High-refractive-index material based on biomass magnolol and honokiol

Through the copolymerization of magnolol and magnolol-based monomers with thiol/thiophenol, the difficulty in synthesizing existing high-refractive materials and the balance of refractive index and Abbe number are solved, and high refractive index and high Abbe number are achieved. Simple and efficient preparation of several optical resin materials suitable for a variety of optical applications.

CN118745246AActive Publication Date: 2024-10-08SHANGHAI INST OF ORGANIC CHEM CHINESE ACAD OF SCI

Patent Information

Application Number
CN202410739887.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-08
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

Existing high-refractive materials are difficult and costly to synthesize, or have a low refractive index, making it difficult to balance the refractive index and Abbe number, and unable to meet the needs of many optical applications.

Method used

Resin materials with high refractive index and high Abbe number are prepared by copolymerizing magnolol and magnolol-based monomers with thiol/thiophenol monomers through photocuring method.

Benefits of technology

Achieving a balance of high refractive index and high Abbe number provides a simple and efficient preparation method suitable for a variety of optical applications, such as lenses, infrared-emitting materials, and anti-reflective coatings for optical devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDA0004884402730000011
    Figure FDA0004884402730000011
  • Figure HDA0004884402750000011
    Figure HDA0004884402750000011
  • Figure HDA0004884402750000021
    Figure HDA0004884402750000021
Patent Text Reader

Abstract

The invention relates to a high refractive index material based on biomass magnolol and honokiol. Specifically, the high refractive index material provided by the invention can be obtained by carrying out a photocuring reaction on a photocurable monomer and various mercaptans / thiophenol under photoinitiation, and the curable monomer is derived from an allyl functional group-containing monomer derived from biomass magnolol and honokiol. The high refractive index material provided by the invention has good optical performance, and especially not only has a high refractive index (1.67-1.71), but also has a relatively high Abbe number (35-24).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of optical resins, and in particular to a high-refractive material based on biomass magnolol and honokiol. Background Art

[0002] Functional materials with a high refractive index are important in modern optical devices. Such materials can reduce the thickness and curvature of optical components, making them more widely used. At the same time, the Abbe number also plays an important role in the application of optical materials. It represents the dispersion ability of the medium. The medium with a high Abbe number has a lower dispersion effect, making the mirror image clearer. Compared with inorganic materials such as glass, organic high refractive index materials have the advantages of light weight, easy processing, and high mechanical strength.

[0003] However, the monomer preparation of the high-refractive materials that have been developed at this stage is often difficult to synthesize or has the limitation of high cost; while the low-cost and easy-to-synthesize materials such as PMMA, PC and other optical materials have a low refractive index and cannot meet the application requirements of many scenarios. In particular, it is difficult to reconcile the balance between the refractive index and the Abbe number for most materials. Therefore, the field urgently needs a new type of optical organic material with high refractive index and high Abbe number that can be directly photocured, has a simple and efficient preparation method, and is directly photocurable. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a resin material with high refractive index and high Abbe number, wherein the material is prepared by curing and copolymerizing magnolol / honokiol-based monomers with thiol / thiophenol monomers.

[0005] In a first aspect of the present invention, there is provided a solidified material, wherein the solidified material is prepared by copolymerizing component (a) and component (b):

[0006] (a) a resin monomer; the resin monomer is selected from the group consisting of a compound having a structure represented by formula (I), a compound having a structure represented by formula (II), or a combination thereof;

[0007]

[0008] in,

[0009] R1, R2, R3 and R4 are each independently selected from the group consisting of hydrogen, C 1-6 Alkyl, C 2-6 Alkenyl, C 1-15 Alkylsilyl;

[0010] One or more hydrogen atoms on the above groups are optionally substituted by a substituent selected from the group consisting of halogen, C 1-4 Alkyl, C 2-4Alkenyl, C 2-4 Alkynyl, phenyl, or 1, 2 or 3 R a Substituted phenyl; R a Selected from the group consisting of halogen, C 1-6 Alkyl, C 2-6 alkenyl;

