Coating for food container and spraying method

Through the combination of polymer acrylic matte baking paint and nano-scale colloidal solution, the problem of friction between food container surface paint and metal and A4 printing paper wiping is solved, achieving cost savings and quality improvement of one spraying instead of two, ensuring the paint film stability and scratch resistance.

CN118745305AInactive Publication Date: 2024-10-08ZHEJIANG XIZERONG PAINT CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411129550.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The matte solid-color paint on existing food containers will produce lead marks after drying at high temperatures when rubbed against metal, and will fade when wiped with A4 printing paper. A second coat of matte transparent varnish needs to be sprayed additionally to solve these problems, but this increases material and labor costs, and increased defective rates.

Method used

Use a combination of polymer acrylic matte baking paint, colloidal solution, diluent and curing agent, stir and mix according to the ratio of 8:2:1:4, and form a polymer acrylic matte baking paint through the mixing of multiple materials to increase its smoothness and structural stability, and uses nano-level low-viscosity colloidal solution and isocyanate curing agent to improve the ductility and viscosity of the coating. It adopts a one-time spraying method and uses a 1.8mm spray gun to bake at 150°C.

Benefits of technology

The paint film on the surface of the food container is lead-free when rubbed against metal, and does not fade when wiped with A4 printing paper. This reduces material and labor costs, significantly reduces the defective rate, ensures product quality, and improves the scratch resistance and ductility of the paint film. Resilience.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a coating for a food container and a spraying method. The coating comprises high-molecular acrylic acid matte baking varnish, a colloidal solution, a diluent and a curing agent. And stirring and mixing the high-molecular acrylic acid matte baking varnish, the colloidal solution, the diluent and the curing agent according to a ratio of 8: 2: 1: 4. According to the paint for the food container and the spraying method, by changing the composition and proportion of the paint and replacing two-time spraying with one-time spraying, a paint film on the surface of the food container is free of lead marks due to friction with metal and does not fade when being wiped with printing paper.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention particularly relates to a coating material and a spraying method for food containers. Background Art

[0002] The existing matte solid color paint for food containers is sprayed on the surface of the food container, and after being dried at high temperature to form a film, the friction between the paint film and the metal parts will leave obvious lead marks. And when the paint film is rubbed back and forth on A4 printing paper, the printing paper will also have obvious color marks.

[0003] In order to solve the problem of lead marks caused by friction between the paint film and metal, and the problem of color fading caused by wiping with A4 printing paper, it is necessary to spray a second coat of matte transparent varnish on the surface of the matte solid color paint film.

[0004] Although matte varnish perfectly solves the problems of lead marks caused by friction with metal and discoloration caused by wiping with A4 printing paper, it requires spraying a first coat of matte solid color primer and then a second coat of matte transparent varnish on the surface of the food container. This not only doubles the material and labor costs, but the two-coating process also increases the defective rate, thereby increasing the cost of the product. Summary of the invention

[0005] The present invention provides a coating and a spraying method for food containers to solve the above-mentioned technical problems, and specifically adopts the following technical solutions: A coating for food containers, comprising: polymer acrylic matte baking varnish, colloidal solution, diluent and curing agent. The material composition of this solution can effectively improve the stability of the coating structure and the coating covering and shielding performance after one-time spraying of the coating.

[0006] Furthermore, the specific method for preparing the coating for food containers is: stirring and mixing the polymer acrylic matte baking varnish, the colloid solution, the diluent and the curing agent in a ratio of 8:2:1:4. The component ratio of this scheme can make the material structure performance of each component in the coating in an optimized state, and after the combination reaction between them, they have a better supporting effect of the material structure, thereby optimizing the structural performance of the coating itself.

[0007] Furthermore, the polymer acrylic matte paint comprises: acrylic resin, dispersant, titanium dioxide, amino resin, polyester resin, epoxy resin, adhesion promoter, leveling agent, organic solvent and silicon dioxide. The polymer acrylic matte paint composed of the above-mentioned multiple materials has a better smoothing effect, not only has a more stable molecular structure, but also has a certain smoothing effect, which can effectively avoid lead marks caused by friction between the paint film and metal, and fading caused by wiping with A4 printing paper.

