Surface modified carbon fiber reinforced polyether-ether-ketone composite material and preparation method thereof
By performing sulfonation treatment, hydroxyl reduction and macromolecule grafting on the surface of carbon fiber polyetheretherketone composites, supramolecular self-assembly is achieved in the high-speed iron environment in vivo, solving its bone repair in iron overload osteoporosis. To solve the problem of insufficient ability, it improves bone regeneration ability and biological activity while maintaining the mechanical properties of the material.
Patent Information
- Application Number
- CN202410778394.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-08
AI Technical Summary
Carbon fiber polyetheretherketone composites have insufficient bone repair capabilities in patients with iron overload osteoporosis, and existing modification methods have a greater impact on mechanical properties or introduce harmful substances, affecting long-term stability.
Through sulfonation treatment, hydroxyl reduction, chain transfer agent esterification, in-situ RAFT polymerization and grafting, macromolecules such as osteoblast adhesion protein and alendronate are promoted on the surface of carbon fiber polyetheretherketone composite materials to achieve in vivo Supramolecular self-assembly and intelligent mechanical transformation in high-speed rail environment.
It improves the bone regeneration ability of carbon fiber polyetheretherketone composite materials under iron overload osteoporosis, maintains excellent mechanical properties, enhances biological activity, and is suitable for bone repair in patients with osteoporosis caused by iron overload.
Smart Images

Figure CN118745263A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomedical materials, and in particular relates to a surface-modified carbon fiber reinforced polyetheretherketone composite material and a preparation method thereof. Background Art
[0002] Carbon fiber polyetheretherketone (CFRPEEK) composite material is an orthopedic implant material with broad application prospects. It is often used as an oral implant material and craniofacial bone defect implant for the treatment of bone damage caused by trauma, disease or congenital defects. This material has excellent mechanical and tribological properties. Its elastic modulus is closer to cortical bone (~20GPa) than traditional metal implant materials (more than 100GPa). It can be adjusted by changing the fiber length and orientation to reduce the risk of osteoporosis and bone resorption caused by stress shielding caused by elastic mismatch between implants and human bones. CFRPEEK composite materials also make up for the weaknesses of PEEK materials in terms of toughness and impact strength deviation, and inherit PEEK's non-toxicity, good chemical resistance, natural radiolucency and MRI (magnetic resonance imaging) compatibility. However, the biological inertness of CFRPEEK composite materials is not conducive to cell growth and adhesion, and its inferior osteointegration ability prevents it from forming a strong bond with human bone tissue after implantation, thereby affecting the long-term stability of implant materials in the human body. These shortcomings seriously hinder the clinical application of CFRPEEK composite materials.
[0003] In order to improve the bioactivity of PEEK (polyetheretherketone) and its composite materials, researchers have modified the surface of PEEK and its composite materials through various methods. Among them, the chemical modification method connects the bioactive material to the surface of the CFRPEEK composite material through covalent bonds, which has little effect on the mechanical properties while improving the bioactivity. However, the CFRPEEK composite material improved by the existing method can only achieve bone defect repair in normal patients, and is insufficient for patients with bone defects in complex in vivo microenvironment, such as osteoporosis, osteosarcoma, bacterial infection and other diseases.
[0004] Osteoporosis is a chronic disease caused by local or systemic metabolic abnormalities, accompanied by decreased bone mass, density and destruction of bone microstructure, most commonly in postmenopausal women and middle-aged and elderly people. Iron overload is one of its main causes, because when the iron content in the body exceeds the original binding capacity of transferrin, the accumulation of free iron will produce an iron overload environment in the body. In an iron overload environment, a large amount of reactive oxygen is produced in bone tissue, the possibility of oxidative stress damage is greatly increased, and the proliferation and differentiation of osteoblasts are inhibited. In addition, the increase in intracellular iron content promotes bone resorption by osteoclasts, ultimately destroying the balance of bone metabolism, thereby inducing osteoporosis. More and more evidence shows that iron overload is the main cause of osteoporosis. At present, the bone repair modification method of CFRPEEK composite materials for patients with iron overload osteoporotic bone defects needs further study. Summary of the invention
[0005] The object of the present invention is to provide a surface-modified carbon fiber reinforced polyetheretherketone composite material and a preparation method thereof, aiming to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material comprises the following steps:
[0008] Step S1, taking a carbon fiber reinforced polyetheretherketone composite material, and performing surface sulfonation treatment on the carbon fiber reinforced polyetheretherketone composite material to obtain a sulfonated carbon fiber reinforced polyetheretherketone composite material;
[0009] Step S2, reducing the carbonyl groups on the surface of the sulfonated carbon fiber reinforced polyetheretherketone composite material to hydroxyl groups using sodium borohydride to obtain a carbon fiber reinforced polyetheretherketone composite material with surface hydroxyl groups modified;
[0010] Step S3, grafting the chain transfer agent 4-((((2-carboxyethyl)thio)carbonylthio)thio)-4-cyanovaleric acid onto the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S2 through a catalytic esterification reaction;
[0011] Step S4, grafting the target macromolecule onto the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S3 by in situ reversible addition fragmentation chain transfer (RAFT) polymerization;
[0012] Step S5, grafting the osteoblast adhesion promoting protein KRSR onto the macromolecular end grafted on the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S4;
[0013] Step S6, grafting the bone-forming promoting drug alendronate onto the macromolecular main chain grafted on the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S5.
