Organosilicon / bismaleimide synergistically modified epoxy resin and preparation method and application thereof
The epoxy resin synergistically modified by silicone and bismaleimide solves the problem of insufficient thermal stability and mechanical properties of epoxy resin in high-temperature environments, improves the glass transition temperature and mechanical properties, and expands its Application scope in aerospace field.
Patent Information
- Application Number
- CN202410894560.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing epoxy resins have insufficient thermal stability and mechanical properties in high-temperature environments, which limits their application in the aerospace field. In particular, carbon fiber composites have poor ablation resistance and heat protection properties, and are modified to increase silicon Elements can impair material properties.
An epoxy resin synergistically modified with silicone and bismaleimide is used to react diallyl bisphenol A and diphenylmethane bismaleimide to generate a bismaleimide prepolymer, and Combined with the terminal methoxymethylphenyl silicone intermediate to form a modified epoxy resin matrix, the material properties are improved through the curing process.
Significantly improves the glass transition temperature and mechanical properties of the epoxy resin composite system, enhances high-temperature mechanical properties, and extends the application of epoxy resin in thermal protection materials and structural materials, especially in the aerospace field. It has good application prospects .
Smart Images

Figure CN118745248A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of advanced materials, and in particular relates to an epoxy resin synergistically modified with silicone / bismaleimide, and a preparation method and application thereof. Background Art
[0002] With the rapid development of industries such as aerospace, higher requirements are placed on the mechanical properties, heat resistance, and ablation resistance of organic heat-resistant coatings and composite matrixes. Commonly used organic heat-resistant coating materials are mainly epoxy resin (EP) and phenolic resin. Among them, epoxy resin is widely used in the resin matrix of various coatings due to its excellent mechanical properties and bonding properties. Due to the poor thermal stability of epoxy resin itself, its application in high-temperature ablation environments is limited. At the same time, epoxy resin-based carbon fiber composites are the main structural materials of aerospace vehicles. Due to the low thermal residual weight of epoxy resin, it is almost not resistant to ablation, so that its carbon fiber composites do not have ablation resistance and heat resistance. At this stage, the main method is to add thermal protection coatings to epoxy carbon fiber composites to prevent the damage of high temperature environments to structural materials. However, the step-by-step implementation of structural and thermal protection functions leads to complex processes, increased quality, and increased costs of structural parts. At the same time, in order to further improve structural efficiency, thermal protection technology is developing towards the integration of heat protection / load bearing and multi-functional integration. Therefore, while maintaining the excellent structural and thermomechanical properties of epoxy resin, improving the ablation resistance of epoxy resin can further expand the application of epoxy resin in the aerospace field and realize the integration of thermal protection / structure based on epoxy resin-based carbon fiber composites.
[0003] Polysiloxane is an organic-inorganic hybrid polymer with Si-O-Si as the main chain and organic groups connected to silicon atoms. It has excellent weather resistance, high and low temperature stability and chemical resistance. Its ability to be ceramicized in high temperature environment is an effective way to improve the ablation resistance of resin-based thermal protection materials. At present, a large number of studies have been conducted to improve the thermal stability and residual weight of epoxy resins by doping with a large amount of silicon elements. However, excessive silicon content may damage the mechanical and thermal properties of the material (High Perform. Polym. 29 (1) (2016) 36-45). Studies have shown that when the silicone content exceeds 40%, the glass transition temperature of the modified epoxy resin is reduced by more than 20°C (React. Funct. Polym. 157 (2020) 104742-104752.). The reduction in glass transition temperature will have an adverse effect on the mechanical properties of epoxy resins and their composites in high temperature environments, and will also lead to a reduction in their use temperature. Therefore, how to maintain or even improve the thermal and mechanical properties of the epoxy resin itself based on silicone-modified epoxy resin is of great significance for the preparation of high-performance thermal protective coatings and thermal protection-structural integrated composite materials. Summary of the invention
[0004] The purpose of the present invention is to provide an epoxy resin synergistically modified with silicone / bismaleimide and a preparation method and use thereof.
