Optical glass, glass preform and optical element

CN118745077APending Publication Date: 2024-10-08CDGM OPTICAL GLASS
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411005227.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-08-26
Publication Date
2024-10-08

AI Technical Summary

Benefits of technology

[0025] The beneficial effects of the present invention are: through reasonable component design, the optical glass obtained by the present invention has a high Young's modulus while having a desired refractive index and Abbe number.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004962830810000121
    Figure BDA0004962830810000121
  • Figure BDA0004962830810000131
    Figure BDA0004962830810000131
  • Figure BDA0004962830810000151
    Figure BDA0004962830810000151
Patent Text Reader

Abstract

The invention provides optical glass which comprises the following components in percentage by weight: 2-18% of SiO2; 8 to 22 percent of B2O3; la2O3: 40% to 55%; 3 to 18 percent of Y2O3; zrO2: 1%-15%; and 2 to 15% of Nb2O5, wherein the ratio of La2O3 to (B2O3 + Nb2O5) is 1.2 to 5.0. Through reasonable component design, the optical glass obtained by the invention has a relatively high Young modulus while having an expected refractive index and an expected Abbe number.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application for the invention patent application with application number 202211031705.0, application date August 26, 2022, and name “Optical glass, glass preforms and optical elements”. Technical Field

[0002] The invention relates to optical glass, in particular to optical glass with high Young's modulus, and a glass preform and an optical element made of the optical glass. Background Art

[0003] In recent years, with the rapid popularization and use of digital cameras, video cameras and camera phones, optical materials have developed rapidly in the direction of high precision and miniaturization. With the continuous integration of optics, electronic information science and new materials science, the application of optical glass as the basic material of optoelectronics in technical fields such as light transmission, light storage and optoelectronic display has made great strides. Optical instruments have developed rapidly in digitalization, integration and high precision, and higher requirements have been put forward for the performance of optical glass used in optical instruments and equipment. Optical glass with a refractive index of 1.82 to 1.89 and an Abbe number of 37 to 44 can achieve a larger viewing angle with a smaller volume due to its high refractive index. It is of great significance to simplify the optical system and improve the imaging quality in the field of optical design and optical communication. When optical glass is processed into smaller or thinner optical components, if its Young's modulus is small, it is easy to deform during use. Therefore, the development of high-refractive-index optical glass with a high Young's modulus plays an important role in the development of high-performance optoelectronic products. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide an optical glass with a higher Young's modulus.

[0005] The technical solution adopted by the present invention to solve the technical problem is:

[0006] (1) Optical glass, the components of which, expressed in weight percentage, contain: SiO2: 2-18%; B2O3: 8-22%; La2O3: 40-60%; Y2O3: 3-18%; ZrO2: 1-15%; Nb2O5: 2-15%, wherein La2O3 / (B2O3+Nb2O5) is 1.2-5.0.

[0007] (2) The optical glass according to (1), wherein the components, expressed in weight percentage, further contain: Ta2O5: 0-10%; and / or Gd2O3: 0-9%; and / or TiO2: 0-6%; and / or RO: 0-10%; and / or Rn2O: 0-8%; and / or WO3: 0-8%; and / or ZnO: 0-10%; and / or Al2O3: 0-5%; and / or Yb2O3: 0-8%; and / or GeO2: 0-5%; and / or a clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0008] (3) Optical glass comprising SiO2, B2O3, La2O3, Y2O3, ZrO2, and Nb2O5, wherein the composition is expressed in weight percentage, wherein La2O3 / (B2O3+Nb2O5) is 1.2 to 5.0, and the refractive index of the optical glass is n d is 1.82~1.89, Abbe number v d is 37-44, and Young's modulus E is 10500×10 7 Pa or above.

[0009] (4) The optical glass according to (3), wherein the components, expressed in weight percentage, are: SiO2: 2-18%; and / or B2O3: 8-22%; and / or La2O3: 40-60%; and / or Y2O3: 3-18%; and / or ZrO2: 1-15%; and / or Nb2O5: 2-15%; and / or Ta2O5: 0-10%; and / or Gd2O3: 0-9%; and / or TiO2: 0-6%; and / or RO: 0-10%; and / or Rn2O: 0-8%; and / or WO3: 0-8%; and / or ZnO: 0-10%; and / or Al2O3: 0-5%; and / or Yb2O3: 0-8%; and / or GeO2: 0-5%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

[0010] (5) The optical glass according to any one of (1) to (4), wherein the components thereof, expressed in weight percentage, satisfy one or more of the following seven conditions:

[0011] 1) (ZnO + Ta2O5) / Nb2O5 is less than 2.0, preferably (ZnO + Ta2O5) / Nb2O5 is less than 1.5, more preferably (ZnO + Ta2O5) / Nb2O5 is less than 1.0, and further preferably (ZnO + Ta2O5) / Nb2O5 is 0.1 to 0.8;

[0012] 2) (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.5, preferably (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.4, more preferably (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.3, and further preferably (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.2;

[0013] 3) (Ta2O5+Gd2O3) / Y2O3 is less than 1.0, preferably (Ta2O5+Gd2O3) / Y2O3 is less than 0.8, more preferably (Ta2O5+Gd2O3) / Y2O3 is less than 0.5, and further preferably (Ta2O5+Gd2O3) / Y2O3 is less than 0.2;

[0014] 4) La2O3 / (B2O3+Nb2O5) is 1.3 to 4.0, preferably La2O3 / (B2O3+Nb2O5) is 1.5 to 3.5, and more preferably La2O3 / (B2O3+Nb2O5) is 1.7 to 2.7;