[0014] Furthermore, the specific steps of step S1 are as follows:
[0015] Step S11, ultrasonically cleaning the carbon fiber reinforced polyetheretherketone composite material with acetone, ethanol, and distilled water in sequence, and then vacuum drying the composite material to obtain a pretreated carbon fiber reinforced polyetheretherketone composite material;
[0016] Step S12, immersing the pretreated carbon fiber reinforced polyetheretherketone composite material in concentrated sulfuric acid and stirring it, then placing it in distilled water to terminate the reaction, and then washing it in acetone and distilled water in turn to remove the concentrated sulfuric acid residue, and then vacuum drying it to obtain a sulfonated carbon fiber reinforced polyetheretherketone composite material.
[0017] Furthermore, the specific operations of step S2 are:
[0018] The sulfonated carbon fiber reinforced polyetheretherketone composite material is mixed with 100 mg of sodium borohydride, and heated at 110-130°C for 5-7 hours with 40-60 ml of anhydrous dimethyl sulfoxide as solvent. Nitrogen is used for protection during the reaction. After the reaction, the surface hydroxyl-modified carbon fiber reinforced polyetheretherketone composite material is ultrasonically cleaned in anhydrous methanol, distilled water, dilute hydrochloric acid, distilled water, and anhydrous ethanol for 15 minutes, 10 minutes, 10 minutes, 10 minutes, and 10 minutes in turn to remove unreacted substances, and then dried with nitrogen to obtain a surface hydroxyl-modified carbon fiber reinforced polyetheretherketone composite material (hydroxyl grafted composite material plate).
[0019] Furthermore, the specific operations of step S3 are:
[0020] 40 mg of 4-(dimethylamino)pyridine (DMAP) and 46 mg of 4-((((2-carboxyethyl)thio)carbonylthio)thio)-4-cyanovaleric acid were put into 23 ml of dichloromethane, and then a hydroxy-grafted composite material plate (12 pieces) was added. After reacting at 0°C for 30 min under an argon environment, 120 mg of N,N'-dicyclohexylcarbodiimide (DCC) dissolved in 2 ml of dichloromethane was put into the system and stirred overnight. The plate was washed 3 times with DCM and ethanol respectively, and dried with a nitrogen gun to obtain a carbon fiber reinforced polyetheretherketone composite material with a surface grafted chain transfer agent (chain transfer agent grafted composite material plate).
[0021] Furthermore, the specific steps of step S4 are as follows:
[0022] Step S41, adding 2,6-bis-(2'-pyridyl)-4-pyridone and potassium carbonate into N,N-dimethylformamide, heating to 80°C, and after 1 hour, adding 3-bromo-1-propanol dropwise into the system, continuing heating and stirring for 7 hours, discharging into deionized water, standing for 1 hour, filtering, and drying to obtain a crude product; purifying the product by a chromatographic column, and evaporating the solvent to obtain a white 4'-(3-hydroxypropoxy)-2,2':6',2"-terpyridine solid;
[0023] Step S42, dissolving 4'-(3-hydroxypropoxy)-2,2':6',2"-terpyridine, 2-isocyanatoethyl acrylate and dibutyltin dilaurate in anhydrous tetrahydrofuran, stirring the mixture for 24 hours, evaporating the solvent under reduced pressure, adding an appropriate amount of petroleum ether, volatilizing at room temperature for 24 hours, and washing with ethanol three times to obtain a white 4'-(propoxyethyl carbamate acrylate)-2,2':6',2"-terpyridine solid;
[0024] Step S43, 0.24g, 0.53mmol 4'-(propoxyethyl carbamate acrylate)-2,2':6',2"-terpyridine monomer and 1.15g, 10mmol N-hydroxyacrylamide are dissolved in a mixed solution of 8ml N,N-dimethylformamide and 2ml deionized water, and then a chain transfer agent is added to graft the composite material plate (12 pieces). After nitrogen bubbling and degassing for 15min, the system is transferred to an oil bath preheated to 80°C. After stirring for 30min, 4,4'-azobis(4-cyanoacetic acid) dissolved in 1ml N,N-dimethylformamide is injected into the system. After continuous reaction for 6h, the composite material plate is washed with deionized water and ethanol for 3 times respectively, and dried with a nitrogen gun to obtain a carbon fiber reinforced polyetheretherketone composite material with in-situ growth of functional random copolymers on the surface (composite material plate after in-situ polymerization).
