relatively low temperature during brazing. The heat generated causes the oxidized copper foil and the aluminum foil to produce a thermite reaction. The high temperature released by the thermite reaction further causes the aluminum, the nickel foil and the copper generated by the thermite reaction to form an intermetallic compound or a solid solution, thereby achieving the purpose of brazing connection. The aluminum foil is located between the oxidized copper foil and the nickel foil, which facilitates the thermite reaction of the aluminum foil and the oxidized copper foil, and also facilitates the aluminum to fuse with the adjacent nickel foil using the heat generated by the thermite reaction. The nickel-aluminum alloy formed by nickel and aluminum has excellent anti-aging performance, is beneficial to improving the strength of the solder joint, enhancing the sealing effect of the solder joint, reducing the risk of leakage, and ultimately effectively reducing the brazing temperature to prevent the aluminum alloy connector from being damaged by overheating and leaking.

[0007] As a preferred solution, the thickness of each layer of the copper oxide foil, aluminum foil and nickel foil is independent and is 150-700 nm.

[0008] By adopting the above scheme, the present invention controls the thickness of the oxidized copper foil, aluminum foil and nickel foil within a specific range, which can reduce the brazing temperature and leakage rate. Since each operation of the magnetron sputtering equipment requires many preparation steps before sputtering, such as vacuuming and cleaning, if the thickness of the oxidized copper foil, aluminum foil and nickel foil is too small, then a corresponding composite metal foil of the same thickness is required, and the preparation time for magnetron sputtering is too long. At the same time, if the thickness of each layer of the oxidized copper foil, aluminum foil and nickel foil is too large, it will affect the progress of the aluminum heat reaction during brazing, and also affect the full contact of aluminum, copper and nickel to form intermetallic compounds or solid solutions to achieve the purpose of brazing connection.

[0009] As a preferred embodiment, the thickness of each layer of the copper oxide foil, aluminum foil and nickel foil is independent and is 300nm-500nm.

[0010] As a preferred solution, the thickness ratio of each layer of the aluminum foil and the copper oxide foil is ≥ 1 / 2.

[0011] By adopting the above scheme, the mass ratio of aluminum to copper oxide for complete reaction is 9:40. After density and volume conversion, the thickness ratio of aluminum foil and copper oxide foil required for complete reaction of aluminum and copper oxide is 1:2. Moreover, the copper and nickel generated by the reaction of aluminum and copper oxide are infinitely solid-soluble, which is beneficial to brazing. If there is excess aluminum after the reaction, it can form intermetallic compounds with nickel, which is beneficial to brazing. Therefore, ensuring that the mass of aluminum foil participating in the reaction is sufficient can reduce the brazing temperature and leakage rate.

[0012] As a preferred solution, the thickness ratio of each layer of the aluminum foil and the copper oxide foil is ≥5 / 3.

[0013] As a preferred solution, the thickness of the carrier is 2-4 μm.

[0014] By adopting the above scheme, the present invention controls the thickness of the carrier within a specific range, which can reduce the brazing temperature and leakage rate. If the thickness of the carrier is too thin, the manufacturing cost will be too high, and the heat generated by the small mass is not enough to trigger thermite reaction; if the thickness of the carrier is too thick, it is not easy to ignite on the one hand, and on the other hand, the magnesium foil is too thick and the magnesium oxide slag generated after ignition will be too much, affecting the brazing quality.

[0015] As a preferred solution, the composite foil layer is away from the carrier and the side facing away from the carrier is coated with aluminum brazing flux.

[0016] By adopting the above scheme, the aluminum brazing flux can break the oxide film on the surface of the aluminum alloy brazing parts, increase the activity of aluminum, and push the oxide slag generated during the brazing process to the periphery of the weld to ensure the brazing quality of the weld.

[0017] As a preferred solution, the mass of the aluminum brazing agent accounts for 5-10% of the total mass of the composite metal foil brazing material.

[0018] As a preferred embodiment, the aluminum brazing flux is cesium fluoroaluminate.

[0019] In order to solve the above technical problems, the second object of the present invention is to provide a method for preparing a preformed composite metal foil solder, comprising the following steps:

[0020] S1. Depositing copper oxide foil, aluminum foil and nickel foil in sequence on a carrier by a magnetron sputtering method to form a composite foil layer, repeatedly depositing multiple composite foil layers, and finally ending with aluminum foil or nickel foil until a desired thickness is obtained;

[0021] S2. The composite foil layer is away from the carrier and the aluminum brazing agent is applied to the side facing away from the carrier to obtain a preformed composite metal foil brazing material.