[0015] 5) (ZnO + WO3) / Nb2O5 is 3.0 or less, preferably (ZnO + WO3) / Nb2O5 is 2.0 or less, more preferably (ZnO + WO3) / Nb2O5 is 1.5 or less, and further preferably (ZnO + WO3) / Nb2O5 is 0.2 to 1.0;

[0016] 6) (Gd2O3+ZnO) / Y2O3 is less than 2.0, preferably (Gd2O3+ZnO) / Y2O3 is less than 1.5, more preferably (Gd2O3+ZnO) / Y2O3 is less than 1.0, and further preferably (Gd2O3+ZnO) / Y2O3 is less than 0.8;

[0017] 7) (B2O3+RO) / La2O3 is 0.15-0.7, preferably (B2O3+RO) / La2O3 is 0.15-0.6, more preferably (B2O3+RO) / La2O3 is 0.18-0.5, and further preferably (B2O3+RO) / La2O3 is 0.2-0.4, and the RO is one or more of MgO, CaO, SrO, and BaO.

[0018] (6) The optical glass according to any one of (1) to (4), wherein the components are expressed in weight percentage, wherein: SiO2: 4-15%, preferably SiO2: 6-12%; and / or B2O3: 10-20%, preferably B2O3: 12-18%; and / or La2O3: 43-55%, preferably La2O3: 46-52%; and / or Y2O3: 5-15%, preferably Y2O3: 7-13%; and / or ZrO2: 2-12%, preferably ZrO2: 3-10%; and / or Nb2O5: 3-13%, preferably Nb2O5: 5-11%; and / or Ta2O5: 0-5%, preferably Ta2O5: 0-2%; and / or Gd2O3: 0-5%, preferably Gd2O3: 0-2%; and / or TiO2: 0-4%, preferably TiO2: 0-2%; and / or RO: 0-5%, preferably RO: 0-2%; and / or Rn2O: 0-4%, preferably Rn2O: 0-2%; and / or WO3: 0-6%, preferably WO3: 0-4%; and / or ZnO: 1-8%, preferably ZnO: 2-7%; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%; and / or Yb2O3: 0-3%, preferably Yb2O3: 0-1%; and / or GeO2: 0-3%, preferably GeO2: 0-1%; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, wherein RO is one or more of MgO, CaO, SrO and BaO, Rn2O is one or more of Li2O, Na2O and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2 and CeO2.

[0019] (7) The optical glass according to any one of (1) to (4), which does not contain Ta2O5; and / or does not contain RO; and / or does not contain Rn2O; and / or does not contain Gd2O3; and / or does not contain Yb2O3; and / or does not contain Al2O3; and / or does not contain GeO2, wherein RO is one or more of MgO, CaO, SrO, and BaO, and Rn2O is one or more of Li2O, Na2O, and K2O.

[0020] (8) The optical glass according to any one of (1) to (4), wherein the refractive index n d is 1.82 to 1.89, preferably 1.83 to 1.88, more preferably 1.84 to 1.87, and the Abbe number v d It is 37-44, preferably 38-43, and more preferably 39-42.

[0021] (9) The optical glass according to any one of (1) to (4), wherein the density ρ of the optical glass is 5.00 g / cm 3 Below, preferably 4.90g / cm3 Below, more preferably 4.80g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 85×10 -7 / K or less, preferably 80×10 -7 / K or less, more preferably 75×10 -7 / K or less, more preferably 70×10 -7 / K or less; and / or water resistance stability D W 2 or more, preferably 1; and / or acid resistance stability D A Two or more types, preferably one type; and / or 70 400nm or less, preferably λ 70 395nm or less, preferably λ 70 390nm or less; and / or λ5 is 350nm or less, preferably λ5 is 345nm or less, more preferably λ5 is 340nm or less; and / or weather resistance CR is 2 or more, preferably 1; and / or Knoop hardness H K 670×10 7 Pa or more, preferably 680×10 7 Pa or more, more preferably 690×10 7 Pa or more, more preferably 695×10 7 Pa or more; and / or Young's modulus E is 10500×10 7 Pa or more, preferably 11000×10 7 Pa or more, more preferably 11500×10 7 Pa or above; and / or wear degree F A The foaming degree is 75 to 120, preferably 80 to 110, and more preferably 86 to 105; and / or the foaming degree is A grade or higher, preferably A0 grade or higher, and more preferably A 00 class.

[0022] (10) A glass preform made of the optical glass described in any one of (1) to (9).

[0023] (11) An optical element, made of the optical glass described in any one of (1) to (9), or made of the glass preform described in (10).

[0024] (12) An optical instrument comprising the optical glass described in any one of (1) to (9) and / or the optical element described in (11).

[0025] The beneficial effect of the present invention is that, through reasonable component design, the optical glass obtained by the present invention has a desired refractive index and Abbe number and a higher Young's modulus. DETAILED DESCRIPTION

[0026] The following will describe the embodiments of the optical glass of the present invention in detail, but the present invention is not limited to the following embodiments, and can be implemented by appropriate changes within the scope of the purpose of the present invention. In addition, although there are appropriate omissions of descriptions of the repeated descriptions, the gist of the invention will not be limited thereby, and in the following content, the optical glass of the present invention is sometimes referred to as glass.

[0027] [Optical glass]

[0028] The following is an explanation of the range of each component (ingredient) of the optical glass of the present invention. In the present invention, unless otherwise specified, the content and total content of each component are all expressed in weight percentage (wt%), that is, the content and total content of each component are expressed in weight percentage relative to the total amount of glass material converted into oxide composition. Here, the "composition converted into oxide" means that when the oxides, complex salts and hydroxides used as raw materials for the optical glass components of the present invention decompose and transform into oxides during melting, the total amount of the oxide material is taken as 100%.