[0025] Furthermore, the specific operations of step S5 are:
[0026] N-(3-Dimethylamide-nonylpropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 160 mg) and N-hydroxysuccinimide (NHS, 96 mg) were added to 20 ml of PBS, and then 24 in situ polymerized composite plates and KRSR (10 mg) short peptide were added, shaken at 37°C overnight, and washed 3 times with PBS.
[0027] Furthermore, the specific operations of step S6 are:
[0028] 20 composite material plates chemically modified in step S5 were placed in 25 ml of 2.5 mg / ml alendronate (ALN) solution (CH3OH:H2O, v / v=6:4), the system was shaken at 37°C overnight, and washed three times with PBS.
[0029] A surface-modified carbon fiber reinforced polyetheretherketone composite material prepared according to the preparation method of the surface-modified carbon fiber reinforced polyetheretherketone composite material described above.
[0030] A use of the surface modified carbon fiber reinforced polyetheretherketone composite material described above in the preparation of bone transplant materials, and / or bone fixation materials, and / or bone repair materials.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. The surface-modified carbon fiber reinforced polyetheretherketone composite material obtained by the present invention has a macromolecular coating grafted on its surface that realizes endogenous supramolecular self-assembly ability under the high-iron environment in the body, which can realize the intelligent conversion of mechanical effects on the implant surface in the body, thereby improving the bone regeneration ability of the carbon fiber reinforced polyetheretherketone composite material under iron overload osteoporosis.
[0033] 2. The preparation method provided by the present invention will neither cause significant damage to the surface of the carbon fiber reinforced polyetheretherketone composite material nor introduce substances harmful to the human body. While retaining the excellent mechanical properties of the carbon fiber polyetheretherketone composite material, it improves the biological activity of the material. The preparation method of the present invention can obtain an artificial bone replacement material with excellent comprehensive performance.
[0034] 3. The preparation method provided by the present invention has the characteristics of clear process, low requirements on instruments, low cost and easy implementation. It is an excellent method for improving the biological activity of carbon fiber reinforced polyetheretherketone composite materials.
[0035] 4. The surface-modified carbon fiber reinforced polyetheretherketone composite material obtained by the present invention is effective, safe and generally applicable to bone repair in patients with osteoporosis caused by iron overload, and plays a guiding role in the design of new biomaterial surfaces. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The present invention provides a schematic diagram of the structure of a surface-modified carbon fiber reinforced polyetheretherketone composite material prepared in the present invention and its in vivo response mechanism.
[0037] Figure 2 This is a total reflection infrared spectrum (ATR-FTIR) diagram of the surface modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1.
[0038] Figure 3This is a confocal laser scanning microscope (CLSM) scan of the surface-modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 2 and Example 3.
[0039] Figure 4 This is a scanning electron microscope (SEM) scan image of the surface-modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1.
[0040] Figure 5 This is a real shot of the water contact angle test of the surface modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1.
[0041] Figure 6 This is an atomic force microscope (AFM) scanning image of the surface modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1.
[0042] Figure 7 This is a comparison chart of the results of the MC3T3-E1 cell proliferation experiment on the surface-modified carbon fiber reinforced polyetheretherketone composite material obtained in Examples 1-3.
[0043] Figure 8 This is a comparison chart of the results of the RAW 264.7 cell proliferation experiment on the surface-modified carbon fiber reinforced polyetheretherketone composite material obtained in Examples 1-3. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0045] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.
[0046] Embodiment 1: A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material provided by one embodiment of the present invention comprises the following steps:
[0047] Step S1, cutting the carbon fiber reinforced polyetheretherketone composite material into discs with a diameter of 8 mm and a thickness of 2 mm, and ultrasonically cleaning them with acetone, ethanol and distilled water for 3 times (30 min each time), and then drying them in a vacuum drying oven at 60°C and storing them for later use to obtain the pretreated carbon fiber reinforced polyetheretherketone composite material.