[0005] The present invention provides an organosilicon / bismaleimide synergistically modified epoxy resin, which is prepared from raw materials in the following weight ratio:
[0006] 100 parts of epoxy resin, 1-50 parts of bismaleimide prepolymer, 30-70 parts of terminal methoxymethyl phenyl silicone intermediate, and 0.01-1 part of catalyst;
[0007] The structure of the bismaleimide prepolymer is:
[0008]
[0009] Furthermore, the aforementioned organosilicon / bismaleimide synergistically modified epoxy resin is prepared from raw materials in the following weight ratio:
[0010] 100 parts of epoxy resin, 20 parts of bismaleimide prepolymer, 30-70 parts of terminal methoxymethyl phenyl silicone intermediate, and 0.15-0.35 parts of catalyst;
[0011] Preferably, it is prepared from the following raw materials in weight ratio:
[0012] 100 parts of epoxy resin, 20 parts of bismaleimide prepolymer, 50 parts of terminal methoxymethyl phenyl silicone intermediate, and 0.25 parts of catalyst.
[0013] Further,
[0014] The epoxy resin is selected from bisphenol A epoxy resin, 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ester, and tetraglycidylamine epoxy resin;
[0015] And / or, the structure of the terminal methoxymethyl phenyl organosilicon intermediate is n is an integer from 12 to 15;
[0016] And / or, the catalyst is selected from butyltin dilaurate, tetraisopropyl titanate, and chloroplatinic acid.
[0017] Furthermore, the bismaleimide prepolymer is prepared from diallyl bisphenol A and diphenylmethane bismaleimide as raw materials; the mass ratio of diallyl bisphenol A to diphenylmethane bismaleimide is (1-10): (1-10);
[0018] Preferably, the mass ratio of diallyl bisphenol A to diphenylmethane bismaleimide is 1:1.
[0019] Furthermore, the preparation method of the bismaleimide prepolymer comprises the following steps:
[0020] Diallyl bisphenol A and diphenylmethane bismaleimide are mixed and reacted to obtain;
[0021] Preferably, the reaction temperature is 100-160° C. and the reaction time is 1-5 h.
[0022] The present invention also provides a method for preparing the aforementioned organosilicon / bismaleimide synergistically modified epoxy resin, which comprises the following steps:
[0023] (1) Weighing each raw material according to the weight ratio;
[0024] (2) mixing the epoxy resin and the bismaleimide prepolymer and reacting them to obtain a bismaleimide-modified epoxy resin;
[0025] (3) mixing the bismaleimide-modified epoxy resin prepared in step (2) with the terminal methoxymethylphenyl silicone intermediate, and then adding a catalyst to react to obtain a silicone / bismaleimide-modified epoxy resin matrix;
[0026] (4) curing the organosilicon / bismaleimide modified epoxy resin matrix prepared in step (3) to obtain.
[0027] Further,
[0028] In step (2), the reaction temperature is 100-150° C., and the reaction time is 1-5 h;
[0029] And / or, in step (3), the reaction temperature is 100 to 160° C., and the reaction time is 1 to 10 h;
[0030] And / or, in step (3), the reaction is carried out under an inert environment;
[0031] And / or, in step (4), when the organosilicon / bismaleimide-modified epoxy resin matrix prepared in step (3) is cured, it is first mixed with a catalyst and preheated, stirred evenly to obtain a resin glue solution, and then cured;
[0032] Preferably,
[0033] In step (4), the catalyst is an amine curing agent;
[0034] And / or, in step (4), the preheating temperature is 100 to 160° C.;
[0035] And / or, in step (4), the curing conditions are sequentially maintained at 140-160° C. for 1-5 h, 160-200° C. for 1-5 h and 180-220° C. for 1-5 h;
[0036] More preferably,
[0037] In step (4), the amine curing agent is selected from 4,4'-diamino-3,3'-dichloroxylene methane, 4,4'-diaminoxylene methane, polyetheramine D400, and polyetheramine D230.
[0038] The present invention also provides the use of the aforementioned organosilicon / bismaleimide synergistically modified epoxy resin in the preparation of heat-resistant thermal protective coatings, high-performance carbon fiber composite materials, and ablation-resistant composite materials.