[0011] (b) a thiol monomer; the thiol monomer is selected from the group consisting of methanethiol, 1,2-ethanethiol, 1,1-propanethiol, 1,2-propanethiol, 1,3-propanethiol, 2,2-propanethiol, 1,6-hexanethiol, 1,2,3-propanetriol, 1,1-cyclohexanethiol, 1,2-cyclohexanethiol, 2,2-dimethylpropane-1,3-thiol, 3,4-dimethoxybutane-1,2-thiol, 2-methylcyclohexane-2,3-thiol, bicyclo[2,2,1]heptyl-exo-cis-2,3-thiol, 1,1-bis(mercaptomethyl)cyclohexane, bis(2-mercaptoethyl)thiomalate, 2,3-dimercaptosuccinic acid (2-mercaptoethyl ester), 2,3-dimercapto-1-propanethiol, 1,3-Bis(2-mercaptoethyl)ether, ethylene glycol bis(2-mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), trimethylolpropane tris(2-mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), 1,2-bis(2-mercaptoethylthio)-3-mercaptopropane), 5,7-dimercaptomethyl-1,11- Dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, 4,6-bis(mercaptomethylthio)-1,3-dithiane, 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithiacyclobutane, 1,2-dimercaptobenzene, 1,3-dimercaptobenzene, 1,4-dimercaptobenzene, 1,2-bis(mercaptomethyl)benzene, 1,3-bis(mercaptomethyl)benzene, 1,4-bis(mercaptomethyl)benzene, 1,2-bis(mercaptoethyl)benzene, 1,3-bis(mercaptoethyl)benzene, 1,4- Bis(mercaptoethyl)benzene, 1,2-bis(mercaptomethyleneoxy)benzene, 1,3-bis(mercaptomethyleneoxy)benzene, 1,4-bis(mercaptomethyleneoxy)benzene, 1,2-bis(mercaptoethyleneoxy)benzene, 1,3-bis(mercaptoethyleneoxy)benzene, 1,4-bis(mercaptoethyleneoxy)benzene, 1,2,3-trimercaptobenzene, 1,2,4-trimercaptobenzene, 1,3,5-trimercaptobenzene, 1,2,3-tris(mercaptomethyl)benzene, 1,2,4-tris(mercaptomethyl)benzene, 1,3,5-tris(mercaptomethyl)benzene, 1,2,3-tris(mercaptoethyl)benzene, 1,2,4-tris(mercaptoethyl)benzene, 1,3,5-tris(mercaptoethyl)benzene, 1,2,3-tris(mercaptomethyleneoxy)benzene, 1,2,4-Tris(mercaptomethyleneoxy)benzene, 1,3,5-tris(mercaptomethyleneoxy)benzene, 1,2,3-tris(mercaptoethyleneoxy)benzene, 1,2,4-tris(mercaptoethyleneoxy)benzene, 1,3,5-tris(mercaptoethyleneoxy)benzene, 1,2,3,4-tetramercaptobenzene, 1,2,3,5-tetramercaptobenzene, 1,2,4,5-tetramercaptobenzene, 1,2,3,4-tetrakis(mercaptomethyl)benzene, 1,2,3,5-tetrakis(mercaptomethyl)benzene, 1,2,4,5-tetrakis(mercaptomethyl)benzene, 1,2,3,4-tetrakis(mercaptoethyl)benzene, 1,2,3,5-tetrakis(mercaptoethyl)benzene, 1,2,4,5-tetrakis(mercaptoethyl)benzene, 1,2,3,4-tetrakis(mercaptoethyl)benzene, 1,2, 3,5-Tetrakis(mercaptomethyleneoxy)benzene, 1,2,4,5-Tetrakis(mercaptomethyleneoxy)benzene, 1,2,3,4-Tetrakis(mercaptoethyleneoxy)benzene, 1,2,3,5-Tetrakis(mercaptoethyleneoxy)benzene, 1,2,4,5-Tetrakis(mercaptoethyleneoxy)benzene, 2,2'-dimercaptobiphenyl, 4,4'-dimercaptobiphenyl, 4,4'-dimercaptobibenzyl, 2,5-toluenedithiols, 3,4-toluenedithiols, 1,4-naphthalenedithiols, 1,5-naphthalenedithiols, 2,6-naphthalenedithiols, 2,7-naphthalenedithiols, 2,4-dimethylbenzene-1,3-dithiol, 4,5-dimethylbenzene-1,3-dithiol, 9,10-anthracenedimethanethiol, 1,3-bis(p-methoxyphenyl)propane-2, 2-dithiol, 1,3-diphenylpropane-2,2-dithiol, phenylmethane-1,1-dithiol, 2,4-di(p-mercaptophenyl)pentane, 2-methylamino-4,6-dimercapto-s-triazine, 2-ethylamino-4,6-dimercapto-s-triazine, 2-amino-4,6-dimercapto-s-triazine, 2-morpholino-4,6-dimercapto-s-triazine, 2-cyclohexylamino-4,6-dimercapto-s-triazine, 2-methoxy-4,6-dimercapto-s-triazine, 2-phenoxy-4,6-dimercapto-s-triazine, 2-thiophenoxy-4,6-dimercapto-s-triazine, 2-thiobutyloxy-4,6-dimercapto-s-triazine, 1,2-bis(mercaptomethylthio)benzene, 1,3-bis(mercaptomethylthio)benzene 1,4-bis(mercaptomethylthio)benzene, 1,2-bis(mercaptoethylthio)benzene, 1,3-bis(mercaptoethylthio)benzene, 1,4-bis(mercaptoethylthio)benzene, 1,2,3-tris(mercaptomethylthio)benzene, 1,2,4-tris(mercaptomethylthio)benzene, 1,3,5-tris(mercaptomethylthio)benzene, 1,2,3-tris(mercaptoethylthio)benzene, 1,2,4-tris(mercaptoethylthio)benzene, 1,3,5-tris(mercaptoethylthio)benzene, 1,2,3,4-tetrakis(mercaptomethylthio)benzene, 1,2,3,5-tetrakis(mercaptomethylthio)benzene, 1,2,4,5-tetrakis(mercaptomethylthio)benzene, 1,2,3,4-tetrakis(mercaptoethylthio)benzene, 1,2,3,5-Tetrakis(mercaptoethylthio)benzene, 1,2,4,5-Tetrakis(mercaptoethylthio)benzene, bis(mercaptomethyl)sulfide, bis(mercaptoethyl)sulfide, bis(mercaptopropyl)sulfide, bis(mercaptomethylthio)methane, bis(2-mercaptoethylthio)methane, bis(3-mercaptopropyl)methane, 1,2-bis(mercaptomethylthio)ethane, 1,2-(2-mercaptoethylthio)ethane, 1,2-(3-mercaptopropyl)ethane, 1,3-bis(mercaptomethylthio)propane, 1,3-bis(2-mercaptoethylthio)propane, 1,3-bis(3-mercaptopropylthio)propane, 1,2,3-tris(mercaptomethylthio)propane, 1,2,3-tris(2-mercaptoethylthio)propane, 1,2,3-tris( 3-Mercaptopropylthio)propane, tetrakis(mercaptomethylthiomethyl)methane, tetrakis(2-mercaptoethylthiomethyl)methane, tetrakis(3-mercaptopropylthiomethyl)methane, bis(2,3-dimercaptopropyl)sulfide, 2,5-dimercapto-1,4-dithiane, bis(mercaptomethyl)disulfide, bis(mercaptoethyl)disulfide, bis(mercaptopropyl)disulfide, 1,5-dimercapto-3-thiapentane, hydroxymethyl sulfide bis(2-mercaptoacetate), hydroxymethyl sulfide bis(3-mercaptopropionate), hydroxyethyl sulfide bis(2-mercaptoacetate), hydroxyethyl sulfide bis(3-mercaptopropionate), hydroxypropyl sulfide bis(2-mercaptoacetate), hydroxypropyl sulfide bis(3-mercaptopropionate), hydroxymethyl disulfide Bis(2-mercaptoacetate), hydroxymethyl disulfide bis(3-mercaptopropionate), hydroxyethyl disulfide bis(2-mercaptoacetate), hydroxyethyl disulfide bis(3-mercaptopropionate), hydroxypropyl disulfide bis(2-mercaptoacetate), hydroxypropyl disulfide bis(3-mercaptopropionate), 2-mercaptoethyl ether bis(2-mercaptoacetate), 2-mercaptoethyl ether bis(3-mercaptopropionate), 1,4-dithiane-2,5-diol bis(2-mercaptoacetate), 1,4-dithiane-2,5-diol bis(3-mercaptopropionate), thioglycolic acid bis(2-mercaptoethyl ester), 4,4-thiodibutyric acid bis(2-mercaptoethyl ester), dithiodisulfide Bis(2-mercaptoethyl) acetate, bis(2-mercaptoethyl) dithiodipropionate, bis(2-mercaptoethyl) 4,4-dithiodibutyrate, bis(2-mercaptoethyl) dithiodiacetate, bis(2,3-dimercaptopropyl) dithiodipropionate, bis(2,3-dimercaptopropyl) dithiodiacetate, 2,3-dimercaptopropyl dithiodipropionate, 2,2'-thiodiethanethiol, biphenyl-4,4'-dithiol, biphenyl-4,4'-dithiol, 4,4'-thiodiphenylthiol, bis(2-mercaptoethyl) ether, 3,3'-dimercaptopropyl ether, 2,5-dimethylmercapto-1,4-dithiane, 2,3-dithio(2-mercapto)-1-propanethiol, 2,3-dithio(2-mercapto)-1-propanethiol, butanediol bis(thioglycolate), butanediol bis(thiopropionate), diethylene glycol bis(thioglycolate), diethylene glycol bis(thiopropionate), 2-[(2-mercaptoethyl)thio]-1,3-propanedithiol, 2,2'-[[2-[[2-[(2-mercaptoethyl)thio]ethyl]thio]-1,3-propanediyl]bis(thio)]bis[ethanethiol], 7-[[(2-mercaptoethyl)thio]methyl]-3,6,9,12-tetrathiotetradecane-1,14-dithiol, 1,3,4,6-tetrakis(2-mercaptoethyl)tetrahydroimidazo[4,5-d]imidazole-2,5(1H,3H)-dione, dicyclic thiomethyl sulfide, or a combination thereof.