[0022] As a preferred solution, in S1, the carrier is preliminarily cleaned with deionized water, anhydrous ethanol, and acetone ultrasonically and then blown dry.

[0023] As a preferred solution, in S1, the purity of the target material used for magnetron sputtering is above 99.95%.

[0024] As a preferred solution, in S1, the sputtering gas pressure of magnetron sputtering is 0.5-1 Pa, the sputtering power is 100-250 W, and the argon gas flow rate is 35-50 ml / min.

[0025] As a preferred solution, in S2, the composite metal foil brazing material can be cut into a required size as needed before or after the aluminum brazing agent is applied.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention uses magnesium foil as a carrier, and its ignition point is as low as 490°C. The heat generated by igniting the magnesium foil can stimulate the oxidized copper foil and the aluminum foil to undergo thermite reaction. The aluminum foil is located between the oxidized copper foil and the nickel foil. The high temperature of the thermite reaction causes the aluminum and nickel foils as well as the copper produced by the thermite reaction to generate intermetallic compounds or solid solutions, thereby achieving brazing connection. The brazing temperature is as low as just over 500°C. The low brazing temperature can prevent overheating damage to heat-sensitive parts of aluminum alloy connectors and reduce the leakage rate.

[0028] 2. The aluminum foil is located between the copper oxide foil and the nickel foil, which is convenient for the aluminum foil and the copper oxide foil to undergo thermite reaction, and also convenient for the aluminum to fuse with the adjacent nickel foil using the heat generated by the thermite reaction. The nickel-aluminum alloy formed by nickel and aluminum has excellent anti-aging properties, which is beneficial to improve the strength of the solder joint, enhance the sealing effect of the solder joint, reduce the risk of leakage, and ultimately effectively reduce the brazing temperature to prevent the aluminum alloy connector from overheating and damage and leakage.

[0029] 3. The composite metal foil brazing material of the present invention is pre-coated with aluminum brazing flux. Compared with the method of dipping liquid aluminum brazing flux during the brazing process, the amount of aluminum brazing flux can be precisely controlled without causing excessive splashing of the aluminum brazing flux. The aluminum brazing flux can break the oxide film on the surface of the aluminum alloy brazing parts, increase the activity of aluminum, and push the oxide slag generated during the brazing process to the vicinity of the weld, thereby ensuring the brazing quality of the weld. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] A preformed composite metal foil solder comprises a carrier and a plurality of composite foil layers stacked, wherein the plurality of composite foil layers are deposited on the upper surface of the carrier, the composite foil layers comprise copper oxide foil, aluminum foil and nickel foil stacked in sequence from bottom to top, the carrier is magnesium foil, i.e., multiple layers of copper oxide foil, aluminum foil and nickel foil are alternately deposited in sequence on the magnesium foil, the thickness of the magnesium foil carrier is 4 μm, the thickness of each layer of aluminum foil is 500 nm, the thickness of each layer of copper oxide foil is 300 nm, the thickness of each layer of nickel foil is 300 nm, i.e., the thickness ratio of the aluminum foil to the copper oxide foil is 5:3, the total thickness of the metal layer of the composite metal foil is about 50 μm, the composite metal foil is in a circular ring sheet structure, the dimensions are 10 mm in inner diameter and 16 mm in outer diameter, the composite foil layer is away from the carrier and the side facing away from the carrier is pre-coated with cesium aluminum fluoroaluminate solder, and the mass of the cesium aluminum fluoroaluminate solder accounts for 10% of the total mass of the composite metal foil.

[0033] The method for preparing the preformed composite metal foil solder comprises the following steps:

[0034] S1, a magnesium foil with a thickness of 4 μm is cleaned with deionized water, anhydrous ethanol, and acetone ultrasonically in sequence and then blown dry to serve as a carrier for depositing metal foil;

[0035] S2. Depositing copper oxide foil on a magnesium foil carrier by magnetron sputtering, and then depositing aluminum foil and nickel foil in sequence on this basis, the purity of the copper oxide target, aluminum target and nickel target used for depositing the copper oxide foil, aluminum foil and nickel foil is more than 99.95%, the sputtering pressure of magnetron sputtering is 1.0 Pa, the sputtering power is 250 W, and the argon gas flow rate is 50 ml / min;

[0036] S3, repeating step S2 to alternately deposit multiple layers of copper oxide foil, aluminum foil and nickel foil, and finally ending with nickel foil, until a composite foil layer with a thickness of about 50 μm is obtained;

[0037] S4, cutting the composite metal foil into circular ring pieces with an outer diameter of 16 mm and an inner diameter of 10 mm as required;

[0038] S5. Pre-coating cesium aluminum fluoroaluminate brazing flux on the side of the composite foil layer away from the magnesium foil and opposite to the magnesium foil to obtain a preformed composite metal foil brazing material.