[0008] Furthermore, the specific method for preparing the polymer acrylic matte baking varnish is: First, add the acrylic resin and the dispersant, disperse at a uniform speed of 800-1000 rpm for 10-20 minutes and preheat; After preheating, the titanium dioxide is slowly added while being dispersed. After the addition is completed, the titanium dioxide is dispersed at a uniform speed of 1000-1500 rpm for 40-50 minutes to serve as a base material; Grinding the dispersed base material; Fully cool the base material that has reached the grinding fineness standard; Then add the amino resin, the polyester resin, the epoxy resin, the adhesion promoter, the leveling agent, the organic solvent and the silicon dioxide, and disperse at a uniform speed of 1100-1400 revolutions for 25-35 minutes to obtain the polymer acrylic matte paint.

[0009] Through the above-mentioned process steps, the smoothness and glide of the polymer acrylic matte paint can be effectively improved, and the adhesion between the components in the polymer acrylic matte paint can be improved, thereby improving the structural stability of the polymer acrylic matte paint.

[0010] Furthermore, the dispersed base material is ground to a fineness of less than 15 um, so that the coating has a more delicate feel and the visual and tactile effects of the coating are better.

[0011] Furthermore, the base material with the grinding fineness meeting the standard is fully cooled to 15-25°C, so as to ensure the structural support of the base material and make the paint surface structure more stable after spraying.

[0012] Furthermore, the colloidal solution is a nano-scale low-viscosity colloidal solution, and the colloidal solution is any one of an aluminum oxide nano-colloidal solution, an iron oxide nano-colloidal solution, a silicon oxide nano-colloidal solution, a titanium oxide nano-colloidal solution, or a zirconium oxide nano-colloidal solution, or a combination of at least two thereof. By designing the composition of such a colloidal solution, the overall ductility and viscosity of the coating can be improved, thereby improving the bump resistance of the paint surface after spraying.

[0013] Furthermore, the diluent comprises ethyl acetate, butyl acetate, xylene, acetone, isophorone, reactive diluent, coupling agent and aromatic agent. Such a diluent has a better dilution effect, can prevent the polymer acrylic matte baking varnish from sticking, and ensure its smoothness and smoothness.

[0014] Furthermore, the curing agent is an isocyanate curing agent.

[0015] A spraying method for spraying the aforementioned coating for food containers comprises: The coating for food containers is evenly sprayed on the surface of the food container with a 1.8 mm diameter spray gun and an air pressure of 0.3-0.5 MPa to a paint film thickness of 15-20 um, and baked at 150° C. for 30 minutes to form.

[0016] The benefit of the present invention lies in the coating and spraying method for food containers provided. By changing the composition and ratio of the coating, one spraying replaces two sprayings, thereby saving material and labor processing costs. In addition, compared with the two-coating process, the defect rate of the one-time spraying process is significantly reduced, thereby ensuring product quality.

[0017] At the same time, by changing the composition and proportion of the paint film, the subsequent thermal transfer construction will not be affected, and the paint film on the surface of the food container will not print lead when rubbed against metal, and will not fade when wiped against A4 printing paper. Such a paint film has better scratch resistance, and even if a hard object such as a metal buckle scratches the surface of the paint film, it will not leave obvious marks, and it can be easily wiped clean, with a certain degree of extension and recovery ability.

[0018] The paint film of the food container processed by the paint and spraying method for food containers of the present invention can be boiled in boiling water at 100° C. for a long time at high temperature without loss of gloss, bubbling or shedding, and has extremely high structural stability.

[0019] The invention is advantageous in that the coating for food containers provided is made of food-grade materials and is highly safe and environmentally friendly. DETAILED DESCRIPTION

[0020] The embodiments of the present application are described in detail below, and examples of the embodiments are shown. The embodiments are illustrative and intended to be used to explain the present application, but cannot be understood as limiting the present application.

[0021] The present application discloses a coating for food containers, comprising: polymer acrylic matte baking varnish, colloidal solution, diluent and curing agent, the material composition can effectively improve the stability of the coating structure and the coating covering and shielding performance after one-time spraying of the coating. The food container is preferably made of metal. In this embodiment, the food container is a stainless steel thermos cup, which is not limited in this application.