[0012] In another preferred embodiment, R1, R2, R3 and R4 are each independently selected from the following group: hydrogen, C 1-4 Alkyl, C 2-4 Alkenyl, C 1-12 Alkylsilyl.

[0013] In another preferred embodiment, R1, R2, R3 and R4 are all allyl groups.

[0014] In another preferred embodiment, the resin monomer is selected from the following group:

[0015]

[0016] In a preferred example, the thiol monomer is selected from the following group: 4,4'-thiodibenzenethiol, 2,5-dimethylmercapto-1,4-dithiane, 2,5-dimercapto-1,4-dithiane, dicyclic thiomethyl sulfide, 2,3-dithio(2-mercapto)-1-propanethiol, pentaerythritol tetrakis(2-thioglycolate), or a combination thereof.

[0017] In a preferred embodiment, the molar ratio of the resin monomer to the thiol monomer is 1:(1-4).

[0018] In another preferred embodiment, the quantitative ratio of the olefin functional groups in the resin monomer to the thiol functional groups in the thiol monomer is 1:(0.5-1.5); preferably 1:1.

[0019] In another preferred embodiment, the curable material is prepared by subjecting a resin monomer and a thiol monomer to a photocuring reaction.

[0020] In a preferred embodiment, the curable material is prepared by copolymerizing component (a) and component (b) in the presence of a photoinitiator;

[0021] Wherein, the photoinitiator is selected from the following group: 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, 2,4,6-trimethylbenzoylphosphonic acid ethyl ester, 2-methyl-1-[4-methylthiophenyl]-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzoin dimethyl ether, methyl o-benzoylbenzoate, benzophenone, 4-phenylbenzophenone, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone, photoinitiator 754 (benzoylformate mixture), phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-hydroxy-1-(4-(2-hydroxy-2-methylpropionylphenyl)benzyl)-2-methyl-1-propanone, bis-2,6-difluoro-3-pyrrolylphenyl titanocene, ethyl 4-dimethylaminobenzoate;

[0022] Preferably, the photoinitiator is selected from the following group: benzoin dimethyl ether, 1-hydroxy-cyclohexyl-phenyl ketone, or a combination thereof.

[0023] The second aspect of the present invention provides a method for preparing the curing material as described in the first aspect of the present invention, comprising the steps of: copolymerizing component (a) and component (b) in the presence of a photoinitiator to prepare the curing material.

[0024] In a preferred embodiment, the reaction is carried out under solvent-free conditions, comprising the following steps:

[0025] A1. Mixing a resin monomer, a thiol monomer and a photoinitiator to obtain a prepolymer;

[0026] B2. The prepolymer is molded to obtain a preform;

[0027] C1. Place the preform under the irradiation of light source B to perform a photocuring reaction to obtain a high-refractive material.

[0028] In a preferred example, the light source B has an ultraviolet light wavelength of 310-400 nm.

[0029] In another preferred embodiment, the intensity of the light source B is 80-130uW / cm 2 ; preferably 100-120uW / cm 2 .

[0030] In another preferred embodiment, in the step C1, the irradiation time of the light source B is 10 to 300 min; preferably 10 to 60 min; more preferably 10 to 30 min.

[0031] In another preferred embodiment, in the step C1, the irradiation time of the light source B is 120 to 250 minutes.

[0032] In another preferred embodiment, in the step C1, the irradiation time of the light source B is 180 to 240 minutes.

[0033] In another preferred embodiment, the temperature of the photocuring reaction is 20-30°C.

[0034] In a preferred embodiment, the photocuring reaction is carried out in the presence of solvent A, comprising the following steps:

[0035] A2. mixing a resin monomer, a thiol monomer, a solvent A and a photoinitiator to obtain a prepolymer mixed solution; removing the solvent A from the prepolymer mixed solution to obtain a prepolymer;

[0036] B2. The prepolymer is molded to obtain a preform;

[0037] C2. placing the preform under the irradiation of light source B to perform a photocuring reaction to obtain a high-refractive material;

[0038] Wherein, the boiling point range of the solvent A is 30-150°C.

[0039] In a preferred example, the solvent A is selected from the following group: dichloromethane, tetrahydrofuran, ethanol, ethyl acetate, n-hexane, diethyl ether, or a combination thereof.

[0040] In another preferred embodiment, the step A2 comprises the following steps: heating the prepolymer mixed solution to the boiling point of the solvent to volatilize and remove the solvent A from the prepolymer mixed solution to obtain a prepolymer.

[0041] In another preferred embodiment, the step A2 comprises the following steps: placing the prepolymer mixed solution under a light source A for irradiation, so that the solvent A is volatilized and removed from the prepolymer mixed solution to obtain a prepolymer.

[0042] In another preferred embodiment, in step A2, the light source A is ultraviolet light with a wavelength of 310-400 nm.

[0043] In another preferred embodiment, in step A2, the intensity of the light source A is 80-130 uW / cm 2 ; preferably 100-120uW / cm 2 .

[0044] In another preferred embodiment, in step A2, the irradiation time of the light source A is 1 to 3 hours, preferably 1 to 2 hours.

[0045] In another preferred embodiment, in step C2, the irradiation time of the light source B is 10 to 300 min; preferably 120 to 250 min; more preferably 180 to 240 min.

[0046] In another preferred embodiment, in step C2, the irradiation time of the light source B is 10 to 60 minutes.

[0047] In another preferred embodiment, in step C2, the irradiation time of the light source B is 10 to 30 minutes.

[0048] In another preferred embodiment, the reaction is carried out in the presence of solvent B, comprising the following steps:

[0049] A3. Mixing a resin monomer, a thiol monomer, a solvent B and a photoinitiator to obtain a prepolymer solution;

[0050] B3. The prepolymer solution is molded to obtain a preform;

[0051] C3. The preform is placed under the irradiation of light source B to perform a photocuring reaction to obtain a high-refractive material;

[0052] The boiling point of the solvent B is 100°C-200°C.

[0053] In another preferred embodiment, the solvent B is selected from the following group: benzene, toluene, xylene, trimethylbenzene, chlorobenzene, chloroform, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, or a combination thereof.

[0054] In another preferred embodiment, the prepolymer solution can also be obtained by the following steps: re-dissolving the prepolymer in solvent B.