[0039] The present invention also provides a composite material, which is prepared by using the aforementioned organosilicon / bismaleimide synergistically modified epoxy resin as a resin matrix and composited with aramid, PBO, quartz, glass fiber or carbon fiber.
[0040] The present invention also provides the use of the aforementioned composite material in preparing parts and / or equipment used in the fields of aviation and aerospace.
[0041] The present invention uses a bismaleimide prepolymer obtained by reacting diallyl bisphenol A (DABPA) and diphenylmethane bismaleimide (BDM) in an equal mass ratio as a modifier for an organosilicon-modified epoxy resin, thereby effectively solving the problem that the organosilicon-modified epoxy resin will cause the epoxy resin system to have a lower glass transition temperature, lower heat resistance, and worse mechanical properties.
[0042] Compared with the prior art, the present invention has the following beneficial effects:
[0043] The present invention prepares an epoxy resin synergistically modified by silicone / bismaleimide. The modified epoxy resin of the present invention solves the problem that silicone-modified epoxy resin leads to a decrease in the glass transition temperature of the epoxy resin system, a decrease in heat resistance, and a deterioration in mechanical properties, thereby improving the glass transition temperature and mechanical properties of the epoxy resin composite system. The use of the modified epoxy resin of the present invention to prepare a composite material can also significantly improve the high-temperature mechanical properties of the composite material. The present invention expands the application of epoxy resin systems in thermal protection materials and structural materials, and has good application prospects in the fields of aviation and aerospace.
[0044] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.
[0045] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0046] Figure 1 This is a flow chart for the preparation of unidirectional carbon fiber composite materials.
[0047] Figure 2 These are the infrared spectra before and after resin curing: a is the infrared spectrum of EP-BD, PMPS and EP-20BD@50P; b is the infrared spectrum of EP@30P-Curing, EP-20BD@30P-Curing, EP@50P-Curing and EP-20BD@50P-Curing; c is the infrared spectrum of EP-20BD@50P-Curing, EP-20BD@50P and PMPS.
[0048] Figure 3 The TGA curve and DTG curve of the modified epoxy resin of the present invention under nitrogen atmosphere: a is the TGA curve; b is the DTG curve.
[0049] Figure 4 It is the DSC curve of the modified epoxy resin of the present invention.
[0050] Figure 5 The linear ablation rate and mass ablation rate results of the modified epoxy resin of the present invention are shown in FIG. DETAILED DESCRIPTION
[0051] The raw materials and equipment used in the specific embodiments of the present invention are all known products and are obtained by purchasing commercially available products.
[0052] Some experimental raw materials are shown in Table 1:
[0053] Table 1. Experimental materials
[0054]
[0055]
[0056] Example 1. Preparation of silicone / bismaleimide synergistically modified epoxy resin of the present invention
[0057] The synthetic route is as follows:
[0058]
[0059] The amounts of raw materials used in the preparation of the epoxy resin modified by organosilicon / bismaleimide synergistically are shown in Table 2. Among them, EP-20BD@30P, EP-20BD@50P, and EP-20BD@70P are epoxy resins modified by organosilicon / bismaleimide synergistically; EP@30P, EP@50P, and EP@70P are epoxy resins modified by organosilicon.
[0060] Table 2. Raw material dosage for preparing epoxy resin modified by organosilicon / bismaleimide synergistically according to the present invention
[0061]
[0062]
[0063] Preparation method:
[0064] The modified epoxy resin was prepared by weighing various raw materials according to the amounts shown in Table 2.
[0065] (1) Synthesis of bismaleimide prepolymer (BD)
[0066] Equal weights of BDM and DABPA were added into a beaker, and stirred in an oil bath at 140° C. for reaction for 1 h to obtain the treated bismaleimide prepolymer (BD), which was then taken out for later use.
[0067] (2) Bismaleimide-modified epoxy resin
[0068] In a three-necked beaker containing 100 g of DGEBA (EP in the synthetic route), 20 g of the bismaleimide prepolymer (BD) prepared in step (1) was added, and the mixture was reacted at 110° C. for 2 h to obtain a bismaleimide-modified epoxy resin (EP-BD).