[0029] Unless otherwise specified in specific circumstances, the numerical ranges listed in the present invention include upper and lower limits, "above" and "below" include endpoint values, and all integers and fractions included in the range, without being limited to the specific values ​​listed when the range is defined. "And / or" referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0030] <Essential Components and Optional Components>

[0031] SiO2 has the effects of adjusting optical constants, improving the chemical stability of glass, maintaining viscosity suitable for molten glass, reducing abrasiveness and reducing erosion of refractory materials. In the present invention, the above-mentioned effect is obtained by containing more than 2% SiO2. Preferably, the content of SiO2 is more than 4%, and more preferably, the content of SiO2 is more than 6%. If the content of SiO2 is too high, the melting difficulty of glass increases and the transition temperature rises. Therefore, in the present invention, the content of SiO2 is upper limited to 18%, preferably upper limited to 15%, and more preferably upper limited to 12%.

[0032] B2O3 can improve the melting property and resistance to devitrification of glass, and is conducive to lowering the transition temperature of glass. The present invention obtains the above effect by containing more than 8% B2O3, preferably more than 10% B2O3, and more preferably more than 12% B2O3. If the content of B2O3 is too high, the chemical stability of the glass deteriorates, especially the water resistance deteriorates, and the refractive index and light transmittance of the glass decrease. Therefore, the content of B2O3 is less than 22%, preferably less than 20%, and more preferably less than 18%.

[0033] La2O3 is an effective component for improving the refractive index of glass, and has a significant effect on improving the chemical stability and resistance to devitrification of glass. If its content is less than 40%, it is difficult to achieve the required optical constants; if the content is higher than 60%, the devitrification tendency of the glass increases and the thermal stability deteriorates. Therefore, the content of La2O3 is limited to 40-60%, preferably 43-55%, and more preferably 46-52%.

[0034] Y2O3 can improve the refractive index and devitrification resistance of glass and adjust the Young's modulus of glass. The present invention achieves the above effects by containing more than 3% Y2O3. If its content exceeds 18%, the chemical stability and weather resistance of glass will deteriorate. Therefore, the content of Y2O3 in the present invention is 3-18%, preferably 5-15%, and more preferably 7-13%.

[0035] Gd2O3 can improve the refractive index and chemical stability of glass, but if its content is higher than 9%, the devitrification resistance and abrasion resistance of glass will deteriorate. Therefore, the content of Gd2O3 is 0 to 9%, preferably 0 to 5%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Gd2O3 is not contained.

[0036] Yb2O3 is also a component that gives glass high refractive and low dispersion properties. If its content exceeds 8%, the anti-crystallization performance of the glass decreases. Therefore, the content of Yb2O3 is 0-8%, preferably 0-3%, more preferably 0-1%, and more preferably no Yb2O3 is contained.

[0037] ZrO2 can improve the viscosity, hardness, refractive index and chemical stability of optical glass, and can also reduce the thermal expansion coefficient of glass; when the content of ZrO2 is too high, the resistance to devitrification of glass decreases, the difficulty of melting increases, the melting temperature rises, and inclusions appear inside the glass and the light transmittance decreases. Therefore, the content of ZrO2 in the present invention is 1-15%, preferably 2-12%, and more preferably 3-10%.

[0038] TiO2 can increase the refractive index of glass, but too high a content will greatly reduce the dispersion coefficient and increase the tendency of crystallization, and even cause the glass to be obviously colored. Therefore, the TiO2 content is limited to 0-6%, preferably 0-4%, and more preferably 0-2%.

[0039] Ta2O5 has the effect of increasing the refractive index and improving the devitrification resistance of glass, but if its content is too high, the thermal stability of the glass will decrease, the density will increase, and the optical constants will be difficult to control within the desired range; on the other hand, compared with other components, the price of Ta2O5 is very expensive. From the perspective of practicality and cost, its usage should be minimized. Therefore, the content of Ta2O5 in the present invention is limited to 0-10%, preferably 0-5%, more preferably 0-2%, and it is further preferred that Ta2O5 is not contained.

[0040] In some embodiments, the ratio of the total content of Ta2O5 and Gd2O3 Ta2O5+Gd2O3 to the content of Y2O3 (Ta2O5+Gd2O3) / Y2O3 is controlled to be below 1.0, which is beneficial for the glass to obtain a suitable abrasiveness, optimize the density and Young's modulus of the glass, and prevent the chemical stability of the glass from deteriorating. Therefore, it is preferred that (Ta2O5+Gd2O3) / Y2O3 is below 1.0, more preferably (Ta2O5+Gd2O3) / Y2O3 is below 0.8, further preferably (Ta2O5+Gd2O3) / Y2O3 is below 0.5, and further preferably (Ta2O5+Gd2O3) / Y2O3 is below 0.2.

[0041] Nb2O5 is a high-refractive and high-dispersion component that can improve the refractive index and devitrification resistance of glass and reduce the thermal expansion coefficient of glass. In the present invention, the above effects are obtained by containing more than 2% Nb2O5. The lower limit of the content of Nb2O5 is preferably 3%, and the lower limit is more preferably 5%. If the content of Nb2O5 exceeds 15%, the thermal stability and weather resistance of the glass will decrease, and the light transmittance will decrease. Therefore, the upper limit of the content of Nb2O5 in the present invention is 15%, preferably 13%, and more preferably 11%.