[0039] Example 2

[0040] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of aluminum foil is 300 nm, that is, the ratio of the thickness of the aluminum foil to the thickness of the copper oxide foil is 1:1.

[0041] Example 3

[0042] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of aluminum foil is 150 nm, that is, the thickness ratio of the aluminum foil to the copper oxide foil is 1:2.

[0043] Example 4

[0044] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of aluminum foil is 700 nm, that is, the thickness ratio of the aluminum foil to the copper oxide foil is 7:3.

[0045] Example 5

[0046] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of copper oxide foil is 500 nm, that is, the ratio of the thickness of the aluminum foil to the copper oxide foil is 1:1.

[0047] Example 6

[0048] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of copper oxide foil is 150 nm, that is, the thickness ratio of the aluminum foil to the copper oxide foil is 10:3.

[0049] Example 7

[0050] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of copper oxide foil is 700 nm, that is, the thickness ratio of the aluminum foil to the copper oxide foil is 5:7.

[0051] Example 8

[0052] A preformed composite metal foil solder, which differs from Example 1 in that the thickness of each layer of aluminum foil is 150 nm, and the thickness of each layer of copper oxide foil is 450 nm, that is, the thickness ratio of the aluminum foil to the copper oxide foil is 1:3.

[0053] Example 9

[0054] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of aluminum foil is 900 nm, that is, the thickness ratio of the aluminum foil to the copper oxide foil is 3:1.

[0055] Example 10

[0056] A preformed composite metal foil solder is different from Example 1 in that the thickness of each layer of copper oxide foil is 1200 nm, that is, the thickness ratio of the aluminum foil to the copper oxide foil is 5:12.

[0057] Embodiment 11

[0058] A preformed composite metal foil solder, which differs from Example 1 in that the thickness of each layer of copper oxide foil is 900 nm, and the thickness ratio of the aluminum foil to the copper oxide foil is 5:9.

[0059] Example 12

[0060] A preformed composite metal foil solder, which differs from Example 1 in that the thickness of each layer of nickel foil is 500 nm.

[0061] Embodiment 13

[0062] A preformed composite metal foil solder, which differs from Example 1 in that the thickness of each layer of nickel foil is 150 nm.

[0063] Embodiment 14

[0064] A preformed composite metal foil solder, which differs from Example 1 in that the thickness of each layer of nickel foil is 700 nm.

[0065] Embodiment 15

[0066] A preformed composite metal foil solder, which differs from Example 1 in that the thickness of each layer of nickel foil is 1000 nm.

[0067] Example 16

[0068] A preformed composite metal foil solder is different from Example 1 in that the thickness of the magnesium foil carrier is 2 μm.

[0069] Embodiment 17

[0070] A preformed composite metal foil solder is different from Example 1 in that the thickness of the magnesium foil carrier is 1 μm.

[0071] Embodiment 18

[0072] A preformed composite metal foil solder is different from Example 1 in that the thickness of the magnesium foil carrier is 8 μm.

[0073] Comparative Example 1

[0074] A preformed composite metal foil solder, which differs from Example 1 in that the carrier is tin foil.

[0075] Comparative Example 2

[0076] A preformed composite metal foil solder, which differs from Example 1 in that the composite foil layer comprises aluminum foil, copper oxide foil and nickel foil stacked in sequence from bottom to top, that is, multiple layers of aluminum foil, copper oxide foil and nickel foil are alternately deposited in sequence on magnesium foil.

[0077] Comparative Example 3

[0078] A preformed composite metal foil brazing material, which differs from Example 1 in that cobalt foil of equal thickness is used instead of nickel foil.

[0079] Comparative Example 4

[0080] The invention discloses an aluminum alloy brazing filler metal, which is made of commercially available Al88Si12 brazing filler metal, has a total thickness of 50 μm, is in a circular ring sheet structure, has an inner diameter of 10 mm and an outer diameter of 16 mm, and is coated with cesium aluminum fluoroaluminate brazing flux on the surface of the brazing filler metal, wherein the mass of the cesium aluminum fluoroaluminate brazing flux accounts for 10% of the total mass.

