Novel antibacterial filler of water-based paint and preparation method of novel antibacterial filler

Through the synergistic effect of chitosan and polyaminopropyl biguanide, a three-dimensional network porous material is generated, which solves the shortcomings of existing paint antibacterial agents in terms of environmental protection and durability, achieves efficient and long-lasting antibacterial effects, and Improved coating stability.

CN118745294AActive Publication Date: 2024-10-08SHENYANG SHUNFENG NEW MATERIAL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411120704.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-08
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Existing paint antibacterial agents have deficiencies in terms of environmental protection, durability and sterilization efficiency. In particular, natural antibacterial agents have low sterilization efficiency and poor durability, while organic antibacterial agents are easily hydrolyzed, making it difficult to meet the needs of environmental protection, non-toxicity and long-lasting antibacterial properties.

Method used

Using a combination of chitosan, methacrylic anhydride, polyaminopropyl biguanide, catalyst and photoinitiator, a three-dimensional network porous material is generated through substitution reaction and free radical copolymerization and cross-linking, forming a synergistic antibacterial filler to improve the antibacterial properties of the coating sex and stability.

Benefits of technology

Significantly improves the antibacterial efficiency and durability of the coating, and enhances its stability and deodorization capabilities, forming an efficient, long-lasting and environmentally friendly antibacterial filler.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention belongs to the technical field of fillers, and relates to a novel antibacterial filler of a water-based coating and a preparation method thereof. The novel antibacterial filler of the water-based paint comprises the following components: 8-10 parts of chitosan, 8-12 parts of methacrylic anhydride, 3-5 parts of polyaminopropyl biguanide, 2-3 parts of a catalyst and 2-3 parts of a photoinitiator. The prepared filler is hydrophilic and convenient to use, the filler can be used after being mixed with the water-based paint in proportion, after the filler absorbs water and swells in the water-based paint, the stability and toughness of the paint are greatly improved through the three-dimensional net-shaped porous structure of the filler, and the filler has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fillers, and relates to a novel antibacterial filler for water-based paint and a preparation method thereof, and in particular to a novel antibacterial filler for water-based paint with durable antibacterial properties and high antibacterial efficiency and a preparation method thereof. Background Art

[0002] With the continuous development of the construction industry, my country's construction capacity has advanced by leaps and bounds, and the amount of paint required for construction has continued to increase. Under the influence of various factors, the paint is very easy to mold and affect the appearance, and even endanger people's lives and health. As people's requirements for quality of life increase and national environmental protection standards are improved, the research and development and production of an environmentally friendly, non-toxic, antibacterial and anti-corrosion filler is particularly urgent.

[0003] There are three main types of antimicrobial agents commonly used in coatings on the market: inorganic antimicrobial agents, organic antimicrobial agents and natural antimicrobial agents. Inorganic antimicrobial agents have been developed and used for the longest time, and the technology is relatively mature, but the antimicrobial ability is obtained by fixing metal atoms (or their ions) to some porous materials through modification. The introduction of metal atoms will cause damage to the environment and even humans; organic antimicrobial agents have fast sterilization efficiency, but are easily hydrolyzed, resistant to temperature changes, and relatively poor in durability; natural antimicrobial agents are mainly derived from various plant tissues, which are environmentally friendly, non-toxic and harmless, but have low sterilization efficiency and need to be modified to improve their performance.

[0004] Therefore, it is necessary to develop an antibacterial agent that works synergistically with natural antibacterial agents and organic antibacterial agents. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a new antibacterial filler for water-based paint and a preparation method thereof, which can not only improve the antibacterial property and durable antibacterial property of the paint, but also improve the stability of the paint.

[0006] A novel antibacterial filler for water-based paint comprises the following components: chitosan, methacrylic anhydride, polyaminopropyl biguanide, a catalyst, and a photoinitiator; the mass proportions of the components are: 8-10 parts of chitosan, 8-12 parts of methacrylic anhydride, 3-5 parts of polyaminopropyl biguanide, 2-3 parts of catalyst, and 2-3 parts of photoinitiator.

[0007] Furthermore, the catalyst is any one of triethylamine, N,N-dimethylbenzylamine and N,N-dimethylcyclohexylamine.