[0042] In some embodiments, the ratio La2O3 / (B2O3+Nb2O5) between the content of La2O3 and the total content of B2O3 and Nb2O5 B2O3+Nb2O5 is controlled within the range of 1.2 to 5.0, which can increase the Young's modulus of the glass and the bubble degree of the glass. Therefore, La2O3 / (B2O3+Nb2O5) is preferably 1.2 to 5.0, and La2O3 / (B2O3+Nb2O5) is more preferably 1.3 to 4.0. Furthermore, La2O3 / (B2O3+Nb2O5) is controlled within the range of 1.5 to 3.5, which can further increase the hardness of the glass and reduce the thermal expansion coefficient of the glass. Therefore, La2O3 / (B2O3+Nb2O5) is further preferably 1.5 to 3.5, and La2O3 / (B2O3+Nb2O5) is further preferably 1.7 to 2.7.

[0043] Alkaline earth metal oxide RO (RO is one or more of MgO, CaO, SrO, BaO) can adjust the optical constants of glass and optimize the chemical stability of glass, but when its content is high, the devitrification resistance of glass decreases. Therefore, the RO content is limited to 0-10%, preferably 0-5%, and more preferably 0-2%. In some embodiments, it is further preferred that RO is not contained.

[0044] In some embodiments, the ratio of the total content of B2O3 and RO B2O3+RO to the content of La2O3 (B2O3+RO) / La2O3 is controlled within the range of 0.15 to 0.7, which can improve the bubble degree and weather resistance of the glass. Therefore, it is preferred that (B2O3+RO) / La2O3 is 0.15 to 0.7, and it is more preferred that (B2O3+RO) / La2O3 is 0.15 to 0.6. Furthermore, by controlling (B2O3+RO) / La2O3 within the range of 0.18 to 0.5, the hardness of the glass can be further improved and the thermal expansion coefficient of the glass can be optimized. Therefore, it is further preferred that (B2O3+RO) / La2O3 is 0.18 to 0.5, and it is further preferred that (B2O3+RO) / La2O3 is 0.2 to 0.4.

[0045] Alkali metal oxide Rn2O (Rn2O is one or more of Li2O, Na2O, K2O) can reduce the transition temperature of glass, adjust the optical constants and high temperature viscosity of glass, and improve the melting property of glass, but when its content is high, the devitrification resistance and chemical stability of glass are reduced. Therefore, the content of Rn2O in the present invention is 0 to 8%, preferably 0 to 4%, and more preferably 0 to 2%. In some embodiments, it is further preferred that Rn2O is not contained.

[0046] ZnO can adjust the refractive index and dispersion of glass, and reduce the high temperature viscosity and transition temperature of glass. If the content of ZnO is too high, the difficulty of glass molding increases and the anti-crystallization performance deteriorates. Therefore, the content of ZnO is 0-10%, preferably 1-8%, and more preferably 2-7%.

[0047] In some embodiments, the ratio (ZnO+Ta2O5) / Nb2O5 between the total content of ZnO and Ta2O5 ZnO+Ta2O5 and the content of Nb2O5 is controlled to be below 2.0, which is beneficial to improving the chemical stability and light transmittance of the glass. Therefore, it is preferred that (ZnO+Ta2O5) / Nb2O5 is below 2.0, and it is more preferred that (ZnO+Ta2O5) / Nb2O5 is below 1.5. Furthermore, controlling (ZnO+Ta2O5) / Nb2O5 below 1.0 can further improve the Young's modulus and bubble degree of the glass. Therefore, it is further preferred that (ZnO+Ta2O5) / Nb2O5 is below 1.0, and it is further preferred that (ZnO+Ta2O5) / Nb2O5 is 0.1 to 0.8.

[0048] In some embodiments, by controlling the ratio (Gd2O3+ZnO) / Y2O3 between the total content of Gd2O3 and ZnO Gd2O3+ZnO and the content of Y2O3 to be below 2.0, the thermal expansion coefficient of the glass can be reduced and the abrasiveness of the glass can be optimized. Therefore, it is preferred that (Gd2O3+ZnO) / Y2O3 is below 2.0, and it is more preferred that (Gd2O3+ZnO) / Y2O3 is below 1.5. Furthermore, controlling (Gd2O3+ZnO) / Y2O3 to be below 1.0 can make the glass easier to obtain a suitable Young's modulus and prevent the hardness of the glass from decreasing. Therefore, it is further preferred that (Gd2O3+ZnO) / Y2O3 is below 1.0, and it is further preferred that (Gd2O3+ZnO) / Y2O3 is below 0.8.

[0049] WO3 can improve the refractive index and mechanical strength of glass. If the content of WO3 exceeds 8%, the thermal stability of glass decreases and the resistance to devitrification decreases. Therefore, the content of WO3 is 0-8%, preferably 0-6%, and more preferably 0-4%.

[0050] In some embodiments, the ratio of the total content of Gd2O3, Ta2O5, and WO3 (Gd2O3+Ta2O5+WO3) to the content of La2O3 (Gd2O3+Ta2O5+WO3) / La2O3) is controlled to be below 0.5, which can reduce the density of the glass and improve the light transmittance of the glass. Therefore, it is preferred that (Gd2O3+Ta2O5+WO3) / La2O3 is below 0.5, and it is more preferred that (Gd2O3+Ta2O5+WO3) / La2O3 is below 0.4. Furthermore, by controlling (Gd2O3+Ta2O5+WO3) / La2O3 to be below 0.3, the abrasiveness and thermal expansion coefficient of the glass can be further optimized. Therefore, it is further preferred that (Gd2O3+Ta2O5+WO3) / La2O3 is below 0.3, and it is further preferred that (Gd2O3+Ta2O5+WO3) / La2O3 is below 0.2.

