Heat-insulating and high-strength PE (polyethylene) mulching film as well as preparation method and application thereof

Through multi-layer structure design and process preparation, the problem of poor thermal insulation performance of the existing PE mulch film has been solved, and a PE mulch film with high strength and good thermal insulation performance has been achieved, which is suitable for agricultural production.

CN118744579AInactive Publication Date: 2024-10-08MAIGAITI XINGLIAN TECH AGRI FILM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410855927.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The thermal insulation performance of existing PE mulch films is relatively average and cannot meet the high requirements of agricultural production.

Method used

The PE mulch film is designed with a multi-layer structure, in which the upper layer contains metallocene polyethylene, metallocene linear low-density polyethylene, low-density polyethylene and high-density polyethylene, the middle layer contains ultra-molecular weight polyethylene and polyethylene resin, and the lower layer contains ethylene. - Vinyl acetate copolymer resin and polyethylene resin, with a UV-absorbing anti-aging layer on each layer, prepared through extrusion, film blowing, cooling and traction processes.

Benefits of technology

It achieves good thermal insulation performance and high strength of PE mulch film, as well as good transparency and weather resistance, meeting the needs of agricultural production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118744579A_ABST
    Figure CN118744579A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of films, and discloses a heat-insulating and high-strength PE mulching film as well as a preparation method and application thereof. The PE mulching film sequentially comprises an upper layer, a middle layer and a lower layer from top to bottom, the material components of the upper layer comprise at least two of metallocene polyethylene, metallocene linear low-density polyethylene, low-density polyethylene, high-density polyethylene and linear low-density polyethylene; the middle layer is prepared from the following material components in parts by weight: 5 to 40 parts of ultra-molecular weight polyethylene and 60 to 90 parts of polyethylene resin; the molecular weight of the ultra-molecular weight polyethylene is 50,000-3,000,000; the lower layer is prepared from the following material components in parts by weight: 10 to 40 parts of ethylene-vinyl acetate copolymer resin and 60 to 90 parts of polyethylene resin. Due to the selection of the material components of the middle layer, the material components of the lower layer and the dosages and the selection of the components of the upper layer in the PE mulching film, the PE mulching film has good heat preservation performance and strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin films, and in particular relates to a heat-insulating, high-strength PE ground film and a preparation method and application thereof. Background Art

[0002] PE (polyethylene) mulch is a thin film that is often used in agricultural production. The thickness of existing PE mulch is generally 10-30μm, resulting in relatively average strength and thermal insulation performance, especially the thermal insulation performance cannot meet the high requirements in agricultural production.

[0003] Therefore, there is an urgent need to provide a new PE mulch film to solve the problem of poor thermal insulation performance in the prior art. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a heat-insulating, high-strength PE ground film and its preparation method and application. The PE ground film of the present invention has good heat-insulating performance and further has high strength characteristics.

[0005] A first aspect of the present invention provides a heat-insulating, high-strength PE ground film.

[0006] Specifically, a heat-insulating, high-strength PE ground film includes, from top to bottom, an upper layer, a middle layer, and a lower layer;

[0007] The material components of the upper layer include at least two of metallocene polyethylene, metallocene linear low-density polyethylene, low-density polyethylene, high-density polyethylene, and linear low-density polyethylene;

[0008] The material components of the intermediate layer include 5-40 parts of ultra-molecular weight polyethylene and 60-90 parts of polyethylene resin by weight; the molecular weight of the ultra-molecular weight polyethylene is 500,000-3,000,000;

[0009] The material components of the lower layer include 10-40 parts of ethylene-vinyl acetate copolymer resin and 60-90 parts of polyethylene resin by weight.

[0010] Preferably, the density of the metallocene polyethylene (mPE) is 0.940-0.955 g / cm 3 .

[0011] Preferably, the density of the metallocene linear low-density polyethylene (mLLDPE) is 0.910-0.930 g / cm 3 .

[0012] Preferably, the density of the low-density polyethylene is 0.910-0.938 g / cm 3 .

[0013] Preferably, the density of the high-density polyethylene is 0.948-0.965 g / cm 3 .

[0014] Preferably, the density of the linear low-density polyethylene is 0.910-0.930 g / cm 3 .