[0048] Step S2, immersing the pretreated carbon fiber reinforced polyetheretherketone composite material in concentrated sulfuric acid with a mass concentration of 90-98%, stirring the reaction for 1-5 minutes, placing it in distilled water after the reaction is completed to terminate the reaction, and then washing it in acetone and distilled water in turn to remove the concentrated sulfuric acid residue, and then vacuum drying to obtain a sulfonated carbon fiber reinforced polyetheretherketone composite material (named SCP).
[0049] Step S3, the sulfonated carbon fiber reinforced polyetheretherketone composite material is mixed with 100 mg of sodium borohydride, and 40-60 ml of anhydrous dimethyl sulfoxide is used as a solvent, and the temperature is 110-130 ° C. for 5-7 hours, and nitrogen protection is passed throughout the reaction. After the reaction is completed, the surface hydroxyl-modified carbon fiber reinforced polyetheretherketone composite material is ultrasonically cleaned in anhydrous methanol, distilled water, dilute hydrochloric acid, distilled water, and anhydrous ethanol for 15 minutes, 10 minutes, 10 minutes, 10 minutes, and 10 minutes to remove unreacted substances, and then dried with nitrogen to obtain a surface hydroxyl-modified carbon fiber reinforced polyetheretherketone composite material (named SCP-OH).
[0050] Step S4, 40 mg of 4-(dimethylamino)pyridine (DMAP) and 46 mg of 4-((((2-carboxyethyl)thio)carbonylthio)thio)-4-cyanovaleric acid are placed in 23 ml of dichloromethane, and then a hydroxyl-grafted composite material plate (12 pieces) is added. After reacting at 0° C. for 30 minutes under an argon environment, 120 mg of N,N'-dicyclohexylcarbodiimide (DCC) dissolved in 2 ml of dichloromethane is placed in the system and stirred overnight. The plate is washed 3 times with DCM and ethanol respectively, and dried with a nitrogen gun to obtain a carbon fiber reinforced polyetheretherketone composite material with a surface grafted chain transfer agent (named SCP-CTA).
[0051] Step S5, 2,6-bis-(2'-pyridyl)-4-pyridone (5g, 20mmol) and potassium carbonate (6g, 43.4mmol) were added to 60ml N,N-dimethylformamide, heated to 80°C, and 3-bromo-1-propanol (3g, 21mmol) was added dropwise to the system after 1h, and the heating and stirring were continued for 7h. The material was discharged into 1L deionized water, and after standing for 1h, it was filtered and dried to obtain a crude product. The product was purified by a chromatographic column (developing solvent: ethanol: ethyl acetate: triethylamine, v / v / v = 1:10:1), and the solvent was evaporated to obtain 4'-(3-hydroxypropoxy)-2,2':6',2"-terpyridine solid (yield: 75%).
[0052] Step S6, 4'-(3-hydroxypropoxy)-2,2':6',2"-terpyridine (1.5 g, 5 mmol), 2-isocyanatoethyl acrylate (0.8 g, 5.6 mmol) and 2 drops of dibutyltin dilaurate were dissolved in anhydrous tetrahydrofuran. The mixture was stirred for 24 h, the solvent was evaporated under reduced pressure, an appropriate amount of petroleum ether was added, and the product was evaporated at room temperature for 24 h to precipitate, and washed with ethanol 3 times to obtain a white 4'-(propoxyethyl carbamate acrylate)-2,2':6',2"-terpyridine solid (yield: 88%).
[0053] Step S7, 4'-(propoxyethyl carbamate acrylate)-2,2':6',2"-terpyridine monomer (0.24 g, 0.53 mmol) and N-hydroxy acrylamide (1.15 g, 10 mmol) were dissolved in a mixed solution of 8 ml N,N-dimethylformamide and 2 ml deionized water, and then a chain transfer agent was added to graft the composite material plate (12 pieces). After nitrogen bubbling and degassing for 15 minutes, the system was transferred to an oil bath preheated to 80°C. After stirring for 30 minutes, 4,4'-azobis(4-cyanoacetic acid) dissolved in 1 ml N,N-dimethylformamide was injected into the system. After continuous reaction for 6 hours, the composite material plate was washed with deionized water and ethanol for 3 times, respectively, and dried with a nitrogen gun to obtain a carbon fiber reinforced polyetheretherketone composite material (named SCP-PHCET) with in situ growth of functional random copolymers on the surface.