[0022] In this application, the specific method for preparing the coating for food containers is: The polymer acrylic matte baking varnish, colloid solution, diluent and curing agent are stirred and mixed in a ratio of 8:2:1:4. The composition ratio of this solution can make the material structure performance of each component in the coating in an optimized state. After the combination and reaction between them, they have a better supporting effect on the material structure, thereby optimizing the structural performance of the coating itself.

[0023] The colloidal solution is used to greatly improve the firmness of the paint film. The colloidal solution is preferably a nano-scale low-viscosity colloidal solution. In an embodiment of the present application, the colloidal solution is any one or more combinations of aluminum oxide nano-colloidal solution, iron oxide nano-colloidal solution, silicon oxide nano-colloidal solution, titanium oxide nano-colloidal solution or zirconium oxide nano-colloidal solution. Through the composition design of such a colloidal solution, the ductility and viscosity of the coating as a whole can be improved, thereby improving the anti-collision ability of the paint surface after spraying. The paint film after molding does not affect the subsequent thermal transfer construction, and its scratch resistance is better. Even if a hard object such as a metal buckle scratches the surface of the paint film, it will not leave obvious marks, and it can be wiped clean gently, with a certain ductility and recovery ability. Optionally, the colloidal solution is: a combination of aluminum oxide nano-colloidal solution and titanium oxide nano-colloidal solution, a combination of titanium oxide nano-colloidal solution and iron oxide nano-colloidal solution, a combination of iron oxide nano-colloidal solution and silicon oxide nano-colloidal solution, or a combination of silicon oxide nano-colloidal solution and zirconium oxide nano-colloidal solution.

[0024] The diluent is used to adjust the paint liquid to a suitable construction viscosity. In an embodiment of the present application, the diluent is composed of: ethyl acetate, butyl acetate, acetone, isophorone, an active diluent, a coupling agent, and a fragrance. Among them, the active diluent is methyl methacrylate. The coupling agent is methacryloxysilane. The fragrance includes tangerine peel and mint. Such a diluent has a better dilution effect, can avoid the stickiness of the polymer acrylic matte baking paint, and ensure its smoothness and smoothness.

[0025] The curing agent is used to increase the hardness of the paint film. In the present application, the curing agent is an isocyanate curing agent.

[0026] In an embodiment of the present application, the polymer acrylic matte baking varnish comprises: acrylic resin, dispersant, titanium dioxide, amino resin, polyester resin, epoxy resin, adhesion promoter, leveling agent, organic solvent and silica.

[0027] The specific method for preparing polymer acrylic matte baking varnish is: 1. First add acrylic resin and dispersant, disperse at 800-1000 rpm for 10-20 minutes and preheat to 70-80°C. Specifically, disperse at 900 rpm for 15 minutes and preheat to. In the present application, the dispersant is polyphosphate, which can be one or more of sodium pyrophosphate, sodium tripolyphosphate, sodium hexametaphosphate, aryl phosphate and dialkyl sulfosuccinate.

[0028] 2. After preheating, slowly add titanium dioxide while dispersing. After adding, disperse at 1000-1500 rpm for 40-50 minutes as the base material. Specifically, disperse at 1200 rpm for 45 minutes.

[0029] 3. Grind the dispersed base material. Specifically, grind the dispersed base material to a fineness of less than 15 um. Preferably, grind the dispersed base material to a fineness of 12 um.

[0030] 4. Fully cool the base material with the grinding fineness that meets the standard. Specifically, fully cool the base material with the grinding fineness that meets the standard to 15-25°C.

[0031] 5. Then add amino resin, polyester resin, epoxy resin, adhesion promoter, leveling agent, organic solvent and silicon dioxide, and disperse at 1100-1400 rpm for 25-35 minutes to obtain a polymer acrylic matte paint. Specifically, disperse at 1200 rpm for 30 minutes.