[0015] Preferably, when the upper layer contains two components, the weight ratio of the two components is (10-50):(50-90); when the upper layer contains three components, the weight ratio of the two components is (10-50):(50-90):1; when the upper layer contains four components, the weight ratio of the two components is (10-50):(20-40):(20-40):1; when the upper layer contains five components, the weight ratio of the two components is (10-50):(10-50):(20-40):(20-40):1.

[0016] Preferably, the melt index of the material component of the upper layer is 0.8-1.2 g / 10 min, more preferably 0.9-1.1 g / 10 min.

[0017] Preferably, a first UV absorbing anti-aging layer is also provided on the upper surface of the upper layer of the PE ground film.

[0018] Preferably, a second ultraviolet absorbing anti-aging layer is also provided on the lower surface of the lower layer of the PE mulch. The first ultraviolet absorbing anti-aging layer and the second ultraviolet absorbing anti-aging layer are provided to absorb ultraviolet light when sunlight passes through the PE mulch and reaches the surface to provide the temperature required for the growth of crops. At the same time, the ultraviolet light emitted by the sunlight on the surface is also absorbed, thereby preventing the PE mulch from being aged and crushed after being irradiated by ultraviolet light and maintaining its original physical properties and integrity. The material components of the first ultraviolet absorbing anti-aging layer and the second ultraviolet absorbing anti-aging layer are conventional anti-ultraviolet aging components and polyethylene resins, such as at least one of 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-n-octyloxybenzophenone, and 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole.

[0019] Preferably, the thickness of the PE ground film is 5-25 μm, more preferably 10-20 μm.

[0020] Preferably, the thickness of the first UV absorbing anti-aging layer and the second UV absorbing anti-aging layer are both 0.5-2.5 μm, more preferably 1-2 μm.

[0021] Preferably, the thickness of the upper layer is 1.0-4.2 μm, more preferably 1.5-3.5 μm.

[0022] Preferably, the thickness of the intermediate layer is 2.5-10.5 μm, more preferably 3-9 μm.

[0023] Preferably, the thickness of the lower layer is 1.0-4.2 μm, more preferably 1.5-3.5 μm.

[0024] A second aspect of the present invention provides a method for preparing a heat-insulating, high-strength PE ground film.

[0025] Specifically, a method for preparing a heat-insulating, high-strength PE mulch film comprises the following steps:

[0026] (1) Extrusion: The material components of the upper layer, the middle layer, and the lower layer are mixed according to the proportions and sent to the extruder respectively;

[0027] (2) Film blowing: PE ground film is made by one-time blowing by an extruder;

[0028] (3) Cooling;

[0029] (4) Traction;

[0030] (5) Coiling.

[0031] Preferably, during the extrusion in step (1), the material components of the first UV absorbing anti-aging layer and the second UV absorbing anti-aging layer are also extruded.

[0032] Preferably, steps (1) and (2) use an extruder of a 5-layer co-extrusion film blowing unit.

[0033] Preferably, during the film blowing process of step (2), the melt flow rate of each raw material is 0.5-2 g / 10 min, more preferably 1.1-1.5 g / 10 min.

[0034] Preferably, the cooling time in step (3) is 60-90 seconds, more preferably 75-80 seconds.

[0035] A third aspect of the present invention provides an application of a heat-insulating, high-strength PE ground film.

[0036] Specifically, the above-mentioned PE mulch film is used in agricultural production.

[0037] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0038] Due to the selection of the material components of the middle layer and the material components and the dosage of the lower layer in the PE ground film, as well as the selection of the upper layer components, the PE ground film of the present invention has good thermal insulation performance and good strength. Among them, the selection of the lower layer material components not only enables the PE ground film to have the functions of retaining moisture and heat preservation for the soil, but also has very good transparency and weather resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a schematic diagram of the structure of the PE ground film of Example 1 of the present invention. DETAILED DESCRIPTION

[0040] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0041] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0042] Example 1

[0043] A heat-insulating, high-strength PE ground film, which comprises, from top to bottom, a first UV absorbing anti-aging layer, an upper layer, a middle layer, a lower layer, and a second UV absorbing anti-aging layer;

[0044] The material component of the upper layer is metallocene polyethylene (density 0.940g / cm 3 ), metallocene linear low-density polyethylene (density 0.920g / cm 3 ), low-density polyethylene (density 0.911g / cm 3 ), high-density polyethylene (density 0.965g / cm 3 ), linear low-density polyethylene (density 0.918g / cm 3 ) is composed according to a weight ratio of 20:25:25:29:1; the melt index of the material component of the upper layer is 1.05g / 10min;