[0054] In an embodiment of the present invention, the carbon fiber reinforced polyetheretherketone composite material in step S1 is taken from the invention patent with publication number CN107245810B, the invention name: carbon fiber long fiber reinforced polyetheretherketone composite material and its preparation method prepared by long carbon fiber reinforced polyetheretherketone, wherein carbon fiber: polyetheretherketone = 30:70 (wt%). Its specific preparation steps are divided into two parts: the preparation of a three-dimensional (3D) needle felt preform and vacuum melting hot pressing. In the process of the 3D needle felt preform, the polyetheretherketone multifilament is spun by a high-temperature melt spinning machine (Beijing Shibuya Equipment Co., Ltd., China) with a melt index of 42g / 10min spinning grade PEEK special material. The obtained PEEK fiber and carbon fiber (T700-24K, Toray, Japan) are cut into 40mm by a fiber cutting machine. Then 70% PEEK fiber and 30% carbon fiber are washed, mixed, combed, laid and needled to prepare a carbon fiber reinforced polyetheretherketone composite needle felt preform. During the vacuum melting hot pressing process, the carbon fiber reinforced polyetheretherketone needle felt preform is cut into the mold size and then placed in a vacuum hot press. After the heating-pressurization-saturation-cooling molding process, the carbon fiber reinforced polyetheretherketone composite material is finally obtained by demolding. The elastic modulus of the carbon fiber reinforced polyetheretherketone composite material is 18 to 20GPa, which is consistent with the elastic modulus of the cortical bone of the human body, which will reduce the risk of osteoporosis and bone absorption caused by the stress shielding effect between it and the human skeleton after implantation into the human body. In addition, the carbon fiber reinforced polyetheretherketone is also isotropic.
[0055] Embodiment 2: A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material provided by an embodiment of the present invention comprises the following steps:
[0056] Steps S1-S7 are the same as steps S1-S7 in Example 1.
[0057] Step S8, put N-(3-dimethylamide-nonylpropyl)-N'-ethylcarbodiimide hydrochloride (EDC, 160 mg) and N-hydroxysuccinimide (NHS, 96 mg) into 20 ml PBS, then add 24 pieces of carbon fiber reinforced polyetheretherketone composite materials with in situ growth of functional random copolymers on the surface and 10 mg of KRSR short peptide, and shake at 37°C overnight, wash with PBS 3 times, and obtain a carbon fiber reinforced polyetheretherketone composite material with osteoblast-specific recognition peptide KRSR grafted at the end of the surface random copolymer (named SCP-PK).
[0058] Embodiment 3: A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material provided by an embodiment of the present invention comprises the following steps:
[0059] Steps S1-S7 are the same as steps S1-S7 in Example 1.
[0060] Step S8 is the same as step S8 in Example 2.
[0061] Step S9, put 20 composite material plates chemically modified by the above steps into 25 ml of 2.5 mg / ml alendronate (ALN) solution (CH3OH:H2O, v / v=6:4), shake the system at 37°C overnight, wash with PBS three times, and obtain a carbon fiber reinforced polyetheretherketone composite material (named SCP-P(A)-K) with a surface random copolymer backbone grafted with an osteoporosis drug alendronate ALN and an end grafted with an osteoblast-specific recognition peptide KRSR.
[0062] In an embodiment of the present invention, the surface modified carbon fiber reinforced polyetheretherketone composite material prepared in this embodiment is implanted in patients with iron overload osteoporosis, and it is expected to promote bone regeneration through the following effects: in the initial implantation stage, the surface modification layer of the composite material prevents excessive adhesion of macrophages due to its brush-like structure, and the modified ALN induces macrophage apoptosis. After suppressing the immune inflammatory response in the body, osteoblasts appear at the interface between the implant and the tissue. The short peptide KRSR with osteoblast-specific recognition and binding function binds to these osteoblasts. At the same time, in an iron overload environment, due to the supramolecular self-assembly behavior of the composite material surface induced by endogenous iron, the molecular chains on the surface of the implant undergo single molecule folding and intermolecular cross-linking, and this process exerts mechanical force on osteoblasts. As osteoblasts continue to differentiate, early osteogenic marker alkaline phosphatase (ALP) is released in large quantities. ALP acts by hydrolyzing phosphate bonds. At a specific concentration, it opens the phosphate bonds between ALN and the main chain of the random copolymer, resulting in ALN release. This widely used osteoporosis drug has a positive impact on the osteoporotic microenvironment at the bone defect. At the same time, the increased macromolecular spacing promoted by ALN release enhances supramolecular self-assembly. In addition, the terpyridine side groups capture more Fe(III), further promoting the adhesion, proliferation and differentiation of osteoblasts on the implant surface (see Figure 1 ).