[0008] Furthermore, the photoinitiator is any one of 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone (I2959), 2-hydroxy-2-methyl-1-phenyl-1-propanone (HMPP), and 1-hydroxycyclohexylphenyl ketone.

[0009] A method for preparing a novel antibacterial filler for water-based coatings comprises the following steps: Step 1 (1) Dissolve chitosan in buffer at room temperature, stir evenly, filter out insoluble matter, and prepare a chitosan solution; (2) Add methyl methacrylate to the chitosan solution and carry out a substitution reaction under constant temperature oscillation conditions, and terminate the reaction after 3 hours. After the reaction is completed, precipitate with 90% ethanol, collect the precipitate by centrifugation, wash it three times with 90% ethanol, and dry it in vacuum to obtain a chitosan derivative.

[0010] Step 2, weighing polyaminopropyl biguanide and methacrylic anhydride, adding them into a dimethyl sulfoxide solvent, mixing them evenly and dissolving them completely, then weighing a catalyst and adding them thereto, after the reaction is completed, extracting with dichloromethane, filtering, and drying to obtain modified polyaminopropyl biguanide.

[0011] Step 3, weigh chitosan derivatives, modified polyaminopropyl biguanide, and photoinitiator, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light to generate a three-dimensional mesh porous material through free radical copolymerization and cross-linking. After filtering, drying, and grinding into powder, it can be used as an antibacterial filler for long-term storage.

[0012] Furthermore, in step 1 (1), the buffer solution is a 1% acetic acid-water mixed solution, and the pH value is 5.5.

[0013] Furthermore, in step 1 (2), the mass ratio of the chitosan solution to methyl methacrylate is 1:1.

[0014] Furthermore, in step 1 (2), the chitosan solution and methyl methacrylate are heated at a temperature of 50-70°C and a rotation speed of 150-200 r·min. -1 The reaction was carried out under the conditions of .

[0015] Furthermore, in step 3, the mass ratio of the chitosan derivative to the modified polyaminopropyl biguanide is 20:2-3.

[0016] Furthermore, in step 3, the irradiation time of the ultraviolet lamp is 8-15 minutes.

[0017] Compared with the prior art, the invention has the following beneficial effects.

[0018] 1. Chitosan and polyaminopropyl biguanide are commonly used antibacterial substances. After modification, the two are free radical copolymerized to form a three-dimensional network structure porous material; the antibacterial mechanism of chitosan derivatives and modified polyaminopropyl biguanide complements each other. Because they are positively charged, they are easily adsorbed on the negatively charged bacterial cell membrane. Chitosan derivatives adsorb on the cell membrane to cause the loss of internal nutrients, while modified polyaminopropyl biguanide can form a film and adsorb on the cell membrane to block bacterial respiration. The copolymerization products of the two work synergistically, greatly improving the antibacterial efficiency, making the antibacterial performance of the filler surpass the antibacterial properties of a single component, and the antibacterial durability is also improved. The addition of modified polyaminopropyl biguanide also has a certain deodorizing effect on the coating.

[0019] 2. The filler prepared by the present invention is hydrophilic and easy to use. It can be used by mixing it with water-based paint in proportion. After the filler absorbs water and swells in the water-based paint, its three-dimensional network porous structure greatly improves the stability and toughness of the paint, and has a relatively broad application prospect. DETAILED DESCRIPTION

[0020] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] A novel antibacterial filler for water-based paint comprises the following components: chitosan, methacrylic anhydride, polyaminopropyl biguanide, a catalyst, and a photoinitiator; the mass proportions of the components are: 8-10 parts of chitosan, 12-15 parts of methacrylic anhydride, 3-5 parts of polyaminopropyl biguanide, 2-3 parts of catalyst, and 2-3 parts of photoinitiator.

[0022] Furthermore, the catalyst is any one of triethylamine, N,N-dimethylbenzylamine and N,N-dimethylcyclohexylamine.

[0023] Furthermore, the photoinitiator is any one of 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone (I2959), 2-hydroxy-2-methyl-1-phenyl-1-propanone (HMPP), and 1-hydroxycyclohexylphenyl ketone.