[0045] The material components of the middle layer are, by weight, 30 parts of ultra-molecular weight polyethylene (the molecular weight of ultra-molecular weight polyethylene is about 800,000, and "about" means there is a 2% error) and 70 parts of polyethylene resin;

[0046] The material components of the lower layer are 40 parts of ethylene-vinyl acetate copolymer resin and 60 parts of polyethylene resin by weight;

[0047] The material components of the first UV absorbing anti-aging layer are 95 parts of polyethylene resin and 5 parts of 2-hydroxy-4-methoxybenzophenone by weight;

[0048] The material components of the second UV absorbing anti-aging layer are 94 parts of polyethylene resin and 6 parts of 2-hydroxy-4-n-octyloxybenzophenone by weight.

[0049] The thickness of the first UV absorbing anti-aging layer and the second UV absorbing anti-aging layer are both 1.5 μm.

[0050] The thickness of the upper layer was 4 μm.

[0051] The thickness of the intermediate layer was 10 μm.

[0052] The thickness of the lower layer was 3 μm.

[0053] A method for preparing a heat-insulating, high-strength PE mulch film comprises the following steps:

[0054] (1) Extrusion: The material components of the first UV absorbing anti-aging layer, the upper layer, the middle layer, the lower layer, and the second UV absorbing anti-aging layer are mixed evenly according to a ratio, and are respectively sent to the extruder of the 5-layer co-extrusion film blowing unit;

[0055] (2) Film blowing: The PE film is produced by one-time blowing by an extruder, and the melt flow rate of each raw material is 1.1 g / 10 min;

[0056] (3) Cooling, the cooling time is 80 seconds;

[0057] (4) Traction;

[0058] (5) Coiling.

[0059] Pulling and reeling are conventional operations in this field.

[0060] Figure 1 This is a schematic diagram of the structure of the PE ground film of Example 1 of the present invention. Figure 1 100 represents the first UV absorbing anti-aging layer, 200 represents the upper layer, 300 represents the middle layer, 400 represents the lower layer, and 500 represents the second UV absorbing anti-aging layer.

[0061] Example 2

[0062] A heat-insulating, high-strength PE ground film, which comprises, from top to bottom, a first UV absorbing anti-aging layer, an upper layer, a middle layer, a lower layer, and a second UV absorbing anti-aging layer;

[0063] The material component of the upper layer is metallocene polyethylene (density 0.940g / cm 3 ), metallocene linear low-density polyethylene (density 0.920g / cm 3 ), low-density polyethylene (density 0.910g / cm 3 ), high-density polyethylene (density 0.960g / cm 3 ), linear low-density polyethylene (density 0.918g / cm 3) is composed according to a weight ratio of 20:25:26:28:1; the melt index of the material component of the upper layer is 1.05g / 10min;

[0064] The material components of the middle layer are, by weight, 10 parts of ultra-molecular weight polyethylene (the molecular weight of ultra-molecular weight polyethylene is about 2 million, "about" means there is a 2% error), and 90 parts of polyethylene resin;

[0065] The material components of the lower layer are 20 parts of ethylene-vinyl acetate copolymer resin and 80 parts of polyethylene resin by weight;

[0066] The material components of the first UV absorbing anti-aging layer are 95 parts of polyethylene resin and 5 parts of 2-hydroxy-4-methoxybenzophenone by weight;

[0067] The material components of the second UV absorbing anti-aging layer are 94 parts of polyethylene resin and 6 parts of 2-hydroxy-4-n-octyloxybenzophenone by weight.

[0068] The thickness of the first UV absorbing anti-aging layer and the second UV absorbing anti-aging layer are both 1 μm.

[0069] The thickness of the upper layer was 3.5 μm.

[0070] The thickness of the intermediate layer was 9 μm.

[0071] The thickness of the lower layer was 3 μm.