[0063] Example 4. A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material provided by an embodiment of the present invention, the only difference between which is from Example 3 is that the ratio of carbon fiber to PEEK fiber inside the carbon fiber reinforced polyetheretherketone composite material preform selected in step S1 is: 40% carbon fiber and 60% PEEK fiber.
[0064] Example 5. A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material provided by an embodiment of the present invention is only different from Example 3 in that the ratio of carbon fiber to PEEK fiber inside the carbon fiber reinforced polyetheretherketone composite material preform selected in step S1 is: 50% carbon fiber and 50% PEEK fiber.
[0065] Example 6. A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material provided by an embodiment of the present invention, the only difference from Example 3 is that the ratio of carbon fiber to PEEK fiber inside the carbon fiber reinforced polyetheretherketone composite material preform selected in step S1 is: 60% carbon fiber and 40% PEEK fiber.
[0066] Experiment 1: The surface modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1 was tested by total reflection infrared spectroscopy (ATR-FTIR). The results are as follows: Figure 2 As shown, after reduction reaction, PEEK (1647cm -1 ) the intensity of the C=O absorption peak is significantly weakened, and the -OH absorption peak (3400cm -1 ), after in situ RAFT polymerization, the characteristic peak of HNC=O appeared in the ATR-FTIR spectrum, confirming that the in situ polymerization of the copolymer was successful.
[0067] Experiment 2: The surface modified carbon fiber reinforced polyetheretherketone composites obtained in Example 2 and Example 3 were scanned by laser confocal microscopy (CLSM) (FITC-labeled ALN and rhodamine-B-labeled KRSR were used to prepare the composites according to the steps in Example 2 and Example 3, respectively). The results are as follows: Figure 3 As shown, it can be found that both SCP-PK and SCP-P(A)-K surfaces have strong green and red fluorescence signals, confirming that ALN and KRSR are successfully grafted on the surface of the composite material.
[0068] Experiment 3: The surface-modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1 was observed using a scanning electron microscope (SEM). Figure 4 As shown in Figure 3, SCP has a relatively uniform surface and multi-level porosity. After the reduction reaction, changes in the pore morphology were observed, which was attributed to the etching effect of NaBH4 on the SCP surface. After CTA grafting on the implant surface, further changes in the surface morphology were obvious, and some pores were covered. After in situ RAFT polymerization, the copolymer formed a film-like structure on the implant surface, covering most of the pores.
[0069] Experiment 4: The hydrophilicity test (water contact angle) of the surface modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1 was performed. The results are as follows Figure 5As shown in the figure, the hydrophilicity of the SCP surface is poor, and the water contact angle is 93.8±5.4°. After reduction with NaBH4, -OH is introduced and the hydrophilicity is improved, and the water contact angle is reduced to 78.8±4.1°. After CTA grafting, with the change of surface morphology and the introduction of -COOH, the water contact angle value becomes 66.5±4.5°. Finally, after in situ RAFT polymerization, the water-soluble copolymer is grafted on the implant surface, and the hydrophilicity is further improved to 63.7±3.9°, which is 32.1% lower than that of SCP, which is conducive to the adhesion and proliferation of osteoblasts.
[0070] Experiment 5: Atomic force microscope (AFM) scanning was performed on the surface modified carbon fiber reinforced polyetheretherketone composite material obtained in Example 1 (wherein the SCP-PHCET group was immersed in ammonium ferric citrate solution for 72 hours to obtain the SCP-P(Fe) group, at which time the copolymer on the surface of the composite material had fully self-assembled into supramolecular). The results are as follows Figure 6 As shown in Figure 3, it can be found that after in situ RAFT polymerization, the surface roughness of the implant increased significantly and the surface morphology changed substantially. After Fe(III) coordination, the surface of the implant became rougher with more thorn-like protrusions, reflecting the physical morphology changes caused by the successful self-assembly of the supramolecular.