[0069] (3) Silicone / bismaleimide modified epoxy resin
[0070] In a three-necked flask with magnetic stirring, add the bismaleimide-modified epoxy resin (EP-BD) synthesized in step (2) and 50g of terminal methoxymethylphenyl silicone intermediate (PMPS), stir evenly at 140°C, add 0.5wt% of the mass of PMPS DBTDL catalyst, react at 140°C under an inert environment for 5h to obtain silicone / bismaleimide-modified epoxy resin matrix EP-BD@PMPS (EP-20BD@50P).
[0071] The amounts of PMPS and DBTDL were replaced according to the amounts of raw materials in Table 2 to prepare EP-20BD@30P and EP-20BD@70P.
[0072] DGEBA and PMPS were added to a three-necked flask with magnetic stirring according to the dosage in Table 2. After stirring evenly at 140°C, DBTDL catalyst was added and reacted at 140°C for 5 h under an inert environment to obtain silicone-modified epoxy resin matrices EP@30P, EP@50P and EP@70P.
[0073] (4) Curing of resin
[0074] According to the amounts in Table 2, the resin matrix synthesized in step (3) and MOCA were preheated at 140°C and then mixed and stirred to obtain a resin glue solution. After removing bubbles in a vacuum oven at 140°C, the solution was poured into a polytetrafluoroethylene mold and cured in a blast oven at 150°C for 2h, 180°C for 2h and 200°C for 2h.
[0075] Example 2: Preparation of composite material using epoxy resin modified by organosilicon / bismaleimide of the present invention
[0076] According to the amounts in Table 2, the organosilicon / bismaleimide-modified epoxy resin matrix (EP-20BD@30P, EP-20BD@50P or EP-20BD@70P) prepared in step (3) of Example 1 and the curing agent MOCA were preheated at 140°C and mixed and stirred to obtain a resin glue solution, and an ultrasonic-guided fiber expansion-winding molding integrated method was used to prepare a unidirectional carbon fiber composite material (the preparation flow chart of the unidirectional carbon fiber composite material is shown in FIG. Figure 1 The specific preparation method is as follows:
[0077] like Figure 1As shown, the carbon fiber / epoxy resin composite material is prepared by dry winding and autoclave molding. The resin matrix synthesized in step (3) and MOCA are mixed and stirred at 140°C for 10 minutes according to the ratio in Table 2 to obtain a resin glue solution. The unidirectional carbon fiber with a widening range of 20 mm is impregnated with the resin glue solution using a yarn spreading machine and wound onto a drum with a diameter of 300 mm, with 50 layers of winding. Subsequently, the unidirectional prepreg is cut radially to obtain a unidirectional prepreg tape, and is flatly laid on the surface of the iron plate mold sputtered with PTFE. The demoulding cloth and the adhesive felt are laid in turn, the iron plate is placed in a bag, and the sealing of the vacuum bag and its surroundings is checked. Finally, the widened carbon fiber / epoxy prepreg with good sealing performance is placed in an autoclave for molding and curing. The curing process is to maintain it at 150°C for 2h, 180°C for 2h and 200°C for 2h, the vacuum bag pressure is 0.09MPa, and the tank pressure is 0.25MPa. The composite materials prepared using the EP@30P, EP@50P, EP@70P, EP-20BD@30P, EP-20BD@50P and EP-20BD@70P resin matrices in Example 1 were named EP@30P / CF, EP@50P / CF, EP@70P / CF, EP-20BD@30P / CF, EP-20BD@50P / CF and EP-20BD@70P / CF, respectively.
[0078] The preparation method of EP / CF is the same as before. EP and MOCA are mixed and stirred at 140°C for 10 minutes according to the ratio in Table 2 to obtain epoxy resin glue. The unidirectional carbon fiber with a widening range of 20 mm is impregnated with resin glue by a yarn spreading machine and wound on a drum with a diameter of 300 mm. The number of winding layers is 50. Subsequently, the unidirectional prepreg is cut radially and laid flat on the surface of the iron plate mold sputtered with PTFE. The demoulding cloth and the adhesive felt are laid in turn, the iron plate is placed in the bag and the sealing of the vacuum bag and its surroundings is checked. Finally, the widened carbon fiber / epoxy prepreg with good sealing performance is placed in an autoclave for molding and curing. The curing process is to keep it at 150°C for 2h, 180°C for 2h and 200°C for 2h, the vacuum bag pressure is 0.09MPa, and the tank pressure is 0.25MPa.