[0024] A method for preparing a novel antibacterial filler for water-based coatings comprises the following steps: Step 1 (1) Dissolve chitosan in buffer at room temperature, stir evenly, filter out insoluble matter, and prepare a chitosan solution; (2) Add methyl methacrylate to the chitosan solution and carry out a substitution reaction under constant temperature oscillation conditions, and terminate the reaction after 3 hours. After the reaction is completed, precipitate with 90% ethanol, collect the precipitate by centrifugation, wash it three times with 90% ethanol, and dry it in vacuum to obtain a chitosan derivative.

[0025] Step 2, weighing polyaminopropyl biguanide and methacrylic anhydride, adding them into a dimethyl sulfoxide solvent, mixing them evenly and dissolving them completely, then weighing a catalyst and adding them thereto, after the reaction is completed, extracting with dichloromethane, filtering, and drying to obtain modified polyaminopropyl biguanide.

[0026] Step 3, weigh chitosan derivatives, modified polyaminopropyl biguanide, and photoinitiator, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light to generate a three-dimensional mesh porous material through free radical copolymerization and cross-linking. After filtering, drying, and grinding into powder, it can be used as an antibacterial filler for long-term storage.

[0027] Furthermore, in step 1 (1), the buffer solution is a 1% acetic acid-water mixed solution, and the pH value is 5.5.

[0028] Furthermore, in step 1 (2), the mass ratio of the chitosan solution to methyl methacrylate is 1:1.

[0029] Furthermore, in step 1 (2), the chitosan solution and methyl methacrylate are heated at a temperature of 50-70°C and a rotation speed of 150-200 r·min. -1 The reaction was carried out under the conditions of .

[0030] Furthermore, in step 3, the mass ratio of the chitosan derivative to the modified polyaminopropyl biguanide is 20:2-3.

[0031] Furthermore, in step 3, the irradiation time of the ultraviolet lamp is 8-15 minutes.

[0032] The invention provides a novel antibacterial filler for water-based coatings, which is synthesized from chitosan, methacrylic anhydride, polyaminopropyl biguanide, a catalyst and a photoinitiator. The catalyst is triethylamine and the photoinitiator is I2959.

[0033] Example 1.

[0034] A method for preparing a novel antibacterial filler for water-based coatings comprises the following steps: Step 1 (1) Dissolve chitosan in 1% acetic acid-water buffer (pH = 5.5) at room temperature, stir evenly, filter out insoluble matter, and prepare a 3% chitosan solution; (2) Take 8 parts of chitosan solution, add 8 parts of methyl methacrylate into it, and heat at 60℃ and 180r·min -1 The substitution reaction was carried out under constant temperature oscillation, and the reaction was terminated after 3 hours. After the reaction was completed, 90% ethanol was used for precipitation, and the precipitate was collected by centrifugation, washed with 90% ethanol for 3 times, and vacuum dried to obtain a chitosan derivative.

[0035] Step 2, weigh 3 parts of polyaminopropyl biguanide and 1 part of methacrylic anhydride, add them into dimethyl sulfoxide good solvent and mix them evenly, then weigh 2 parts of triethylamine catalyst and add them thereto, after the reaction is completed, extract with dichloromethane, filter and dry to obtain modified polyaminopropyl biguanide.

[0036] Step 3: Take 20 parts of chitosan derivatives, 3 parts of modified polyaminopropyl biguanide, and 2 parts of photoinitiator I2959, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light for 10 minutes to generate a three-dimensional mesh porous material through free radical copolymerization and cross-linking, which is then filtered, dried, and ground into powder.

[0037] Its performance was tested and the results are listed in Table 1.

[0038] Example 2.

[0039] A method for preparing a novel antibacterial filler for water-based coatings comprises the following steps: Step 1 (1) Dissolve chitosan in 1% acetic acid-water buffer (pH = 5.5) at room temperature, stir evenly, filter out insoluble matter, and prepare a 3% chitosan solution; (2) Take 8 parts of chitosan solution, add 8 parts of methyl methacrylate into it, and heat at 60℃ and 180r·min -1 The substitution reaction was carried out under constant temperature oscillation, and the reaction was terminated after 3 hours. After the reaction was completed, 90% ethanol was used for precipitation, and the precipitate was collected by centrifugation, washed with 90% ethanol for 3 times, and vacuum dried to obtain a chitosan derivative.