[0072] A method for preparing a heat-insulating, high-strength PE mulch film comprises the following steps:

[0073] (1) Extrusion: The material components of the first UV absorbing anti-aging layer, the upper layer, the middle layer, the lower layer, and the second UV absorbing anti-aging layer are mixed evenly according to a ratio, and are respectively sent to the extruder of the 5-layer co-extrusion film blowing unit;

[0074] (2) Film blowing: The PE film is produced by one-time blowing by an extruder, and the melt flow rate of each raw material is 1.1 g / 10 min;

[0075] (3) Cooling, the cooling time is 80 seconds;

[0076] (4) Traction;

[0077] (5) Coiling.

[0078] Pulling and reeling are conventional operations in this field.

[0079] Example 3

[0080] A heat-insulating, high-strength PE ground film, which comprises, from top to bottom, a first UV absorbing anti-aging layer, an upper layer, a middle layer, a lower layer, and a second UV absorbing anti-aging layer;

[0081] The material component of the upper layer is metallocene polyethylene (density 0.940g / cm 3 ), metallocene linear low-density polyethylene (density 0.925g / cm 3 ), low-density polyethylene (density 0.910g / cm 3 ), high-density polyethylene (density 0.965g / cm 3 ), linear low-density polyethylene (density 0.918g / cm 3 ) is composed according to a weight ratio of 20:27:27:25:1; the melt index of the material component of the upper layer is 1.05g / 10min;

[0082] The material components of the middle layer are, by weight, 20 parts of ultra-molecular weight polyethylene (the molecular weight of ultra-molecular weight polyethylene is about 1.5 million, "about" means there is a 2% error), and 80 parts of polyethylene resin;

[0083] The material components of the lower layer are 10 parts of ethylene-vinyl acetate copolymer resin and 90 parts of polyethylene resin by weight;

[0084] The material components of the first UV absorbing anti-aging layer are 95 parts of polyethylene resin and 5 parts of 2-hydroxy-4-methoxybenzophenone by weight;

[0085] The material components of the second UV absorbing anti-aging layer are 94 parts of polyethylene resin and 6 parts of 2-hydroxy-4-n-octyloxybenzophenone by weight.

[0086] The thickness of the first UV absorbing anti-aging layer and the second UV absorbing anti-aging layer are both 1 μm.

[0087] The thickness of the upper layer is 3 μm.

[0088] The thickness of the intermediate layer was 8 μm.

[0089] The thickness of the lower layer was 2 μm.

[0090] A method for preparing a heat-insulating, high-strength PE mulch film comprises the following steps:

[0091] (1) Extrusion: The material components of the first UV absorbing anti-aging layer, the upper layer, the middle layer, the lower layer, and the second UV absorbing anti-aging layer are mixed evenly according to a ratio, and are respectively sent to the extruder of the 5-layer co-extrusion film blowing unit;

[0092] (2) Film blowing: The PE film is produced by one-time blowing by an extruder, and the melt flow rate of each raw material is 1.1 g / 10 min;

[0093] (3) Cooling, the cooling time is 75 seconds;

[0094] (4) Traction;

[0095] (5) Coiling.

[0096] Pulling and reeling are conventional operations in this field.

[0097] Example 4

[0098] Compared with Example 1, Example 4 does not contain the first UV absorbing anti-aging layer and the second UV absorbing anti-aging layer, and the remaining components and processes are the same as those in Example 1.

[0099] Comparative Example 1

[0100] Compared with Example 1, the difference of Comparative Example 1 is that in the preparation process of the middle layer, an equal amount of ultra-molecular weight polyethylene with a molecular weight of 400,000 is used to replace the ultra-molecular weight polyethylene with a molecular weight of 800,000 in Example 1, and the other components and processes are the same as those in Example 1.

[0101] Comparative Example 2

[0102] Compared with Example 1, the difference of Comparative Example 2 is that in the preparation process of the lower layer, an equal amount of polyethylene resin is used instead of ethylene-vinyl acetate copolymer resin, and the other components and processes are the same as those of Example 1.

[0103] Product effect testing

[0104] 1. Thermal insulation effect test

[0105] The temperature at 5 cm underground in the test field without PE mulch was 17.4°C at 18:00. Then the temperature at 5 cm underground covered with PE mulch prepared in Example 1 and Comparative Examples 1-2 was tested from 20:00 to 6:00 in the morning. The temperature was measured every 2 hours for a total of 6 times, and the average temperature was calculated. The results are shown in Table 1.