[0079] The beneficial effects of the present invention are demonstrated below through specific test examples.
[0080] Test Example 1: Molecular structure of the modified epoxy resin of the present invention
[0081] Infrared spectrum test: FTIR spectrometer produced by Thermo Nicolet Corporation was used to analyze and test each sample. The scanning range was 4000cm -1 -400cm -1 .
[0082] Figure 2 is the infrared spectrum of each sample, Figure 2 Here, EP-BD is the bismaleimide-modified epoxy resin prepared in Example 1, PMPS is the raw material terminal methoxymethylphenyl silicone intermediate, EP-20BD@50P is the uncured silicone / bismaleimide-modified epoxy resin matrix prepared in Example 1, EP-20BD@50P-Curing, EP-20BD@30P-Curing, EP@30P-Curing and EP@50P-Curing are the cured resins prepared in Example 1.
[0083] In the infrared spectrum, at 2840 cm -1 、1600cm -1 、1710cm -1 、1635cm -1 、910cm -1 The infrared peaks at are attributed to Si-OCH3, benzene ring, C=O in imide, C=C in allyl group, and epoxy group. Figure 2 a As can be seen, EP-20BD@50P is at 2840cm -1 The infrared peak of the methoxyl group at the position almost disappeared, the epoxy group was retained, and C=O and C=C bonds were also observed, proving that the epoxy resin containing bismaleimide and silicone was successfully synthesized. Figure 2 As shown in b, after curing, the C=C double bonds in the epoxy group and the allyl group completely disappeared, indicating that while the curing reaction was complete, a cross-linking network was formed between the double bonds and the epoxy resin. Figure 2 From the infrared spectra of the cured resins in b and 2c, it can be seen that compared with EP@30P and EP@50P, the infrared absorption peaks of the silyl methoxy groups of EP-20BD@30P and EP-20BD@50P indicate that more silicones are involved in the grafting reaction. Figure 2 In c, compared with before and after curing, the silyl methoxy group disappears further, indicating that more silicone undergoes grafting reaction during the curing process.
[0084] Depend on Figure 2 It can be seen that bismaleimide is successfully introduced into the silicone-modified epoxy resin, and the grafting degree of silicone in the epoxy resin is also improved.
[0085] Test Example 2: Thermal stability of the modified epoxy resin of the present invention
[0086] Thermogravimetric analysis (TGA) was performed on the cured modified epoxy resin using a thermogravimetric analyzer produced by NETZSCH Instrument Manufacturing Co., Ltd., Germany, under the conditions of a temperature increase of 10°C / min, an N2 atmosphere, and a temperature range of 30 to 800°C.
[0087] The TGA curve and DTG curve of the modified epoxy resin under nitrogen atmosphere are as follows: Figure 3 The thermal stability results are shown in Table 3. As the content of organic silicon increases, the residual weight (Residual char) and the initial pyrolysis temperature (T5%) gradually increase, and the pyrolysis rate gradually decreases (DW). At the same silicon content, the pyrolysis rate of the curing system with the addition of 20phr bismaleimide prepolymer is further reduced.
[0088] The heat resistance index (Ts) of the epoxy resin synergistically modified with silicone / bismaleimide is significantly improved compared with EP, indicating that in the epoxy resin system containing bismaleimide prepolymer, as the silicone content increases, it has an adverse effect on the thermal stability in the low temperature stage (<400°C), but can significantly improve the thermal stability at high temperature, especially T30% is significantly increased, and the thermal decomposition rate is significantly reduced.
[0089] This is mainly because after the ring-opening reaction, the cross-linking density of EP is appropriately destroyed, but more silicone segments participate in the cross-linking network to improve the thermal stability in the high-temperature stage. The silicon oxide compound barrier constructed by the thermal decomposition of the silicon oxide segments in the cross-linking network further hinders the thermal decomposition of EP and BDM, thereby further reducing the thermal decomposition rate, but the impact on the final residual weight is relatively small.