[0081] Performance testing

[0082] In order to further verify the performance of the preformed composite metal foil of the present invention, the composite metal foil brazing materials in Examples 1-18 and Comparative Examples 1-3 were used as the test group, and the brazing material in Comparative Example 4 was used as the control group. Brazing tests were carried out respectively, and the sealing device was assembled with the brazing materials in the test group and the control group, respectively, and laser brazing was carried out. The brazing materials in the test group and the control group were both circular ring sheets with an inner diameter of 10 mm, an outer diameter of 16 mm, and a thickness of 50 μm, and the following tests were carried out:

[0083] 1) Record the temperature range required for brazing. The temperature range required for brazing is measured with an infrared temperature detector. The lower the temperature, the easier it is to achieve a good brazing sealing effect. The test results are shown in Table 1.

[0084] 2) After brazing is completed, a sealing leakage test is performed. The sealing leakage test is performed using a helium mass spectrometer leak detector. The test standard is QJ3212-2005 "Helium Mass Spectrometer Back Pressure Leak Detection Method". The smaller the leakage rate, the better the sealing effect. The test results are shown in Table 1.

[0085] Table 1 Brazing performance test of solders of the embodiments of the present invention and comparative examples

[0086]

[0087]

[0088] From the comparison of the performance test results of Example 1 of the present invention and Comparative Example 4 in Table 1, it can be seen that since magnesium has the advantage of a low ignition point of 490°C, the heat generated by igniting the magnesium foil at a relatively low temperature during brazing stimulates the oxidized copper foil and the aluminum foil to produce a thermite reaction. The high temperature released by the thermite reaction further causes the aluminum and nickel foil and the copper generated by the thermite reaction to form an intermetallic compound or a solid solution, thereby achieving the purpose of brazing connection. The present invention only needs to apply a temperature as low as 500°C to the weld to achieve the purpose of burning the brazing material and connecting the aluminum alloy connector; while the aluminum-silicon brazing material used in Comparative Example 4 has a brazing temperature of more than 600°C, which is close to the melting point of the aluminum alloy connector, and is very likely to cause local heat resistance and damage to the aluminum alloy connector. The local damage leads to a significantly higher leakage rate, and the energy consumption of brazing is high.

[0089] From the comparison of the performance test results of Example 1 of the present invention and Comparative Example 3 in Table 1, it can be seen that Example 1 of the present invention utilizes the heat generated by the thermite reaction to promote the fusion of aluminum and the adjacent nickel foil. The formed nickel-aluminum alloy has excellent anti-aging performance, which is beneficial to improving the strength of the solder joint, enhancing the sealing effect of the solder joint, and reducing the risk of leakage.

[0090] By comparing the performance test results of Example 1 of the present invention and Comparative Example 2 in Table 1, it can be seen that in Comparative Example 2, since aluminum foil is first plated on the magnesium foil, when the magnesium foil is ignited, the aluminum foil is easily oxidized to aluminum oxide first. Due to the presence of other components, part of the thermite reaction cannot be completely carried out, the brazing temperature is relatively high, and the leakage rate is also increased; while in the present invention, copper oxide foil, aluminum foil and nickel foil are first deposited on the magnesium foil in sequence. The temperature generated when the magnesium foil is ignited can trigger the thermite reaction between the copper oxide foil and the aluminum foil, thereby achieving the purpose of reducing the brazing temperature and the leakage rate.

[0091] From the comparison of the performance test results of Examples 1, 16-18 of the present invention in Table 1, it can be seen that the lower or higher thickness of the carrier magnesium foil affects the brazing temperature and leakage rate. If the thickness of the magnesium foil is too thin, the manufacturing cost is too high, and the heat generated due to the small mass is too little to trigger the thermite reaction; if the thickness of the magnesium foil is too thick, on the one hand, it is not easy to ignite, and on the other hand, too much magnesium oxide slag will be generated after ignition, affecting the brazing quality. The thickness of the magnesium foil in Examples 1 and 16 is in the range of 2-4 μm, so that the brazing temperature and leakage rate of the solder are relatively low.

[0092] From the comparison of the performance test results of Example 1 of the present invention and Comparative Example 1 in Table 1, it can be seen that since the magnesium foil of the present invention can burn and generate heat at a low ignition point of 490°C, it can stimulate thermite reaction, while the tin foil of Comparative Example 1 will not burn, but will only melt from a solid state to a liquid state at high temperature without generating heat, and cannot provide a higher temperature to stimulate thermite reaction, resulting in higher brazing temperature and leakage rate.