[0055] In a preferred embodiment, the molding is selected from the following group: inverted molding, drop coating, solution drop coating, solution spin coating, or a combination thereof.

[0056] In another preferred embodiment, the molding comprises the following steps: drop coating the prepolymer on a substrate to obtain a preform.

[0057] In another preferred embodiment, the substrate is a frosted glass substrate or a flat glass substrate.

[0058] In another preferred embodiment, the molding comprises the following steps: pouring the prepolymer into a mold to obtain a preform.

[0059] In another preferred embodiment, the molding comprises the following steps: dripping the prepolymer solution to obtain a preform.

[0060] In another preferred embodiment, the molding comprises the following steps: spin coating the prepolymer solution to obtain a preform.

[0061] The third aspect of the present invention provides a use of the solidified material according to the first aspect of the present invention, characterized in that it is used for preparing a high-refractive material.

[0062] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below (such as embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here. BRIEF DESCRIPTION OF THE DRAWINGS

[0063] Figure 1 The refractive index and Abbe number of the optical resin materials P1 to P8 of the present invention are shown.

[0064] Figure 2 The storage modulus and glass transition temperature of the optical resin materials P3, P6, P8 and P4 of the present invention are shown.

[0065] Figure 3 The storage modulus and glass transition temperature of the optical resin materials P1, P5, P7 and P2 of the present invention are shown. Specific implementation plan

[0066] After extensive and in-depth experimental research and a large number of screenings, the inventors have developed for the first time a class of allyl-containing functional monomers derived from biomass magnolol / honokiol, and through the thiol-olefin reaction, the above-mentioned alkenyl-containing monomers can be converted into optical materials with high refractive index and high Abbe number. The monomers of the present invention are easy to synthesize, easy to purify, and have a simple polymerization process. They are suitable for use as matrix resins in the lens industry (for example, manufacturing optical lenses), infrared emitting materials and anti-reflective coatings of optical devices, encapsulation resins of light-emitting diodes (LEDs), and microlenses of complementary metal oxide semiconductor image sensors in digital devices. Based on this, the inventors have completed the present invention.

[0067] the term

[0068] In the present invention, unless otherwise specified, the terms used have the general meanings known to those skilled in the art.

[0069] Unless otherwise specified, the term "C 1-n " means that the group has 1-n carbon atoms, for example, "C 1-12 " means that the group has 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12 carbon atoms; "C 6~10 ” means that the group has 6, 7, 8, 9 or 10 carbon atoms.

[0070] The term "C 2-6 "Alkenylphenyl" refers to a substituted C 2-6 The alkenyl group is formed by losing a hydrogen atom from the benzene ring of the alkenyl group, such as styryl, 1-propenylphenyl, 1-butenylphenyl, etc.

[0071] The term "C 1-15 "Alkylsilyl" means A group, wherein R1, R2, and R3 are each independently C 1-6 Alkyl groups, such as trimethylsilyl, triethylsilyl, triisopropylsilyl, tributylsilyl and the like.

[0072] The term "halogen" refers to F, Cl, Br or I.

[0073] The term "C 1-6 "Alkyl" refers to a straight or branched chain alkyl group containing 1 to 6 carbon atoms, such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, neopentyl, tert-pentyl, or the like. 1-4 "Alkyl" has a similar meaning.

[0074] The term "C 2-6 "Alkenyl" refers to a straight or branched alkenyl group having 2 to 6 carbon atoms and containing one double bond, including but not limited to ethenyl, propenyl, butenyl, isobutenyl, pentenyl and hexenyl. 2-4 "Alkenyl" has a similar meaning.

[0075] The term "C 2-4 The term "alkynyl" refers to a straight or branched chain alkynyl group having 2 to 4 carbon atoms and containing one triple bond, including but not limited to ethynyl, propynyl, butynyl, isobutynyl, etc.

[0076] The term "Abbe number" is a physical quantity used to measure the degree of light dispersion in a transparent medium. The smaller the Abbe number, the more severe the dispersion. The generally used calculation formula is (nd-1) / (nF-nC), where nd, nF and nC are the refractive indices of the material under d-light, F-light and C-light respectively.

[0077] The term "room temperature" refers to 20 to 30°C.

[0078] The main advantages of the present invention are:

[0079] 1. The magnolol and honokiol used in the present application have a biphenyl structure, which can contribute a high refractive index, and the allyl groups in their structures can form cross-linking points, which is conducive to the formation of copolymer materials.

[0080] 2. The magnolol and honokiol used in the present application are derived from plants and can be used directly without complicated synthesis processes. They are also easy to be derivatized and synthesized into photocurable monomers (i.e., resin monomers).

[0081] 3. The high-refractive material of the present application can be obtained by curing a photocurable monomer with a variety of thiol / thiophenol monomers under light initiation, and the preparation method is simple, convenient and efficient; wherein the curable monomer is derived from a monomer containing an allyl functional group derived from biomass magnolol and honokiol.

[0082] 4. The optical resin material in the present application has good optical properties. Among existing optical resin materials, optical resins with high refractive index usually have low Abbe numbers. For example, optical resins with a refractive index of about 1.7 only have an Abbe number of 10-20. However, the optical resin in the present application not only has a high refractive index (1.67-1.71) but also has a high Abbe number (35-24).

[0083] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0084] Unless otherwise indicated, percentages and parts are by weight.

[0085] Unless otherwise stated, reactions were performed at room temperature.

[0086] Example 1 Preparation of 5,5'-di-2-propene-1-yl-2,2'-bis(2-propene-1-yloxy)-1,1'-biphenyl (magnolia phenol bisallyl ether) (S1)

[0087]

[0088] At room temperature (rt), magnolol (10.654 g) and 160 mL of dimethyl sulfoxide were added to a 500 mL three-necked flask and stirred until dissolved to form a yellow solution. Sodium hydride (60%, 3.6 g in total) was added in 10-15 batches. After the addition, the solution gradually became a suspension, and foam floated up and down on the liquid surface. After stirring for about 40 minutes, it became an orange-brown solution. At this time, 3-bromopropylene (12.582 g) was added and stirred for about 4-5 h to obtain an orange-yellow solution. The solution was washed with water for many times and the solvent was removed under reduced pressure after extraction. After rapid column chromatography, 13.80 g of a slightly yellow transparent oil was obtained, with a yield of about 99%. The main product was about 93% monitored by HPLC. Secondary column chromatography separation was able to obtain 11.80 g of an almost colorless transparent oil (S1) with a purity of about 99.5%, and a total yield of the target product of about 84.7%.

[0089] 1H NMR(400MHz,cdcl3)δ7.17–7.05(m,4H),6.89(d,J=8.1Hz,2H),6.12–5.78(m,4H),5.24(dq ,J=17.3,1.7Hz,2H),5.17–5.02(m,6H),4.49(dt,J=4.8,1.7Hz,4H),3.38(d,J=6.7Hz,4H).