[0090] Table 3. Thermal stability results of modified epoxy resin
[0091]
[0092]
[0093] The above results indicate that the modified epoxy resin of the present invention has excellent thermal stability and high carbon residue.
[0094] Test Example 3: Glass transition temperature of the modified epoxy resin of the present invention
[0095] The cured modified epoxy resin was tested using a differential scanning calorimeter produced by NETZSCH Instrument Manufacturing Co., Ltd., Germany, with a temperature increase of 10°C / min and a temperature range of 30 to 200°C.
[0096] The DSC curve of modified epoxy resin is as follows: Figure 4 As shown. The inflection point of the DSC curve is the transition region of the resin, which is defined as the glass transition temperature. Figure 4It can be seen that in the silicone-modified epoxy resin system, as the silicone content increases, the glass transition temperature of the epoxy resin system first decreases significantly and then increases, but when the silicone content increases to 70phr, the glass transition temperature of the epoxy resin system is only close to that of EP. This is because when a low amount of silicone is added to EP, it is evenly dispersed in the cross-linked network of EP, resulting in an increase in the flexibility of the cross-linked structure, which causes the glass transition temperature to decrease; as the silicone content increases, excessive silicone will aggregate, reducing the silicone molecular chains entering the cross-linked network to a certain extent, thereby avoiding the decrease in the heat resistance of the system caused by the increase in the active flexibility of the molecular chain, which increases the glass transition temperature.
[0097] With the introduction of 20phr BD prepolymer, it can be seen that the glass transition temperature of the epoxy resin system is significantly increased, compensating for the damage to the heat resistance caused by silicone in the epoxy resin system. The glass transition temperature is higher than that of the curing system with the same silicon content. When the silicone content is 70phr, the glass transition temperature is 22°C higher than that of EP. This shows that the introduction of BD prepolymer significantly improves the heat resistance of the modified epoxy resin.
[0098] Test Example 4: Mechanical properties of the modified epoxy resin of the present invention
[0099] The bending strength was tested using an Instron 5567 universal material testing machine from Instron, and the bending properties of the samples were tested according to the GB / T528-2008 standard. The sample size was 80mm×10mm×4mm, and the test speed was 2mm / min. The impact strength was tested using a SANS impact testing machine from Sansi Metrology Technology, and the impact strength was measured according to the GB / T 2567-2008 standard. The test sample size was 80mm×10mm×4mm.
[0100] The bending strength and impact strength of the resin curing system are shown in Table 4. In the silicone-modified epoxy resin system, the bending strength gradually decreases with the increase of silicone content. This is because with the increase of silicon content, the dispersed phase size gradually increases, which easily leads to stress concentration, and the phase interface is a defect of weak point, resulting in reduced strength and modulus. The trend of impact strength change is opposite to that of bending strength. With the increase of silicon content, the impact strength gradually increases. This may be because the silicon phase absorbs a lot of energy when it is destroyed or pulled out.
[0101] In the resin system containing 20phr of bismaleimide prepolymer, the impact strength gradually increases with the silicon content and is higher than that of the pure silicone-modified epoxy system, indicating that the EP-BD@PMPS system has excellent toughness. The impact strength of EP-20BD@70P reaches 15.25kJ / m 2, which is 68.7% higher than that of EP. However, the flexural strength is the highest in EP-20BD@50P, because the 20phr BMI prepolymer has limited improvement on the compatibility of the two due to the agglomeration formed by excessive silicone.
[0102] The above experimental results show that adding silicone to the epoxy resin system will lead to a decrease in the bending and impact resistance of the epoxy resin system, while the addition of bismaleimide prepolymer can significantly improve the bending and impact resistance of the epoxy resin system and enhance the mechanical strength of the epoxy resin system.