[0040] Step 2, weigh 3 parts of polyaminopropyl biguanide and 1 part of methacrylic anhydride, add them into dimethyl sulfoxide good solvent and mix them evenly, then weigh 2 parts of triethylamine catalyst and add them thereto, after the reaction is completed, extract with dichloromethane, filter and dry to obtain modified polyaminopropyl biguanide.

[0041] Step 3: Take 20 parts of chitosan derivatives, 2 parts of modified polyaminopropyl biguanide, and 1 part of photoinitiator I2959, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light for 10 minutes to generate a three-dimensional mesh porous material through free radical copolymerization and cross-linking, which is then filtered, dried, and ground into powder.

[0042] Its performance was tested and the results are listed in Table 1.

[0043] Comparative example 1.

[0044] A method for preparing a novel antibacterial filler for water-based coatings comprises the following steps: Step 1 (1) Dissolve chitosan in 1% acetic acid-water buffer (pH = 5.5) at room temperature, stir evenly, filter out insoluble matter, and prepare a 3% chitosan solution; (2) Take 8 parts of chitosan solution, add 8 parts of methyl methacrylate into it, and heat at 60℃ and 180r·min -1 The substitution reaction was carried out under constant temperature oscillation, and the reaction was terminated after 3 hours. After the reaction was completed, 90% ethanol was used for precipitation, and the precipitate was collected by centrifugation, washed with 90% ethanol for 3 times, and vacuum dried to obtain a chitosan derivative.

[0045] Step 2: Take 20 parts of chitosan derivatives and 2 parts of photoinitiator I2959, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light for 10 minutes to cross-link them, filter them, dry them, and grind them into powder.

[0046] Its performance was tested and the results are listed in Table 1.

[0047] Comparative example 2.

[0048] A method for preparing a novel antibacterial filler for water-based coatings comprises the following steps: Step 1 (1) Dissolve chitosan in 1% acetic acid-water buffer (pH = 5.5) at room temperature, stir evenly, filter out insoluble matter, and prepare a 3% chitosan solution; (2) Take 8 parts of chitosan solution, add 8 parts of methyl methacrylate into it, and heat at 60℃ and 180r·min -1 The substitution reaction was carried out under constant temperature oscillation, and the reaction was terminated after 3 hours. After the reaction was completed, 90% ethanol was used for precipitation, and the precipitate was collected by centrifugation, washed with 90% ethanol for 3 times, and vacuum dried to obtain a chitosan derivative.

[0049] Step 2: Take 20 parts of chitosan derivatives, 3 parts of polyaminopropyl biguanide, and 2 parts of photoinitiator I2959, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light for 10 minutes to cross-link them, filter them, dry them, and grind them into powder.

[0050] Its performance was tested and the results are listed in Table 1.

[0051] Comparative example 3.

[0052] A method for preparing a novel antibacterial filler for water-based coatings comprises the following steps: Step 1 (1) Dissolve chitosan in 1% acetic acid-water buffer (pH = 5.5) at room temperature, stir evenly, filter out insoluble matter, and prepare a 3% chitosan solution; (2) Take 8 parts of chitosan solution, add 8 parts of methyl methacrylate into it, and heat at 60℃ and 180r·min -1 The substitution reaction was carried out under constant temperature oscillation, and the reaction was terminated after 3 hours. After the reaction was completed, 90% ethanol was used for precipitation, and the precipitate was collected by centrifugation, washed with 90% ethanol for 3 times, and vacuum dried to obtain a chitosan derivative.

[0053] Step 2, weigh 3 parts of polyaminopropyl biguanide and 1 part of methacrylic anhydride, add them into dimethyl sulfoxide good solvent and mix them evenly, then weigh 2 parts of triethylamine catalyst and add them thereto, after the reaction is completed, extract with dichloromethane, filter and dry to obtain modified polyaminopropyl biguanide.