[0071] Experiment 6: Mouse osteoblast precursor cells (MC3T3-E1) were cultured in vitro to evaluate the osteoblast proliferation activity of SCP, SCP-PHCET, SCP-PK, and SCP-P(A)-K. Cell Counting Kit (CKK-8, Beyotime, Shanghai, China) was used to detect the proliferation of cells on the surface of the material. The specific operation method is as follows: the sample sterilized by ultraviolet irradiation for 2 hours was placed in a 48-well culture plate, and the drop density in each well was 1×10 4 cell / mL cell suspension; place the cell culture plate in a cell culture incubator with 5% CO2 saturated humidity at 37°C, and change the culture medium every 2-3 days (add 250μM ammonium ferric citrate to the culture medium to simulate the high iron environment in the patient's body); after 1, 4 and 7 days of cell culture, remove the original culture medium, add 200-400μL of new culture medium containing 10% CKK-8 solution, place the culture plate in the incubator and culture for 1-4 hours, then take out 100μL of culture medium from each well and put it into a 96-well plate; use an ELISA reader (iMark, Bio-Rad, USA) to measure the absorbance value of each well at a wavelength of 450nm. The comparison results are as follows Figure 7 As shown, after in situ RAFT polymerization, KRSR conjugation and ALN grafting on the composite surface, the osteoblast proliferation activity was enhanced successively, proving that the endogenous response of the composite surface was achieved as expected and successfully increased the osteoblast proliferation activity.
[0072] Experiment 7: Mouse mononuclear macrophages (RAW 264.7) were used to culture in vitro to evaluate the inflammatory cell proliferation activity of SCP, SCP-PHCET, SCP-PK, and SCP-P(A)-K. Cell Counting Kit (CKK-8, Beyotime, Shanghai, China) was used to detect the proliferation of cells on the surface of the material. The specific operation method is as follows: the sample sterilized by ultraviolet irradiation for 2 hours was placed in a 48-well culture plate, and the drop density in each well was 1×10 4 cell / mL cell suspension; place the cell culture plate in a cell culture incubator with 5% CO2 saturated humidity at 37°C, and change the culture medium every 2-3 days (add 250μM ammonium ferric citrate to the culture medium to simulate the high iron environment in the patient's body); after 1, 3 and 5 days of cell culture, remove the original culture medium, add 200-400μL of new culture medium containing 10% CKK-8 solution, place the culture plate in the incubator and culture for 1-4 hours, then take out 100μL of culture medium from each well and put it into a 96-well plate; use an ELISA reader (iMark, Bio-Rad, USA) to measure the absorbance value of each well at a wavelength of 450nm. The comparison results are as follows Figure 8 As shown, after in situ RAFT polymerization, KRSR conjugation and ALN grafting on the composite surface, the macrophage proliferation activity was weakened successively, proving that the endogenous response of the composite surface was achieved as expected and successfully reduced the proliferation activity of inflammatory cells.
[0073] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.
Claims
1. A method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material, It is characterized in that The following steps are involved: Step S1, taking a carbon fiber reinforced polyetheretherketone composite material, and performing surface sulfonation treatment on the carbon fiber reinforced polyetheretherketone composite material to obtain a sulfonated carbon fiber reinforced polyetheretherketone composite material; Step S2, reducing the carbonyl groups on the surface of the sulfonated carbon fiber reinforced polyetheretherketone composite material to hydroxyl groups using sodium borohydride to obtain a carbon fiber reinforced polyetheretherketone composite material with surface hydroxyl groups modified; Step S3, grafting the chain transfer agent 4-((((2-carboxyethyl)thio)carbonylthio)thio)-4-cyanovaleric acid onto the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S2 through a catalytic esterification reaction; Step S4, grafting the target macromolecule onto the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S3 by in-situ reversible addition-fragmentation chain transfer polymerization; Step S5, grafting the osteoblast adhesion promoting protein KRSR onto the macromolecular end grafted on the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S4; Step S6, grafting the bone-forming promoting drug alendronate onto the macromolecular main chain grafted on the surface of the carbon fiber reinforced polyetheretherketone composite material obtained in step S5.
2. The method for preparing the surface-modified carbon fiber reinforced polyetheretherketone composite material according to claim 1, It is characterized in that The specific steps of step S1 are as follows: Step S11, ultrasonically cleaning the carbon fiber reinforced polyetheretherketone composite material with acetone, ethanol, and distilled water in sequence, and then vacuum drying the composite material to obtain a pretreated carbon fiber reinforced polyetheretherketone composite material; Step S12, immersing the pretreated carbon fiber reinforced polyetheretherketone composite material in concentrated sulfuric acid and stirring it, then placing it in distilled water to terminate the reaction, and then washing it in acetone and distilled water in turn to remove the concentrated sulfuric acid residue, and then vacuum drying it to obtain a sulfonated carbon fiber reinforced polyetheretherketone composite material.