[0103] Table 4. Mechanical properties of modified epoxy resin system
[0104]
[0105] Test Example 5: Ablation Performance of the Modified Epoxy Resin of the Present Invention
[0106] According to the GJB323A-96 standard, the ablation resistance of the modified epoxy resin prepared in Example 1 was tested on an oxyacetylene ablation machine produced by Xi'an Zhirui Industrial System Engineering Co., Ltd. The test heat flux density was adjusted to 4 MW / m 2 , the test time is 20s. The mass ablation rate (R m ) and line ablation rate (R l ):
[0107] R m =(m1-m2) / t, R l =(h1-h2) / t
[0108] Wherein: m1 and m2 are the masses of the samples before and after the modified epoxy resin test; h1 and h2 are the thicknesses of the samples before and after the modified epoxy resin test; t is the time of the oxyacetylene ablation test.
[0109] The ablation rate results of the resin-cured system are as follows: Figure 5 As shown in the figure. Due to its poor thermal stability and low residual weight, EP exhibits extremely poor ablation resistance. The substrate is quickly burned through by the flame and no effective carbon layer is formed. For the silicon-containing system, the ablation rate decreases significantly with the increase of silicon content, and EP@50P exhibits the best ablation resistance.
[0110] After the introduction of 20phr bismaleimide prepolymer, the ablation rate of the system tends to be stable, and the ablation rate of EP-20BD@30P is significantly lower than that of EP@30P. Its mass ablation rate and line ablation rate are 0.0717g / s and 0.0762mm / s, respectively, which are 76.13% and 82.92% lower than those of EP, and 33.43% and 73.13% lower than those of EP@30P. This shows that at low content of organosilicon, organosilicon and bismaleimide can produce a good improvement effect, and when the content is higher than 50phr, the ablation performance of the system tends to be stable, and the overall performance is very excellent ablation resistance.
[0111] Test Example 6: Study on the performance of the composite material of the present invention
[0112] The flexural strength and interlaminar shear strength (ILSS) were tested using Instron 5567 universal material testing machine. The flexural strength was tested according to GB / T1449-2005 standard, with a sample size of 80mm×12.5mm×2mm and a test speed of 2mm / min. The interlaminar shear strength (ILSS) was tested according to ASTMD2344 standard, with a sample size of 25mm×6mm×2mm and a test speed of 1mm / min.
[0113] The mechanical properties of the resin have a great influence on the composite material. The strength change trend of the composite material at room temperature is similar to that of the matrix. However, at 100°C, the strength decreases with the increase of the silicone content. The flexural strength of EP@70P / CF is reduced to 340.47MPa, and the ILSS is reduced by 9.29MPa, a decrease of more than 70%. The introduction of BD effectively compensates for the loss of thermomechanical properties caused by silicone. At the same silicon content, the high-temperature flexural strength and interlaminar shear strength of the composite material containing bismaleimide are significantly improved, and EP-20BD@30P / CF even exceeds EP / CF. The composite material exhibits excellent high-temperature mechanical properties.
[0114] Table 5. Mechanical properties of composite materials
[0115]
[0116] In summary, the present invention prepares an epoxy resin synergistically modified by silicone / bismaleimide. The modified epoxy resin of the present invention solves the problem that silicone-modified epoxy resin will lead to a decrease in the glass transition temperature of the epoxy resin system, a decrease in heat resistance, and a deterioration in mechanical properties, thereby improving the glass transition temperature and mechanical properties of the epoxy resin composite system. The use of the modified epoxy resin of the present invention to prepare composite materials can also significantly improve the high-temperature mechanical properties of the composite materials. The present invention expands the application of epoxy resin systems in thermal protection materials and structural materials, and has good application prospects in the fields of aviation and aerospace.
Claims
1. An epoxy resin synergistically modified with silicone / bismaleimide, characterized in that: It is prepared from the following raw materials in the following weight ratio: 100 parts of epoxy resin, 1-50 parts of bismaleimide prepolymer, 30-70 parts of terminal methoxymethyl phenyl silicone intermediate, and 0.01-1 part of catalyst; The structure of the bismaleimide prepolymer is:
2. The organosilicon / bismaleimide synergistically modified epoxy resin according to claim 1, characterized in that: It is prepared from the following raw materials in the following weight ratio: 100 parts of epoxy resin, 20 parts of bismaleimide prepolymer, 30-70 parts of terminal methoxymethyl phenyl silicone intermediate, and 0.15-0.35 parts of catalyst; Preferably, it is prepared from the following raw materials in weight ratio: 100 parts of epoxy resin, 20 parts of bismaleimide prepolymer, 50 parts of terminal methoxymethyl phenyl silicone intermediate, and 0.25 parts of catalyst.