[0051] In some embodiments, the ratio (ZnO+WO3) / Nb2O5 between the total content of ZnO and WO3 ZnO+WO3 and the content of Nb2O5 is controlled to be below 3.0, which can improve the weather resistance of the glass and reduce the density of the glass. Therefore, it is preferred that (ZnO+WO3) / Nb2O5 is below 3.0, more preferably (ZnO+WO3) / Nb2O5 is below 2.0, and further preferably (ZnO+WO3) / Nb2O5 is below 1.5. Furthermore, controlling (ZnO+WO3) / Nb2O5 within the range of 0.2 to 1.0 can further optimize the hardness of the glass. Therefore, it is further preferred that (ZnO+WO3) / Nb2O5 is 0.2 to 1.0.

[0052] Al2O3 can improve the chemical stability of glass, but when its content exceeds 5%, the melting property and light transmittance of glass deteriorate. Therefore, the content of Al2O3 in the present invention is 0 to 5%, preferably 0 to 3%, and more preferably 0 to 1%. In some embodiments, it is further preferred that Al2O3 is not contained.

[0053] GeO2 has the effect of increasing the refractive index and resistance to devitrification, but if its content is too high, the chemical stability of the glass will decrease; on the other hand, compared with other components, GeO2 is very expensive, and its usage should be minimized from the perspective of practicality and cost. Therefore, the content of GeO2 in the present invention is limited to 0-5%, preferably 0-3%, more preferably 0-1%, and it is further preferred that GeO2 is not contained.

[0054] In the present invention, by containing 0-1% of one or more of Sb2O3, SnO, SnO2, and CeO2 as a clarifier, the clarification effect of the glass can be improved, and the bubble degree of the glass can be improved. The content of the clarifier is preferably 0-0.5%, and the content of the clarifier is more preferably 0-0.2%. Since the component types and contents of the optical glass of the present invention are reasonably designed and its bubble degree is excellent, it is further preferred in some embodiments that no clarifier is contained. When the Sb2O3 content exceeds 1%, the glass tends to have reduced clarification performance. At the same time, due to its strong oxidizing effect, it promotes the corrosion of platinum or platinum alloy vessels for melting glass and the deterioration of the molding mold. Therefore, the present invention preferably has a Sb2O3 content of 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably no Sb2O3. SnO and SnO2 can also be used as clarifiers, but when their content exceeds 1%, the glass tends to color more, or when the glass is heated, softened, and molded again, Sn will become the starting point for nucleation, resulting in a tendency to devitrification. Therefore, the content of SnO2 in the present invention is preferably 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably does not contain SnO2; the content of SnO is preferably 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably does not contain SnO. The role and content ratio of CeO2 are consistent with those of SnO2, and its content is preferably 0-1%, more preferably 0-0.5%, further preferably 0-0.2%, and further preferably does not contain CeO2.

[0055] <Components that should not be contained>

[0056] In the glass of the present invention, even if oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo are contained alone or in combination in small amounts, the glass will be colored and absorption will occur at specific wavelengths in the visible light region, thereby weakening the property of the present invention of improving the visible light transmittance. Therefore, it is preferably substantially free of oxides of transition metals such as V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo, especially for optical glasses that require transmittance at wavelengths in the visible light region.

[0057] The oxides of Th, Cd, Tl, Os, Be and Se have a tendency to be controlled in recent years as harmful chemical substances, and environmental protection measures are necessary not only in the manufacturing process of glass, but also in the processing process and the disposal after productization. Therefore, in the case of paying attention to the impact on the environment, it is preferred that they are not actually contained except for being inevitably mixed in. Thus, the optical glass does not actually contain substances that pollute the environment. Therefore, even if special environmental countermeasures are not taken, the optical glass of the present invention can be manufactured, processed and discarded.

[0058] In order to achieve environmental friendliness, the optical glass of the present invention preferably does not contain As2O3 and PbO.

[0059] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the optical glass of the present invention; however, as raw materials and / or equipment for producing optical glass, there will be certain impurities or components that are not intentionally added, which will be contained in a small amount or trace amount in the final optical glass, and this situation is also within the scope of protection of the patent of this invention.

[0060] Next, the properties of the optical glass of the present invention will be described.

[0061] <Refractive Index and Abbe Number>

[0062] The refractive index of optical glass (n d ) and the Abbe number (ν d ) Tested according to the method specified in GB / T 7962.1-2010.

[0063] In some embodiments, the refractive index (n d ) has a lower limit of 1.82, a preferred lower limit is 1.83, and a more preferred lower limit is 1.84.

[0064] In some embodiments, the refractive index (n d ) is 1.89, preferably 1.88, and more preferably 1.87.

[0065] In some embodiments, the Abbe number (ν d ) has a lower limit of 37, a preferred lower limit of 38, and a more preferred lower limit of 39.

[0066] In some embodiments, the Abbe number (ν d ) has an upper limit of 44, a preferred upper limit of 43, and a more preferred upper limit of 42.

[0067] <density>

[0068] The density (ρ) of optical glass is tested according to the method specified in GB / T7962.20-2010.

[0069] In some embodiments, the density (ρ) of the optical glass of the present invention is 5.00 g / cm 3 Below, preferably 4.90g / cm 3 Below, more preferably 4.80g / cm 3 the following.

[0070] <Coefficient of Thermal Expansion>

[0071] Thermal expansion coefficient of optical glass (α -30 / 70℃ ) The data at -30~70℃ were tested according to the method specified in GB / T7962.16-2010.

[0072] In some embodiments, the thermal expansion coefficient (α -30 / 70℃ ) is 85×10 -7 / K or less, preferably 80×10 -7 / K or less, more preferably 75×10 -7 / K or less, more preferably 70×10 -7 / K or less.