[0106] Table 1

[0107]

[0108] It can be seen from Table 1 that the PE mulch prepared in Example 1 has a better thermal insulation effect than that of Comparative Examples 1-2.

[0109] 2. Strength test

[0110] The PE mulch films prepared in Examples 1-4 and Comparative Examples 1-2 were tested for tensile properties according to the film tensile properties test method in GB13022-1991. The transverse tensile strength results of the PE mulch films are shown in Table 2.

[0111] Table 2

[0112] Transverse tensile strength (MPa) Example 1 48.1 Example 2 47.9 Example 3 48.3 Example 4 47.8 Comparative Example 1 46.6 Comparative Example 2 45.8

[0113] It can be seen from Table 2 that the PE mulch prepared in the embodiment has better tensile strength than that in the comparative examples 1-2.

[0114] In addition, the visible light transmittance of the PE ground film prepared in Example 1 was tested to be 90.7%.

Claims

1. A PE ground film, characterized in that: From top to bottom, it includes the upper layer, the middle layer, and the lower layer; The material components of the upper layer include at least two of metallocene polyethylene, metallocene linear low-density polyethylene, low-density polyethylene, high-density polyethylene, and linear low-density polyethylene; The material components of the intermediate layer include 5-40 parts of ultra-molecular weight polyethylene and 60-90 parts of polyethylene resin by weight; the molecular weight of the ultra-molecular weight polyethylene is 500,000-3,000,000; The material components of the lower layer include 10-40 parts of ethylene-vinyl acetate copolymer resin and 60-90 parts of polyethylene resin by weight.

2. The PE ground film according to claim 1, characterized in that: The density of the metallocene polyethylene is 0.940-0.955 g / cm 3 ; and / or, the density of the metallocene linear low-density polyethylene is 0.910-0.930g / cm 3 ; and / or, the density of the low-density polyethylene is 0.910-0.938g / cm 3 ; and / or, the density of the high-density polyethylene is 0.948-0.965g / cm 3 ; and / or, the density of the linear low density polyethylene is 0.910-0.930g / cm 3 .

3. The PE ground film according to claim 1, characterized in that: When the upper layer contains two components, the weight ratio of the two components is (10-50):(50-90); when the upper layer contains three components, the weight ratio of the two components is (10-50):(50-90):1; when the upper layer contains four components, the weight ratio of the two components is (10-50):(20-40):(20-40):1; when the upper layer contains five components, the weight ratio of the two components is (10-50):(10-50):(20-40):(20-40):

1.

4. The PE ground film according to claim 1, characterized in that: The melt index of the material component of the upper layer is 0.8-1.2 g / 10 min.

5. The PE ground film according to claim 1, characterized in that: A first UV absorbing and anti-aging layer is further provided on the upper surface of the upper layer of the PE ground film; and / or a second UV absorbing and anti-aging layer is further provided on the lower surface of the lower layer of the PE ground film.

6. The PE ground film according to any one of claims 1 to 5, characterized in that: The thickness of the upper layer is 1.0-4.2 μm; and / or the thickness of the middle layer is 2.5-10.5 μm; and / or the thickness of the lower layer is 1.0-4.2 μm.

7. The method for preparing the PE mulch film according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) Extrusion: The material components of the upper layer, the middle layer, and the lower layer are mixed according to the proportions and sent to the extruder respectively; (2) Film blowing: PE ground film is made by one-time blowing by an extruder; (3) Cooling; (4) Traction; (5) Coiling.

8. The preparation method according to claim 7, characterized in that: During the extrusion in step (1), the material components of the first UV absorbing anti-aging layer and the second UV absorbing anti-aging layer are also extruded.

9. The preparation method according to claim 7, characterized in that: The cooling time in step (3) is 60-90 seconds.

10. Use of the PE mulch film according to any one of claims 1 to 6 in agricultural production.

Citation Information

Patent Citations

  • Hydrophilic weeding environmental-protection type mulch film

    CN104744757A

  • PE (polyethylene) Mulching film

    CN108207443A

  • Composite waterproof coiled material synthesized by means of in-situ reactive compatibilization and method for preparing composite waterproof coiled material

    CN109082000A

  • Recyclable polyethylene agricultural film as well as preparation method and application thereof

    CN116080227A

  • Recyclable polyethylene agricultural film as well as preparation method and application thereof

    CN117362797A