3. The organosilicon / bismaleimide synergistically modified epoxy resin according to claim 1 or 2, characterized in that: The epoxy resin is selected from bisphenol A epoxy resin, 4,5-epoxyhexane-1,2-dicarboxylic acid diglycidyl ester, and tetraglycidylamine epoxy resin; And / or, the structure of the terminal methoxymethyl phenyl organosilicon intermediate is n is an integer from 12 to 15; And / or, the catalyst is selected from butyltin dilaurate, tetraisopropyl titanate, and chloroplatinic acid.
4. The organosilicon / bismaleimide synergistically modified epoxy resin according to claim 1 or 2, characterized in that: The bismaleimide prepolymer is prepared from diallyl bisphenol A and diphenylmethane bismaleimide as raw materials; the mass ratio of diallyl bisphenol A to diphenylmethane bismaleimide is (1-10): (1-10); Preferably, the mass ratio of diallyl bisphenol A to diphenylmethane bismaleimide is 1:
1.
5. The organosilicon / bismaleimide synergistically modified epoxy resin according to claim 4, characterized in that: The preparation method of the bismaleimide prepolymer comprises the following steps: Diallyl bisphenol A and diphenylmethane bismaleimide are mixed and reacted to obtain; Preferably, the reaction temperature is 100-160° C. and the reaction time is 1-5 h.
6. The method for preparing the organosilicon / bismaleimide synergistically modified epoxy resin according to any one of claims 1 to 5, characterized in that: It includes the following steps: (1) Weighing each raw material according to the weight ratio; (2) mixing the epoxy resin and the bismaleimide prepolymer and reacting them to obtain a bismaleimide-modified epoxy resin; (3) mixing the bismaleimide-modified epoxy resin prepared in step (2) with the terminal methoxymethylphenyl silicone intermediate, and then adding a catalyst to react to obtain a silicone / bismaleimide-modified epoxy resin matrix; (4) curing the organosilicon / bismaleimide modified epoxy resin matrix prepared in step (3) to obtain.
7. The preparation method according to claim 6, characterized in that: In step (2), the reaction temperature is 100-150° C., and the reaction time is 1-5 h; And / or, in step (3), the reaction temperature is 100 to 160° C., and the reaction time is 1 to 10 h; And / or, in step (3), the reaction is carried out under an inert environment; And / or, in step (4), when the organosilicon / bismaleimide-modified epoxy resin matrix prepared in step (3) is cured, it is first mixed with a catalyst and preheated, stirred evenly to obtain a resin glue solution, and then cured; Preferably, In step (4), the catalyst is an amine curing agent; And / or, in step (4), the preheating temperature is 100 to 160° C.; And / or, in step (4), the curing conditions are sequentially maintained at 140-160° C. for 1-5 h, 160-200° C. for 1-5 h and 180-220° C. for 1-5 h; More preferably, In step (4), the amine curing agent is selected from 4,4'-diamino-3,3'-dichloroxylene methane, 4,4'-diaminoxylene methane, polyetheramine D400, and polyetheramine D230.
8. Use of the organosilicon / bismaleimide synergistically modified epoxy resin according to any one of claims 1 to 5 in the preparation of heat-resistant thermal protective coatings, high-performance carbon fiber composites, and ablation-resistant composites.
9. A composite material, characterized in that: The invention is prepared by using the epoxy resin modified by organic silicon / bismaleimide as a resin matrix and compounding it with aramid, PBO, quartz, glass fiber or carbon fiber.
10. Use of the composite material according to claim 9 in preparing parts and / or equipment for the aviation and aerospace fields.
Citation Information
Patent Citations
Polyphenyl methoxylsilane and preparation method and application thereof
CN101638481A
Preparation method and application of epoxy resin adhesive
CN102911345A
Bismaleimide modified epoxy resin as well as preparation method and application of bismaleimide modified epoxy resin
CN105385105A
Ablation-resistant organic silicon modified epoxy resin-based carbon fiber composite material and preparation method thereof