[0090] 13 C NMR (126MHz, CDCl3) δ154.54, 137.91, 133.81, 131.85 (d, J = 3.3Hz), 128.27 (d, J = 4.9Hz), 116.36, 115.50, 112.55, 69.21, 39.47.

[0091] Example 2 Preparation of 3',5-di-2-propen-1-yl-2,4'-bis(2-propen-1-yloxy)-1,1'-biphenyl (honokiol bisallyl ether) (S4)

[0092]

[0093] At room temperature (rt), honokiol (2.651 g) and 40 mL of dimethyl sulfoxide were added to a 100 mL three-necked flask and stirred until dissolved to form a brown solution. Sodium hydride (60%, 900 mg in total) was added in 10-15 batches. After the addition, the solution gradually became a suspension with foam floating on the surface of the liquid. After stirring for about 40 minutes, it became a dark brown solution. At this time, 3-bromopropylene (3.196 g) was added and stirred for about 4-5 h to obtain a brown solution. The solution was washed with water for many times and the solvent was removed under reduced pressure after extraction. After flash column chromatography, 3.18 g of a slightly yellow transparent oil (S4) was obtained with a yield of about 92%. The main product was monitored by HPLC at about 99.0%.

[0094] 1 H NMR (500MHz, CDCl3) δ7.51–7.37(m,1H),7.24–7.05(m,1H),6.93(dd,J=8.4,4.4Hz,1H),6.35–5.85(m,2H),5 .59–5.22(m,2H),5.22–5.00(m,2H),4.59(ddt,J=44.1,4.9,1.7Hz,2H),3.47(ddd,J=49.3,6.8,1.6Hz,2H).

[0095] 13C NMR(126MHz, CDCl3)δ155.38,153.92,137.82,137.07,133.60(d,J=14.1Hz),132.63,131.25,131.15–130.72(m),12 8.27(d,J=2.1Hz),127.86,116.86(d,J=12.4Hz),115.54(d,J=14.1Hz),113.18,111.21,69.37,68.86,39.49,34.59.

[0096] Example 3 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 2,3-Dithio (2-Mercapto)-1-Propanethiol to Prepare Optical Resin Material P1

[0097]

[0098] Take a 20 mL glass sample bottle, add resin monomer S1 (1.040 g), thiol monomer S2 (1.042 g) and 1-hydroxycyclohexyl phenyl ketone (60 mg), mix and stir until uniform, and obtain a colorless clear oily liquid (i.e., prepolymer);

[0099] The mixed liquid was drop-coated on a glass substrate, and another glass substrate was flattened into a circular liquid film (preform). The preform was moved to a UV curing box and irradiated with 315-400 nm wavelength light at 115 mW / cm 2 The energy density is irradiated (hv) for at least 10 minutes, and a colorless transparent film (i.e., the high refractive index material of the present invention) can be obtained. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0100] Example 4 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 4,4'-Thiodibenzenethiol to Prepare Optical Resin Material P2

[0101]

[0102] Take a 20 mL glass sample bottle, add resin monomer S1 (1.040 g), thiol monomer S3 (1.502 g) and 1-hydroxycyclohexyl phenyl ketone (250 mg), and then add 7-10 mL of dichloromethane, mix and stir until uniform, and obtain a colorless clear solution (i.e., prepolymer mixed solution);

[0103] The solution was transferred to a UV curing box and irradiated with 315-400 nm wavelength light at 115 mW / cm 2 The irradiation is performed at an energy density of at least 100 minutes, and the solvent evaporates to obtain a light yellow viscous liquid (i.e., a prepolymer);

[0104] The mixed liquid is dripped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0105] The liquid film was transferred to a UV curing box and irradiated with 315-400 nm wavelength light at 115 mW / cm 2 The light yellow transparent film (i.e., the high refractive index material of the present invention) can be obtained by irradiating with an energy density of at least 120 minutes. In particular, the substrate can be a frosted glass substrate or a flat glass substrate. n is 2-10000; preferably 2-5000.

[0106] Example 5 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 4,4'-Thiodibenzenethiol to Prepare Optical Resin Material P2

[0107]

[0108] Take a 20 mL glass sample bottle, add monomer S1 (1.040 g), S3 (1.502 g), 1-hydroxycyclohexyl phenyl ketone (250 mg), and then add dichloromethane dropwise until all the solids are dissolved, stir until uniform, and obtain a light yellow viscous liquid (i.e., prepolymer mixed solution);

[0109] Heating the prepolymer mixed solution to evaporate all the solvents and obtain a mixed liquid (i.e., prepolymer);

[0110] The mixed liquid is dripped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform).

[0111] The film was moved to a UV curing box and irradiated with 315-400 nm wavelength light at 115 mW / cm 2 The light yellow transparent film can be obtained by irradiating with an energy density of at least 180 minutes. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0112] Example 6 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 2,3-Dithio (2-Mercapto)-1-Propanethiol to Prepare Optical Resin Material P3

[0113]

[0114] Take a 20 mL glass sample bottle, add monomer S4 (1.040 g), S2 (1.042 g), 1-hydroxycyclohexyl phenyl ketone (60 mg), mix and stir until uniform, and obtain an almost colorless clear oily liquid (i.e., prepolymer);

[0115] The mixed liquid is dripped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0116] The liquid film was transferred to a UV curing box and irradiated with 315-400 nm wavelength light at 115 mW / cm 2 The irradiation is carried out at an energy density of at least 10 minutes, and a colorless transparent film can be obtained. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0117] Example 7 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 4,4'-Thiodibenzenethiol to Prepare Optical Resin Material P4

[0118]

[0119] Take a 20 mL glass sample bottle, add monomer S1 (1.040 g), S3 (1.502 g), 1-hydroxycyclohexyl phenyl ketone (250 mg), and then add 7-10 mL of dichloromethane, mix and stir until uniform, and obtain a colorless clear solution (i.e., prepolymer mixed solution);

[0120] The liquid was transferred to a UV curing box and irradiated with 315-400 nm wavelength radiation at an energy density of 115 mW / cm2 for at least 100 minutes, and the solvent was evaporated to obtain a light yellow viscous liquid (i.e., a prepolymer);

[0121] The above liquid is dropped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0122] The film is moved to a UV curing box and irradiated with 315-400 nm wavelength radiation light at an energy density of 115 mW / cm2 for at least 120 minutes to obtain a light yellow transparent film. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0123] Example 8 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 4,4'-Thiodibenzenethiol to Prepare Optical Resin Material P4

[0124]

[0125] Take a 20 mL glass sample bottle, add monomer S1 (1.040 g), S3 (1.502 g), 1-hydroxycyclohexyl phenyl ketone (250 mg), and then add dichloromethane dropwise until all solids are dissolved, stir until uniform, and obtain a light yellow viscous liquid (i.e., prepolymer mixed solution);

[0126] Heating the prepolymer mixed solution to evaporate all the solvents and obtain a mixed liquid (i.e., prepolymer);