[0032] Through the above process steps, the smoothness and glossiness of the polymer acrylic matte paint can be effectively improved, and the viscosity between the components in the polymer acrylic matte paint can be improved, thereby improving the structural stability of the polymer acrylic matte paint. The paint film of the food container processed by the paint and spraying method for food containers can be boiled in 100°C boiling water for about 1 hour without loss of gloss, bubbling, or shedding, and the structural stability is extremely high.

[0033] Embodiment 1:

[0034] 1. First add acrylic resin and dispersant, disperse at 900 rpm for 15 minutes, and preheat to 70°C.

[0035] 2. After preheating, slowly add titanium dioxide while dispersing. After adding, disperse it at a uniform speed of 1200 rpm for 45 minutes as the base material.

[0036] 3. Grind the dispersed base material to a fineness of 12um.

[0037] 4. Cool the base material that meets the grinding fineness standard to 15℃.

[0038] 5. Then add amino resin, polyester resin, epoxy resin, adhesion promoter, leveling agent, organic solvent and silica, and disperse at a uniform speed of 1200 rpm for 30 minutes to obtain a polymer acrylic matte paint.

[0039] Embodiment 2:

[0040] 1. First add acrylic resin and dispersant, disperse at 800 rpm for 20 minutes, and preheat to 80°C.

[0041] 2. After preheating, slowly add titanium dioxide while dispersing. After adding, disperse it at a uniform speed of 1000 rpm for 50 minutes as the base material.

[0042] 3. Grind the dispersed base material to a fineness of 11um.

[0043] 4. Cool the base material that meets the grinding fineness standard to 20℃.

[0044] 5. Then add amino resin, polyester resin, epoxy resin, adhesion promoter, leveling agent, organic solvent and silica, and disperse at a uniform speed of 1100 rpm for 35 minutes to obtain a polymer acrylic matte paint.

[0045] Embodiment 3:

[0046] 1. First add acrylic resin and dispersant, disperse at 1000 rpm for 10 minutes, and preheat to 75°C.

[0047] 2. After preheating, slowly add titanium dioxide while dispersing. After adding, disperse it at a uniform speed of 1500 rpm for 40 minutes as the base material.

[0048] 3. Grind the dispersed base material to a fineness of 14um.

[0049] 4. Cool the base material that meets the grinding fineness standard to 25℃.

[0050] 5. Then add amino resin, polyester resin, epoxy resin, adhesion promoter, leveling agent, organic solvent and silica, and disperse at a uniform speed of 1400 rpm for 25 minutes to obtain a high molecular weight acrylic matte paint.

[0051] The present application also discloses a spraying method for spraying the aforementioned coating for food containers. Specifically, the spraying method comprises: using a 1.8mm caliber spray gun, an air pressure of 0.3-0.5MPa, and spraying the coating for food containers evenly on the surface of the food container with a paint film thickness of 15-20um. Based on the structural properties of the coating for food containers mentioned above, such a spraying method can quickly smooth the coating while ensuring the one-time coverage performance of the coating. While the structure is stable, the paint color can be applied once without the need for a second spraying.

[0052] Bake at 140-160℃ for 25-35 minutes to form. Such baking temperature and baking time can make the coating used for food containers set quickly without affecting the molecular structure performance of each component in the coating, ensuring the original structural advantages of the coating, that is, the bonding structure between the molecular structures of the original components of the coating is stable and unaffected, and it is not easy to have baking wrinkles, and it is not easy to break due to hard collision, ensuring the anti-collision performance.

[0053] Specifically, a 1.8-mm-caliber spray gun was used with an air pressure of 0.3-MPa to uniformly spray the paint for food containers on the surface of the food containers with a paint film thickness of 20 μm, and the paint was baked at 150° C. for 30 minutes to form the containers.

[0054] The coatings prepared in Examples 1 to 3 were sprayed on food containers through the above steps to prepare Examples 1 to 3. Then, ordinary coatings were sprayed on food containers through the above steps to prepare Comparative Example 1.

[0055] The food container prepared above was subjected to a wear resistance test. Specifically, a predetermined white paper was used, pressed on the surface of the thermos cup with a force of 10N, and the paper was rubbed back and forth 10 and 20 times (the distance back and forth remained the same). After that, the contact part of the paper was counted and photographed, and then the photographed results were gray-converted to calculate the average gray value of the image. The results are shown in Table 1 below. It can be seen that the coating prepared by the present application has greater wear resistance after being sprayed on the food container, and the coating is not easily transferred to other objects during the contact and friction process.