3. The method for preparing the surface-modified carbon fiber reinforced polyetheretherketone composite material according to claim 1, It is characterized in that The specific operations of step S2 are: The sulfonated carbon fiber reinforced polyetheretherketone composite material is mixed with 100 mg of sodium borohydride, and heated at 110-130°C for 5-7 hours with 40-60 ml of anhydrous dimethyl sulfoxide as solvent. Nitrogen is used for protection during the reaction. After the reaction, the surface hydroxyl-modified carbon fiber reinforced polyetheretherketone composite material is ultrasonically cleaned in anhydrous methanol, distilled water, dilute hydrochloric acid, distilled water, and anhydrous ethanol for 15 min, 10 min, 10 min, 10 min, and 10 min in turn to remove unreacted substances, and then dried with nitrogen to obtain a hydroxyl-grafted composite material plate.
4. The method for preparing the surface-modified carbon fiber reinforced polyetheretherketone composite material according to claim 3, It is characterized in that The specific operations of step S3 are: 40 mg of 4-(dimethylamino)pyridine and 46 mg of 4-((((2-carboxyethyl)thio)carbonylthio)thio)-4-cyanovaleric acid were placed in 23 ml of dichloromethane, and then 12 hydroxyl-grafted composite material plates were added. After reacting at 0°C for 30 min under an argon environment, 120 mg of N,N'-dicyclohexylcarbodiimide dissolved in 2 ml of dichloromethane was added to the system and stirred overnight. The plate was washed 3 times with DCM and ethanol respectively, and dried with a nitrogen gun to obtain a chain transfer agent grafted composite material plate.
5. The method for preparing the surface-modified carbon fiber reinforced polyetheretherketone composite material according to claim 4, It is characterized in that The specific steps of step S4 are as follows: Step S41, adding 2,6-bis-(2'-pyridyl)-4-pyridone and potassium carbonate into N,N-dimethylformamide, heating to 80°C, and after 1 hour, adding 3-bromo-1-propanol dropwise into the system, continuing heating and stirring for 7 hours, discharging into deionized water, standing for 1 hour, filtering, and drying to obtain a crude product; purifying the product by a chromatographic column, and evaporating the solvent to obtain a white 4'-(3-hydroxypropoxy)-2,2':6',2"-terpyridine solid; Step S42, dissolving 4'-(3-hydroxypropoxy)-2,2':6',2"-terpyridine, 2-isocyanatoethyl acrylate and dibutyltin dilaurate in anhydrous tetrahydrofuran, stirring the mixture for 24 hours, evaporating the solvent under reduced pressure, adding an appropriate amount of petroleum ether, volatilizing at room temperature for 24 hours, and washing with ethanol three times to obtain a white 4'-(propoxyethyl carbamate acrylate)-2,2':6',2"-terpyridine solid; Step S43, 0.24g, 0.53mmol 4'-(propoxyethyl carbamate acrylate)-2,2':6',2"-terpyridine monomer and 1.15g, 10mmol N-hydroxyacrylamide are dissolved in a mixed solution of 8ml N,N-dimethylformamide and 2ml deionized water, and then 12 pieces of chain transfer agent grafted composite material plates are added. After nitrogen bubbling degassing for 15min, the system is transferred to an oil bath preheated to 80°C, stirred for 30min, and 4,4'-azobis(4-cyanoacetic acid) dissolved in 1ml N,N-dimethylformamide is injected into the system. After continuous reaction for 6h, the composite material plate is washed 3 times with deionized water and ethanol respectively, and dried with a nitrogen gun to obtain a composite material plate after in-situ polymerization.
6. The method for preparing the surface-modified carbon fiber reinforced polyetheretherketone composite material according to claim 5, It is characterized in that The specific operations of step S5 are: 160 mg of N-(3-dimethylamide-nonylpropyl)-N'-ethylcarbodiimide hydrochloride and 96 mg of N-hydroxysuccinimide were added to 20 ml of PBS, and then 24 in situ polymerized composite plates and 10 mg of KRSR short peptide were added, shaken at 37°C overnight, and washed 3 times with PBS.
7. The method for preparing the surface-modified carbon fiber reinforced polyetheretherketone composite material according to claim 1, It is characterized in that The specific operations of step S6 are: 20 composite material plates chemically modified in step S5 were placed in 25 ml of 2.5 mg / ml alendronate solution, the system was shaken overnight at 37°C, and washed three times with PBS; In alendronate solution, CH 3 OH and H 2 The v / v of O is 6:
4.
8. A surface-modified carbon fiber reinforced polyetheretherketone composite material prepared according to the method for preparing a surface-modified carbon fiber reinforced polyetheretherketone composite material according to any one of claims 1 to 7.
9. Use of the surface-modified carbon fiber reinforced polyetheretherketone composite material according to claim 8 in the preparation of bone transplant materials, and / or bone fixation materials, and / or bone repair materials.