[0073] <Water resistance stability>

[0074] Water resistance stability of optical glass (D W ) (Powder method) Tested in accordance with the method specified in GB / T 17129.

[0075] In some embodiments, the water resistance stability (D W ) is 2 or more types, preferably 1 type.

[0076] <Acid resistance stability>

[0077] Acid resistance stability of optical glass (D A ) (Powder method) Tested in accordance with the method specified in GB / T 17129.

[0078] In some embodiments, the acid resistance stability (D A ) is 2 or more types, preferably 1 type.

[0079] <Color>

[0080] The short-wave transmission spectrum characteristics of the glass of the present invention are expressed by the coloration (λ 70 and λ5). 70 It refers to the wavelength when the glass transmittance reaches 70%. 70 The measurement is to use a glass with a thickness of 10±0.1mm and two opposite planes parallel to each other and optically polished, and measure the spectral transmittance in the wavelength range from 280nm to 700nm and the wavelength at which the transmittance is 70%. The so-called spectral transmittance or transmittance is the wavelength at which the incident intensity I is perpendicular to the above surface of the glass. in Light of intensity I passes through the glass and emerges from a plane out The light of the case through I out / I inThe amount expressed by λ also includes the transmittance of the surface reflection loss on the above surfaces of the glass. The higher the refractive index of the glass, the greater the surface reflection loss. Therefore, in high refractive index glass, λ 70 A small value of means that the glass itself is less colored and has a high light transmittance.

[0081] In some embodiments, the λ of the optical glass of the present invention is 70 400nm or less, preferably λ 70 395nm or less, preferably λ 70 Below 390nm.

[0082] In some embodiments, the λ5 of the optical glass of the present invention is 350 nm or less, preferably 345 nm or less, and more preferably 340 nm or less.

[0083] <Weather resistance>

[0084] The test method for weather resistance (CR) of optical glass is as follows: place the sample in a test box with a saturated water vapor environment of 90% relative humidity, alternately cycle every 1 hour at 40-50°C, and cycle for 15 cycles. The weather resistance category is divided according to the change in turbidity before and after the sample is placed. The weather resistance classification is shown in Table 1:

[0085] Table 1.

[0086]

[0087] In some embodiments, the weather resistance (CR) of the optical glass of the present invention is Class 2 or higher, preferably Class 1.

[0088] <Knoop hardness>

[0089] Knoop hardness of optical glass (H K ) The test shall be carried out according to the test method specified in GB / T7962.18-2010.

[0090] In some embodiments, the Knoop hardness (H K ) is 670×10 7 Pa or more, preferably 680×10 7 Pa or more, more preferably 690×10 7 Pa or more, more preferably 695×10 7 Pa or above.

[0091] <Young's modulus>

[0092] Young's modulus (E) is calculated using the following formula by ultrasonic testing of its longitudinal wave velocity and transverse wave velocity.

[0093]

[0094] Where: E is Young's modulus, Pa;

[0095] G is the shear modulus, Pa;

[0096] V T is the shear wave velocity, m / s;

[0097] V S is the longitudinal wave velocity, m / s;

[0098] ρ is the glass density, g / cm 3 .

[0099] In some embodiments, the Young's modulus (E) of the optical glass of the present invention is 10500×10 7 Pa or more, preferably 11000×10 7 Pa or more, more preferably 11500×10 7 Pa or above.

[0100] <Abrasion>

[0101] Abrasiveness of optical glass (F A ) refers to the value obtained by multiplying the ratio of the wear volume of the sample to the wear volume (volume) of the standard sample (H-K9 glass) under exactly the same conditions by 100, and is expressed by the following formula:

[0102] F A =V / V0×100=(W / ρ) / (W0 / ρ0)×100

[0103] Where: V—volume wear of the sample being tested;

[0104] V0—Volume loss of standard sample;

[0105] W—mass wear loss of the sample being tested;

[0106] W0—standard sample mass wear;

[0107] ρ—density of the sample being tested;

[0108] ρ0—standard sample density.

[0109] In some embodiments, the abrasiveness (F A ) has a lower limit of 75, a preferred lower limit of 80, and a more preferred lower limit of 86.

[0110] In some embodiments, the abrasiveness (F A ) has an upper limit of 120, a preferred upper limit of 110, and a more preferred upper limit of 105.

[0111] <Bubble Degree>

[0112] The bubble degree of optical glass is tested according to the method specified in GB / T7962.8-2010.

[0113] In some embodiments, the bubble degree of the optical glass of the present invention is above grade A, preferably above grade A0, and more preferably above grade A1. 00 class.

[0114] [Method for producing optical glass]

[0115] The manufacturing method of the optical glass of the present invention is as follows: the glass of the present invention is produced using conventional raw materials and processes, including but not limited to using oxides, hydroxides, complex salts (such as carbonates, nitrates, sulfates, etc.), boric acid, etc. as raw materials, and after the ingredients are prepared according to the conventional method, the prepared furnace materials are put into a melting furnace (such as platinum or platinum alloy crucible) at 1200-1500°C for melting, and after clarification and homogenization, a homogeneous molten glass without bubbles and undissolved substances is obtained, and the molten glass is cast in a mold and annealed. Those skilled in the art can appropriately select raw materials, process methods and process parameters according to actual needs.

[0116] [Glass preforms and optical components]

[0117] The prepared optical glass can be used to make a glass preform by means of direct drop molding, grinding, or compression molding such as hot press molding. That is, the molten optical glass can be directly precision drop molded into a glass precision preform, or the glass preform can be made by mechanical processing such as grinding and grinding, or the preform for compression molding made of the optical glass can be made by hot press molding and then grinding. It should be noted that the means for preparing the glass preform are not limited to the above means.