[0093] By comparing the performance test results of Examples 1, 12-15 of the present invention in Table 1, it can be seen that the thickness of the nickel foil in Examples 1, 12-14 is controlled to be 150-700nm, which can ensure a lower brazing temperature and leakage rate, while the thickness of the nickel foil in Example 15 is relatively large, which will affect the thermal reaction during brazing, resulting in an increase in the brazing temperature and the leakage rate.

[0094] By comparing the performance test results of Examples 1-7 and 10 of the present invention in Table 1, it can be seen that the mass ratio of aluminum to copper oxide in complete thermite reaction is 9:40. After conversion according to density and volume, the total thickness ratio of aluminum foil and copper oxide foil required for complete reaction of aluminum and copper oxide is 1:2, and the copper and nickel generated by the thermite reaction are infinitely solid-dissolved, which is beneficial to brazing. If there is excess aluminum after the reaction, it can form an intermetallic compound with Ni, which is beneficial to brazing. Therefore, it is only necessary to ensure that the mass of aluminum foil participating in the reaction is sufficient, that is, the thickness ratio of aluminum foil to copper oxide foil must be not less than 1:2; while the thickness ratio of aluminum foil to copper oxide foil in Examples 8 and 10 is less than 1:2, and the thickness of aluminum foil is less, which affects the occurrence of partial thermite reaction, resulting in an increase in the leakage rate of Example 8, and a higher brazing temperature and leakage rate in Example 10.

[0095] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. It is particularly pointed out that for those skilled in the art, any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention should be included in the scope of protection of the present invention.

Claims

1. A preformed composite metal foil solder, It is characterized in that It comprises a carrier and a plurality of composite foil layers, wherein the plurality of composite foil layers are stacked and deposited on the surface of the carrier, the composite foil layers comprise copper oxide foil, aluminum foil and nickel foil which are stacked and deposited in sequence away from the carrier, and the carrier is magnesium foil.

2. A preformed composite metal foil solder according to claim 1, It is characterized in that The thickness of each layer of the copper oxide foil, aluminum foil and nickel foil is independent and is 150-700 nm.

3. A preformed composite metal foil solder as claimed in claim 2, It is characterized in that The thickness of each layer of the copper oxide foil, aluminum foil and nickel foil is independent and is 300-500 nm.

4. A preformed composite metal foil solder according to claim 1, It is characterized in that The thickness ratio of each layer of the aluminum foil and the oxidized copper foil is ≥ 1 / 2.

5. A preformed composite metal foil solder as claimed in claim 4, It is characterized in that The thickness ratio of each layer of aluminum foil to copper oxide foil is ≥5:

3.

6. A preformed composite metal foil solder according to claim 1, It is characterized in that The thickness of the carrier magnesium foil is 2-4 μm.

7. The preformed composite metal foil solder according to claim 1, It is characterized in that The composite foil layer is far away from the carrier and the side facing away from the carrier is coated with aluminum brazing agent, and the mass of the aluminum brazing agent accounts for 5-10% of the total mass of the composite metal foil brazing material.

8. A preformed composite metal foil solder according to claim 7, It is characterized in that The aluminum brazing flux is cesium fluoroaluminate.

9. A method for preparing the preformed composite metal foil solder according to any one of claims 1 to 8, It is characterized in that The following steps are involved: S1. Depositing copper oxide foil, aluminum foil and nickel foil in sequence on a carrier by a magnetron sputtering method to form a composite foil layer, repeatedly depositing multiple composite foil layers, and finally ending with aluminum foil or nickel foil until a desired thickness is obtained; S2. The composite foil layer is away from the carrier and the aluminum brazing agent is applied to the side facing away from the carrier to obtain a preformed composite metal foil brazing material.

10. A method for preparing a preformed composite metal foil solder according to claim 9, It is characterized in that In S1, the carrier is ultrasonically cleaned with deionized water, anhydrous ethanol and acetone in sequence and blown dry; the purity of the target material used for magnetron sputtering is above 99.95%, the sputtering pressure of magnetron sputtering is 0.5-1Pa, the sputtering power is 100-250W, and the argon flow rate is 35-50ml / min.

Citation Information

Patent Citations

  • Thermofusion welding agent for welding copper covered steel grounded screen

    CN101412167A

  • Thermit reaction foil, manufacturing method thereof and application thereof to welding process

    CN102248280A

  • Method for connecting carbon fiber reinforced aluminum-based composite with metal

    CN102658368A

  • Methods of forming polymer coatings on metallic substrates

    CN107073890A