[0127] The mixed liquid is dripped onto a glass substrate and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0128] The liquid film was transferred to a UV curing box and irradiated with 315-400 nm wavelength light at 115 mW / cm 2 The light yellow transparent film can be obtained by irradiating with an energy density of at least 180 minutes. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0129] Example 9 Copolymerization of Magnolia Bark Phenol Diallyl Ether and Tetrakis(3-Mercaptopropionic Acid) Pentaerythritol Ester Thiol to Prepare Optical Resin Material P5

[0130]

[0131] Take a 20 mL glass sample bottle, add monomer S1 (1.040 g), S5 (1.538 g), 1-hydroxycyclohexyl phenyl ketone (80 mg), mix and stir until uniform, and obtain a colorless clear oily liquid (i.e., prepolymer);

[0132] The mixed liquid is dripped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0133] The liquid film is moved to a UV curing box and irradiated with 315-400 nm wavelength radiation light at an energy density of 115 mW / cm2 for at least 10 minutes to obtain a colorless transparent film. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0134] Example 10 Copolymerization of Magnolia Bark Phenol Diallyl Ether and Tetrakis(3-Mercaptopropionic Acid) Pentaerythritol Ester Thiol to Prepare Optical Resin Material P6

[0135]

[0136] Take a 20 mL glass sample bottle, add monomer S4 (1.040 g), S5 (1.538 g), 1-hydroxycyclohexyl phenyl ketone (80 mg), mix and stir until uniform, and obtain a colorless clear oily liquid (i.e., prepolymer);

[0137] The mixed liquid is dripped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0138] The liquid film is moved to a UV curing box and irradiated with 315-400 nm wavelength radiation light at an energy density of 115 mW / cm2 for at least 10 minutes to obtain a colorless transparent film. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0139] Example 11 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 2,5-Dimethylmercapto-1,4-Dithianethiol to Prepare Optical Resin Material P7

[0140]

[0141] Take a 20 mL glass sample bottle, add monomer S1 (1.040 g), S6 (1.258 g), 1-hydroxycyclohexyl phenyl ketone (75 mg), mix and stir until uniform, and obtain a colorless clear oily liquid (i.e., prepolymer);

[0142] The mixed liquid is dripped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0143] The film is moved to a UV curing box and irradiated with 315-400 nm wavelength radiation light at an energy density of 115 mW / cm2 for at least 10 minutes to obtain a colorless transparent film. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0144] Example 12 Copolymerization of Magnolia Bark Phenol Diallyl Ether and 2,5-Dimethylmercapto-1,4-Dithianethiol to Prepare Optical Resin Material P8

[0145]

[0146] Take a 20 mL glass sample bottle, add monomer S4 (1.040 g), S6 (1.258 g), 1-hydroxycyclohexyl phenyl ketone (75 mg), mix and stir until uniform, and obtain a colorless clear oily liquid (i.e., prepolymer);

[0147] The above liquid is dropped onto a glass substrate, and another glass substrate is flattened into a circular liquid film (i.e., a preform);

[0148] The liquid film was transferred to a UV curing box and irradiated with 315-400 nm wavelength light at 115 mW / cm 2The irradiation is carried out at an energy density of at least 10 minutes, and a colorless transparent film can be obtained. In particular, the substrate can be a frosted quartz glass substrate or a flat quartz glass substrate. n is 2-10000; preferably 2-5000.

[0149] Example 13 Study on the optical properties of optical resin materials P1-P8 prepared by copolymerization of magnolol / honokiol-based bisallyl ether resin monomers

[0150] 1. Experimental Methods

[0151] 1.1 Refractive index test

[0152] The sample film was tested by an ellipsometer (model: ELLIP-SR-I) with a test band of 300nm-1000nm and a step length of 10nm.

[0153] 1.2 Abbe number test

[0154] Calculation formula: (nd-1) / (nF-nC)

[0155] Among them, nd, nF and nC are the refractive indices of the material under d-light, F-light and C-light respectively, and d-light, F-light and C-light refer to light in the wavelength bands of 486.3nm, 589.1nm and 656.1nm respectively.

[0156] 2. Experimental results

[0157] The glass substrate-supported copolymer thin film resin materials (i.e., the optical resin materials described in the present application) P1-P8 were obtained by using frosted glass substrate or flat glass substrate as auxiliary molding, and their refractive index and Abbe number were tested. The experimental results are shown in Tables 1 and 2. Figure 1 shown.

[0158] Table 1. Refractive index and Abbe number of optical resin materials P1-P8

[0159]

[0160] 3. Experimental conclusion

[0161] Experimental results show that the optical resin material prepared from the compound of the present application has a higher refractive index (1.67-1.71) and a higher Abbe number (35-24), and has excellent optical properties.

[0162] Example 14 DMA test of optical resin materials P1-P8 prepared by copolymerization of magnolol / honokiol-based bisallyl ether resin monomers

[0163] 1. Experimental Methods

[0164] Dynamic mechanical analysis (DMA) was tested by DMA / Q800 instrument in a nitrogen atmosphere with a heating rate of 5°C / min. The storage modulus and glass transition temperature of the optical resin material obtained are shown in Table 2. Figure 2 and Figure 3 shown.

[0165] 2. Experimental results

[0166] Table 2. Storage modulus and glass transition temperature of optical resin materials P1-P8

[0167]

[0168]

[0169] 3. Experimental conclusion

[0170] Experimental results show that the optical resin material prepared from the compound of the present application has a higher storage modulus and a higher glass transition temperature, and has excellent thermomechanical properties.