[0118] As described above, the optical glass of the present invention is useful for various optical elements and optical designs, and it is particularly preferred to form a preform from the optical glass of the present invention and use the preform to perform re-hot pressing, precision stamping, etc. to produce optical elements such as lenses and prisms.

[0119] The glass preform and optical element of the present invention are both formed of the optical glass of the present invention. The glass preform of the present invention has the excellent properties of optical glass; the optical element of the present invention has the excellent properties of optical glass, and can provide various optical elements such as lenses and prisms with high optical value.

[0120] Examples of the lens include various lenses having spherical or aspherical lens surfaces, such as a concave meniscus lens, a convex meniscus lens, a biconvex lens, a biconcave lens, a plano-convex lens, and a plano-concave lens.

[0121] [Optical instruments]

[0122] The optical element formed by the optical glass of the present invention can be used to manufacture optical instruments such as photographic equipment, video equipment, projection equipment, display equipment, vehicle-mounted equipment and monitoring equipment.

[0123] Example

[0124] <Optical Glass Example>

[0125] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided.

[0126] This embodiment adopts the above optical glass manufacturing method to obtain optical glasses having the compositions shown in Tables 2 to 4. In addition, the properties of each glass are measured by the testing method described in the present invention, and the measurement results are shown in Tables 2 to 4.

[0127] Table 2.

[0128]

[0129]

[0130] Table 3.

[0131]

[0132]

[0133]

[0134] Table 4.

[0135]

[0136]

[0137] <Glass Preform Example>

[0138] The glass obtained from optical glass examples 1 to 24# is used, for example, by grinding processing, or by molding methods such as hot pressing, precision stamping, etc., to make preforms of various lenses, prisms, etc., such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses.

[0139] <Optical Element Embodiment>

[0140] The preforms obtained in the above-mentioned glass preform embodiments are annealed to reduce the internal stress of the glass and fine-tune the refractive index so that the optical properties such as the refractive index reach the desired values.

[0141] Next, each preform is ground and polished to produce various lenses and prisms such as concave meniscus lenses, convex meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses. The surface of the obtained optical element may be coated with an anti-reflection film.

[0142] <Optical Instrument Embodiment>

[0143] The optical element obtained by the above-mentioned optical element embodiment is optically designed to form an optical component or optical assembly by using one or more optical elements, and can be used in, for example, imaging equipment, sensors, microscopes, medical technology, digital projection, communications, optical communication technology / information transmission, optics / lighting in the automotive field, lithography technology, excimer lasers, wafers, computer chips, and integrated circuits and electronic devices including such circuits and chips.

Claims

1. Optical glass, characterized in that: Its components, expressed in weight percentage, include: SiO2: 2-18%; B2O3: 8-22%; La2O3: 40-55%; Y2O3: 3-18%; ZrO2: 1-15%; Nb2O5: 2-15%, wherein La2O3 / (B2O3+Nb2O5) is 1.2-5.

0.

2. The optical glass according to claim 1, characterized in that: Its components are expressed in weight percentage and further contain: Ta2O5: 0-10%; and / or Gd2O3: 0-9%; and / or TiO2: 0-6%; and / or RO: 0-10%; and / or Rn2O: 0-8%; and / or WO3: 0-8%; and / or ZnO: 0-10%; and / or Al2O3: 0-5%; and / or Yb2O3: 0-8%; and / or GeO2: 0-5%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

3. Optical glass, characterized in that: Contains SiO2, B2O3, La2O3, Y2O3, ZrO2, Nb2O5, and the components are expressed in weight percentage, wherein La2O3 / (B2O3+Nb2O5) is 1.2 to 5.0, and the refractive index of the optical glass is n d is 1.82~1.89, Abbe number v d is 37-44, and Young's modulus E is 10500×10 7 Pa or above.

4. The optical glass according to claim 3, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 2-18%; and / or B2O3: 8-22%; and / or La2O3: 40-55%; and / or Y2O3: 3-18%; and / or ZrO2: 1-15%; and / or Nb2O5: 2-15%; and / or Ta2O5: 0-10%; and / or Gd2O3: 0-9%; and / or TiO2: 0-6%; and / or RO: 0-10%; and / or Rn2O: 0-8 %; and / or WO3: 0-8%; and / or ZnO: 0-10%; and / or Al2O3: 0-5%; and / or Yb2O3: 0-8%; and / or GeO2: 0-5%; and / or clarifier: 0-1%, wherein RO is one or more of MgO, CaO, SrO, and BaO, Rn2O is one or more of Li2O, Na2O, and K2O, and the clarifier is one or more of Sb2O3, SnO, SnO2, and CeO2.

5. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage and meet one or more of the following 7 conditions: 1) (ZnO + Ta2O5) / Nb2O5 is less than 2.0, preferably (ZnO + Ta2O5) / Nb2O5 is less than 1.5, more preferably (ZnO + Ta2O5) / Nb2O5 is less than 1.0, and further preferably (ZnO + Ta2O5) / Nb2O5 is 0.1 to 0.8; 2) (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.5, preferably (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.4, more preferably (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.3, and further preferably (Gd2O3+Ta2O5+WO3) / La2O3 is less than 0.2; 3) (Ta2O5+Gd2O3) / Y2O3 is less than 1.0, preferably (Ta2O5+Gd2O3) / Y2O3 is less than 0.8, more preferably (Ta2O5+Gd2O3) / Y2O3 is less than 0.5, and further preferably (Ta2O5+Gd2O3) / Y2O3 is less than 0.2; 4) La2O3 / (B2O3+Nb2O5) is 1.3 to 4.0, preferably La2O3 / (B2O3+Nb2O5) is 1.5 to 3.5, and more preferably La2O3 / (B2O3+Nb2O5) is 1.7 to 2.7; 5) (ZnO + WO3) / Nb2O5 is 3.0 or less, preferably (ZnO + WO3) / Nb2O5 is 2.0 or less, more preferably (ZnO + WO3) / Nb2O5 is 1.5 or less, and further preferably (ZnO + WO3) / Nb2O5 is 0.2 to 1.0; 6) (Gd2O3+ZnO) / Y2O3 is less than 2.0, preferably (Gd2O3+ZnO) / Y2O3 is less than 1.5, more preferably (Gd2O3+ZnO) / Y2O3 is less than 1.0, and further preferably (Gd2O3+ZnO) / Y2O3 is less than 0.8; 7) (B2O3+RO) / La2O3 is 0.15-0.7, preferably (B2O3+RO) / La2O3 is 0.15-0.6, more preferably (B2O3+RO) / La2O3 is 0.18-0.5, and further preferably (B2O3+RO) / La2O3 is 0.2-0.4, and the RO is one or more of MgO, CaO, SrO, and BaO.

6. The optical glass according to any one of claims 1 to 4, characterized in that: Its components are expressed in weight percentage, wherein: SiO2: 4-15%, preferably SiO2: 6-12%; and / or B2O3: 10-20%, preferably B2O3: 12-18%; and / or La2O3: 43-55%, preferably La2O3: 46-52%; and / or Y2O3: 5-15%, preferably Y2O3: 7-13%; and / or ZrO2: 2-12%, preferably ZrO2: 3-10%; and / or or Nb2O5: 3-13%, preferably Nb2O5: 5-11%; and / or Ta2O5: 0-5%, preferably Ta2O5: 0-2%, more preferably no Ta2O5; and / or Gd2O3: 0-5%, preferably Gd2O3: 0-2%, more preferably no Gd2O3; and / or TiO2: 0-4%, preferably TiO2: 0-2%; and / or RO: 0-5%, preferably RO: 0-2%, more preferably no RO; and / or Rn2O: 0-4%, preferably Rn2O: 0-2%, more preferably no Rn2O; and / or WO3: 0-6%, preferably WO3: 0-4%; and / or ZnO: 1-8%, preferably ZnO: 2-7%; and / or Al2O3: 0-3%, preferably Al2O3: 0-1%, more preferably no Al2O3; and / or Yb2O3: 0-3%, preferably Yb2O3: 0-1%, more preferably no Contains Yb2O3; and / or GeO2: 0-3%, preferably GeO2: 0-1%, more preferably contains no GeO2; and / or clarifier: 0-0.5%, preferably clarifier: 0-0.2%, the RO is one or more of MgO, CaO, SrO, BaO, Rn2O is one or more of Li2O, Na2O, K2O, the clarifier is one or more of Sb2O3, SnO, SnO2, CeO2.

7. The optical glass according to any one of claims 1 to 4, characterized in that: The refractive index n of the optical glass d is 1.82 to 1.89, preferably 1.83 to 1.88, more preferably 1.84 to 1.87, and the Abbe number v d It is 37-44, preferably 38-43, and more preferably 39-42.

8. The optical glass according to any one of claims 1 to 4, characterized in that: The density of the optical glass is 5.00 g / cm 3 Below, preferably 4.90g / cm 3 Below, more preferably 4.80g / cm 3 Below; and / or thermal expansion coefficient α -30 / 70℃ 85×10 -7 / K or less, preferably 80×10 -7 / K or less, more preferably 75×10 -7 / K or less, more preferably 70×10 -7 / K or less; and / or water resistance stability D W 2 or more, preferably 1; and / or acid resistance stability D A Two or more types, preferably one type; and / or 70 400nm or less, preferably λ 70 395nm or less, preferably λ 70 390nm or less; and / or λ5 is 350nm or less, preferably λ5 is 345nm or less, more preferably λ5 is 340nm or less; and / or weather resistance CR is 2 or more, preferably 1; and / or Knoop hardness H K 670×10 7 Pa or more, preferably 680×10 7 Pa or more, more preferably 690×10 7 Pa or more, more preferably 695×10 7 Pa or more; and / or Young's modulus E is 10500×10 7 Pa or more, preferably 11000×10 7 Pa or more, more preferably 11500×10 7 Pa or above; and / or wear degree F A The foaming degree is 75 to 120, preferably 80 to 110, and more preferably 86 to 105; and / or the foaming degree is A grade or higher, preferably A0 grade or higher, and more preferably A 00 class.

9. A glass preform, characterized in that: Made of the optical glass described in any one of claims 1 to 8.

10. An optical element, characterized in that The optical glass is made of the optical glass described in any one of claims 1 to 8, or the glass preform described in claim 9.

11. An optical instrument, characterized in that Contains the optical glass according to any one of claims 1 to 8, and / or contains the optical element according to claim 10.

Citation Information

Patent Citations

  • Optical glass and optical element

    CN104010982A

  • Composition used for glass, alkaline earth aluminosilicate glass, making method of alkaline earth aluminosilicate glass, and application of composition or alkaline earth aluminosilicate glass

    CN107032604A

  • Optical glass and optical element

    CN107285622A

  • Glass, glass material for press molding, optical element blank, and optical element

    CN109641781A

  • Optical glass, glass prefabricated part, optical element and optical instrument

    CN109775981A