[0054] Step 3. Take 20 parts of chitosan derivatives, 4 parts of modified polyaminopropyl biguanide, and 2 parts of photoinitiator I2959, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light for 10 minutes to cross-link them. A three-dimensional porous network material is generated through free radical copolymerization and cross-linking, which is then filtered, dried, and ground into powder.

[0055] Its performance was tested and the results are listed in Table 1.

[0056] Table 1 Test results of embodiments and comparative examples.

Claims

1. A novel antibacterial filler for water-based coatings, characterized in that: The invention comprises the following components: chitosan, methacrylic anhydride, polyaminopropyl biguanide, a catalyst and a photoinitiator; the mass proportions of the components are: 8-10 parts of chitosan, 8-12 parts of methacrylic anhydride, 3-5 parts of polyaminopropyl biguanide, 2-3 parts of the catalyst and 2-3 parts of the photoinitiator.

2. The novel antibacterial filler for water-based coatings according to claim 1, characterized in that: The catalyst is any one of triethylamine, N,N-dimethylbenzylamine and N,N-dimethylcyclohexylamine.

3. The novel antibacterial filler for water-based coating according to claim 1, characterized in that: The photoinitiator is any one of 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]-1-propanone, 2-hydroxy-2-methyl-1-phenyl-1-propanone and 1-hydroxycyclohexylphenyl ketone.

4. A method for preparing a novel antibacterial filler for water-based coatings, characterized in that: The following steps are involved: Step 1 (1) Dissolve chitosan in buffer at room temperature, stir evenly, filter out insoluble matter, and prepare a chitosan solution; (2) adding methyl methacrylate to the chitosan solution to carry out a substitution reaction under constant temperature oscillation conditions, and terminating the reaction after 3 hours; after the reaction is completed, precipitating with 90% ethanol, collecting the precipitate by centrifugation, washing with 90% ethanol for 3 times, and vacuum drying to obtain a chitosan derivative; Step 2, weighing polyaminopropyl biguanide and methacrylic anhydride, adding them to a dimethyl sulfoxide solvent, mixing them evenly and dissolving them completely, then weighing a catalyst and adding them thereto, after the reaction is completed, extracting with dichloromethane, filtering, and drying to obtain modified polyaminopropyl biguanide; Step 3, weigh chitosan derivatives, modified polyaminopropyl biguanide, and photoinitiator, dissolve them in deionized water, stir them evenly on a magnetic stirrer, and then irradiate them with ultraviolet light to generate a three-dimensional mesh porous material through free radical copolymerization and cross-linking. After filtering, drying, and grinding into powder, it can be used as an antibacterial filler for long-term storage.

5. The method for preparing the novel antibacterial filler for water-based coating according to claim 4, characterized in that: In step 1 (1), the buffer solution is a 1% acetic acid-water mixed solution, and the pH value is 5.

5.

6. The method for preparing the novel antibacterial filler for water-based coating according to claim 4, characterized in that: In step 1 (2), the mass ratio of chitosan solution to methyl methacrylate is 1:

1.

7. The method for preparing the novel antibacterial filler for water-based coating according to claim 4, characterized in that: In step 1 (2), chitosan solution and methyl methacrylate are heated at a temperature of 50-70°C and a rotation speed of 150-200 r·min. -1 The reaction was carried out under the conditions of .

8. The method for preparing the novel antibacterial filler for water-based coating according to claim 4, characterized in that: In step 3, the chitosan derivative and the modified polyaminopropyl biguanide are in a mass ratio of 20:2-3.

9. The method for preparing a novel antibacterial filler for water-based coatings according to claim 4, characterized in that: In step 3, the ultraviolet lamp irradiation time is 8-15 minutes.

Citation Information

Patent Citations

  • Preparation method of chitosan hydrogel for antiseptic dressing

    CN102675651A

  • Chitosan derivative containing quaternary ammonium nitrogen atoms and guanidyl as well as preparation method and application thereof

    CN103467623A

  • Bio-based antibacterial coating and preparation method thereof

    CN109762447A

  • Preparation method of guanidyl chitosan quaternary ammonium salt antibacterial agent

    CN111057164A

  • Chitosan modified guanidine salt polymer and preparation method thereof, modified waterborne polyurethane and preparation method thereof, and modified waterborne polyurethane coating

    CN112300386A