[0171] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A curing material, It is characterized in that The solidified material is prepared by copolymerizing component (a) and component (b): (a) a resin monomer; the resin monomer is selected from the group consisting of a compound having a structure represented by formula (I), a compound having a structure represented by formula (II), or a combination thereof; in, R 1 , R 2 , R 3 and R 4 are independently selected from the group consisting of hydrogen, C 1-6 Alkyl, C 2-6 Alkenyl, C 1-15 Alkylsilyl; One or more hydrogen atoms on the above groups are optionally substituted by a substituent selected from the group consisting of halogen, C 1-4 Alkyl, C 2-4 Alkenyl, C 2-4 Alkynyl, phenyl, or 1, 2 or 3 R a Substituted phenyl; R a Selected from the group consisting of halogen, C 1-6 Alkyl, C 2-6 alkenyl; (b) a thiol monomer; the thiol monomer is selected from the group consisting of methanethiol, 1,2-ethanethiol, 1,1-propanethiol, 1,2-propanethiol, 1,3-propanethiol, 2,2-propanethiol, 1,6-hexanethiol, 1,2,3-propanetriol, 1,1-cyclohexanethiol, 1,2-cyclohexanethiol, 2,2-dimethylpropane-1,3-thiol, 3,4-dimethoxybutane-1,2-thiol, 2-methylcyclohexane-2,3-thiol, bicyclo[2,2,1]heptyl-exo-cis-2,3-thiol, 1,1-bis(mercaptomethyl)cyclohexane, bis(2-mercaptoethyl)thiomalate, 2,3-dimercaptosuccinic acid (2-mercaptoethyl ester), 2,3-dimercapto-1-propanethiol, 1,3-Bis(2-mercaptoethyl)ether, ethylene glycol bis(2-mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), trimethylolpropane tris(2-mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), 1,2-bis(2-mercaptoethylthio)-3-mercaptopropane), 5,7-dimercaptomethyl-1,11- Dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 1,1,3,3-tetrakis(mercaptomethylthio)propane, 4,6-bis(mercaptomethylthio)-1,3-dithiane, 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithiacyclobutane, 1,2-dimercaptobenzene, 1,3-dimercaptobenzene, 1,4-dimercaptobenzene, 1,2-bis(mercaptomethyl)benzene, 1,3-bis(mercaptomethyl)benzene, 1,4-bis(mercaptomethyl)benzene, 1,2-bis(mercaptoethyl)benzene, 1,3-bis(mercaptoethyl)benzene, 1,4- Bis(mercaptoethyl)benzene, 1,2-bis(mercaptomethyleneoxy)benzene, 1,3-bis(mercaptomethyleneoxy)benzene, 1,4-bis(mercaptomethyleneoxy)benzene, 1,2-bis(mercaptoethyleneoxy)benzene, 1,3-bis(mercaptoethyleneoxy)benzene, 1,4-bis(mercaptoethyleneoxy)benzene, 1,2,3-trimercaptobenzene, 1,2,4-trimercaptobenzene, 1,3,5-trimercaptobenzene, 1,2,3-tris(mercaptomethyl)benzene, 1,2,4-tris(mercaptomethyl)benzene, 1,3,5-tris(mercaptomethyl)benzene, 1,2,3-tris(mercaptoethyl)benzene, 1,2,4-tris(mercaptoethyl)benzene, 1,3,5-tris(mercaptoethyl)benzene, 1,2,3-tris(mercaptomethyleneoxy)benzene, 1,2,4-Tris(mercaptomethyleneoxy)benzene, 1,3,5-tris(mercaptomethyleneoxy)benzene, 1,2,3-tris(mercaptoethyleneoxy)benzene, 1,2,4-tris(mercaptoethyleneoxy)benzene, 1,3,5-tris(mercaptoethyleneoxy)benzene, 1,2,3,4-tetramercaptobenzene, 1,2,3,5-tetramercaptobenzene, 1,2,4,5-tetramercaptobenzene, 1,2,3,4-tetrakis(mercaptomethyl)benzene, 1,2,3,5-tetrakis(mercaptomethyl)benzene, 1,2,4,5-tetrakis(mercaptomethyl)benzene, 1,2,3,4-tetrakis(mercaptoethyl)benzene, 1,2,3,5-tetrakis(mercaptoethyl)benzene, 1,2,4,5-tetrakis(mercaptoethyl)benzene, 1,2,3,4-tetrakis(mercaptoethyl)benzene, 1,2, 3,5-Tetrakis(mercaptomethyleneoxy)benzene, 1,2,4,5-Tetrakis(mercaptomethyleneoxy)benzene, 1,2,3,4-Tetrakis(mercaptoethyleneoxy)benzene, 1,2,3,5-Tetrakis(mercaptoethyleneoxy)benzene, 1,2,4,5-Tetrakis(mercaptoethyleneoxy)benzene, 2,2'-dimercaptobiphenyl, 4,4'-dimercaptobiphenyl, 4,4'-dimercaptobibenzyl, 2,5-toluenedithiols, 3,4-toluenedithiols, 1,4-naphthalenedithiols, 1,5-naphthalenedithiols, 2,6-naphthalenedithiols, 2,7-naphthalenedithiols, 2,4-dimethylbenzene-1,3-dithiol, 4,5-dimethylbenzene-1,3-dithiol, 9,10-anthracenedimethanethiol, 1,3-bis(p-methoxyphenyl)propane-2, 2-dithiol, 1,3-diphenylpropane-2,2-dithiol, phenylmethane-1,1-dithiol, 2,4-di(p-mercaptophenyl)pentane, 2-methylamino-4,6-dimercapto-s-triazine, 2-ethylamino-4,6-dimercapto-s-triazine, 2-amino-4,6-dimercapto-s-triazine, 2-morpholino-4,6-dimercapto-s-triazine, 2-cyclohexylamino-4,6-dimercapto-s-triazine, 2-methoxy-4,6-dimercapto-s-triazine, 2-phenoxy-4,6-dimercapto-s-triazine, 2-thiophenoxy-4,6-dimercapto-s-triazine, 2-thiobutyloxy-4,6-dimercapto-s-triazine, 1,2-bis(mercaptomethylthio)benzene, 1,3-bis(mercaptomethylthio)benzene 1,4-bis(mercaptomethylthio)benzene, 1,2-bis(mercaptoethylthio)benzene, 1,3-bis(mercaptoethylthio)benzene, 1,4-bis(mercaptoethylthio)benzene, 1,2,3-tris(mercaptomethylthio)benzene, 1,2,4-tris(mercaptomethylthio)benzene, 1,3,5-tris(mercaptomethylthio)benzene, 1,2,3-tris(mercaptoethylthio)benzene, 1,2,4-tris(mercaptoethylthio)benzene, 1,3,5-tris(mercaptoethylthio)benzene, 1,2,3,4-tetrakis(mercaptomethylthio)benzene, 1,2,3,5-tetrakis(mercaptomethylthio)benzene, 1,2,4,5-tetrakis(mercaptomethylthio)benzene, 1,2,3,4-tetrakis(mercaptoethylthio)benzene, 1,2,3,5-Tetrakis(mercaptoethylthio)benzene, 1,2,4,5-Tetrakis(mercaptoethylthio)benzene, bis(mercaptomethyl)sulfide, bis(mercaptoethyl)sulfide, bis(mercaptopropyl)sulfide, bis(mercaptomethylthio)methane, bis(2-mercaptoethylthio)methane, bis(3-mercaptopropyl)methane, 1,2-bis(mercaptomethylthio)ethane, 1,2-(2-mercaptoethylthio)ethane, 1,2-(3-mercaptopropyl)ethane, 1,3-bis(mercaptomethylthio)propane, 1,3-bis(2-mercaptoethylthio)propane, 1,3-bis(3-mercaptopropylthio)propane, 1,2,3-tris(mercaptomethylthio)propane, 1,2,3-tris(2-mercaptoethylthio)propane, 1,2,3-tris( 3-Mercaptopropylthio)propane, tetrakis(mercaptomethylthiomethyl)methane, tetrakis(2-mercaptoethylthiomethyl)methane, tetrakis(3-mercaptopropylthiomethyl)methane, bis(2,3-dimercaptopropyl)sulfide, 2,5-dimercapto-1,4-dithiane, bis(mercaptomethyl)disulfide, bis(mercaptoethyl)disulfide, bis(mercaptopropyl)disulfide, 1,5-dimercapto-3-thiapentane, hydroxymethyl sulfide bis(2-mercaptoacetate), hydroxymethyl sulfide bis(3-mercaptopropionate), hydroxyethyl sulfide bis(2-mercaptoacetate), hydroxyethyl sulfide bis(3-mercaptopropionate), hydroxypropyl sulfide bis(2-mercaptoacetate), hydroxypropyl sulfide bis(3-mercaptopropionate), hydroxymethyl disulfide Bis(2-mercaptoacetate), hydroxymethyl disulfide bis(3-mercaptopropionate), hydroxyethyl disulfide bis(2-mercaptoacetate), hydroxyethyl disulfide bis(3-mercaptopropionate), hydroxypropyl disulfide bis(2-mercaptoacetate), hydroxypropyl disulfide bis(3-mercaptopropionate), 2-mercaptoethyl ether bis(2-mercaptoacetate), 2-mercaptoethyl ether bis(3-mercaptopropionate), 1,4-dithiane-2,5-diol bis(2-mercaptoacetate), 1,4-dithiane-2,5-diol bis(3-mercaptopropionate), thioglycolic acid bis(2-mercaptoethyl ester), 4,4-thiodibutyric acid bis(2-mercaptoethyl ester), dithiodisulfide Bis(2-mercaptoethyl) acetate, bis(2-mercaptoethyl) dithiodipropionate, bis(2-mercaptoethyl) 4,4-dithiodibutyrate, bis(2-mercaptoethyl) dithiodiacetate, bis(2,3-dimercaptopropyl) dithiodipropionate, bis(2,3-dimercaptopropyl) dithiodiacetate, 2,3-dimercaptopropyl dithiodipropionate, 2,2'-thiodiethanethiol, biphenyl-4,4'-dithiol, biphenyl-4,4'-dithiol, 4,4'-thiodiphenylthiol, bis(2-mercaptoethyl) ether, 3,3'-dimercaptopropyl ether, 2,5-dimethylmercapto-1,4-dithiane, 2,3-dithio(2-mercapto)-1-propanethiol, 2,3-dithio(2-mercapto)-1-propanethiol, butanediol bis(thioglycolate), butanediol bis(thiopropionate), diethylene glycol bis(thioglycolate), diethylene glycol bis(thiopropionate), 2-[(2-mercaptoethyl)thio]-1,3-propanedithiol, 2,2'-[[2-[[2-[(2-mercaptoethyl)thio]ethyl]thio]-1,3-propanediyl]bis(thio)]bis[ethanethiol], 7-[[(2-mercaptoethyl)thio]methyl]-3,6,9,12-tetrathiotetradecane-1,14-dithiol, 1,3,4,6-tetrakis(2-mercaptoethyl)tetrahydroimidazo[4,5-d]imidazole-2,5(1H,3H)-dione, dicyclic thiomethyl sulfide, or a combination thereof.

2. The solidified material according to claim 1, It is characterized in that The thiol monomer is selected from the following group: 4,4'-thiodibenzenethiol, 2,5-dimethylmercapto-1,4-dithiane, 2,5-dimercapto-1,4-dithiane, dicyclic thiomethyl sulfide, 2,3-dithio(2-mercapto)-1-propanethiol, pentaerythritol tetrakis(2-thioglycolate), or a combination thereof.

3. The solidified material according to claim 1, It is characterized in that The molar ratio of the resin monomer to the thiol monomer is 1:(1-4).

4. The solidified material according to claim 1, It is characterized in that The curing material is prepared by copolymerizing component (a) and component (b) in the presence of a photoinitiator; Wherein, the photoinitiator is selected from the following group: 2,4,6 (trimethylbenzoyl) diphenylphosphine oxide, 2,4,6-trimethylbenzoylphosphonic acid ethyl ester, 2-methyl-1-[4-methylthiophenyl]-2-morpholinyl-1-propanone, 2-isopropylthioxanthone, 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzoin dimethyl ether, methyl o-benzoylbenzoate, benzophenone, 4-phenylbenzophenone, 2-phenylbenzyl-2-dimethylamine-1-(4-morpholinobenzylphenyl)butanone, photoinitiator 754 (benzoylformate mixture), phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2-hydroxy-1-(4-(2-hydroxy-2-methylpropionylphenyl)benzyl)-2-methyl-1-propanone, bis-2,6-difluoro-3-pyrrolylphenyl titanocene, ethyl 4-dimethylaminobenzoate; Preferably, the photoinitiator is selected from the following group: benzoin dimethyl ether, 1-hydroxy-cyclohexyl-phenyl ketone, or a combination thereof.

5. The method for preparing the solidified material according to claim 1, It is characterized in that The method comprises the following steps: in the presence of a photoinitiator, the component (a) and the component (b) undergo copolymerization reaction to prepare the curing material.

6. The preparation method according to claim 5, It is characterized in that The reaction is carried out under solvent-free conditions and comprises the following steps: A1. Mixing a resin monomer, a thiol monomer and a photoinitiator to obtain a prepolymer; B2. The prepolymer is molded to obtain a preform; C1. Place the preform under the irradiation of light source B to perform a photocuring reaction to obtain a high-refractive material.

7. The preparation method according to claim 5, It is characterized in that The light source B is ultraviolet light with a wavelength of 310-400nm.

8. The preparation method according to claim 5, It is characterized in that The photocuring reaction is carried out in the presence of solvent A, comprising the following steps: A2. mixing a resin monomer, a thiol monomer, a solvent A and a photoinitiator to obtain a prepolymer mixed solution; removing the solvent A from the prepolymer mixed solution to obtain a prepolymer; B2. The prepolymer is molded to obtain a preform; C2. placing the preform under the irradiation of light source B to perform a photocuring reaction to obtain a high-refractive material; Wherein, the boiling point range of the solvent A is 30-150°C.

9. The preparation method according to claim 8, It is characterized in that The solvent A is selected from the group consisting of dichloromethane, tetrahydrofuran, ethanol, ethyl acetate, n-hexane, diethyl ether, or a combination thereof.

10. The preparation method as claimed in claims 6 to 9, It is characterized in that The molding is selected from the group consisting of: inverted molding, drop coating, solution drop coating, solution spin coating, or a combination thereof.

Citation Information

Patent Citations

  • Magnolol derivative as well as preparation method and application thereof

    CN110668985A

  • Synthesis method of magnolol derivative and intermediate thereof

    CN113845410A

  • Polythiol compound and preparation method thereof, curing agent, resin composition, adhesive and sealant

    CN113912523A

Cited By

  • Polythiol compound, preparation method thereof and application of polythiol compound in optical material

    CN119775179A

  • High-refractive-index material based on biomass magnolol and magnolol

    WO2025252160A1