[0056] That is to say, the coating and spraying method for food containers mentioned above, by changing the composition and proportion of the coating, replaces two sprayings with one spraying, so that the paint film on the surface of the food container does not print lead when rubbed against the metal, and does not fade when wiped with A4 printing paper. At the same time, one spraying instead of two sprayings also saves material and labor processing costs, and compared with the two-coating process, the defect rate of the one-spraying process is significantly reduced, ensuring product quality. In addition, the benefit of the present invention is that the coating for food containers provided is made of food-grade materials and is highly environmentally friendly.

[0057] Table 1 Comparison results of wear resistance test Average gray value when the number of frictions is 10 Average gray value when the number of frictions is 20 Example 1 249 248 Example 2 251 251 Example 3 251 250 Comparative Example 1 233 230 The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.

Claims

1. A coating for food containers, characterized in that: Contains: polymer acrylic matte baking varnish, colloid solution, diluent and curing agent.

2. The coating for food containers according to claim 1, characterized in that: The specific method for preparing the coating for food containers is: The polymer acrylic matte baking varnish, the colloid solution, the diluent and the curing agent are stirred and mixed in a ratio of 8:2:1:

4.

3. The coating for food containers according to claim 1, characterized in that: The polymer acrylic matte baking varnish comprises: acrylic resin, dispersant, titanium dioxide, amino resin, polyester resin, epoxy resin, adhesion promoter, leveling agent, organic solvent and silicon dioxide.

4. The coating for food containers according to claim 3, characterized in that: The specific method for preparing the polymer acrylic matte baking varnish is: First, add the acrylic resin and the dispersant, disperse at a uniform speed of 800-1000 rpm for 10-20 minutes and preheat; After preheating, the titanium dioxide is slowly added while being dispersed. After the addition is completed, the titanium dioxide is dispersed at a uniform speed of 1000-1500 rpm for 40-50 minutes to serve as a base material; Grinding the dispersed base material; Fully cool the base material that has reached the grinding fineness standard; Then add the amino resin, the polyester resin, the epoxy resin, the adhesion promoter, the leveling agent, the organic solvent and the silicon dioxide, and disperse at a uniform speed of 1100-1400 revolutions for 25-35 minutes to obtain the polymer acrylic matte paint.

5. The coating for food containers according to claim 4, characterized in that: Grind the dispersed base material to a fineness less than 15um.

6. The coating for food containers according to claim 4, characterized in that: The base material with the grinding fineness meeting the standard is fully cooled to 15-25℃.

7. The coating for food containers according to claim 1, characterized in that: The colloidal solution is a nano-scale low-viscosity colloidal solution, and the colloidal solution is any one of an aluminum oxide nano-colloidal solution, an iron oxide nano-colloidal solution, a silicon oxide nano-colloidal solution, a titanium oxide nano-colloidal solution, or a zirconium oxide nano-colloidal solution, or a combination of at least two thereof.

8. The coating for food containers according to claim 1, characterized in that: The diluent comprises ethyl acetate, butyl acetate, xylene, acetone, isophorone, a reactive diluent, a coupling agent and a aromatic agent.

9. The coating for food containers according to claim 1, characterized in that: The curing agent is an isocyanate curing agent.

10. A spraying method for spraying the coating for food containers according to any one of claims 1 to 9, characterized in that: Include: The coating for food containers is evenly sprayed on the surface of the food container with a 1.8 mm diameter spray gun and an air pressure of 0.3-0.5 MPa to a paint film thickness of 15-20 um, and baked at 150° C. for 30 minutes to form.

Citation Information

Patent Citations

  • Matte clear coating composition for aluminum member

    CN108070308A

  • High-hardness high-gloss environment-friendly coating for metal surface and preparation process thereof

    CN112266671A

  • Scratch-resistant wear-resistant water-based matte solid-color stoving varnish for stainless steel vacuum cup and preparation method thereof

    CN114702870A

  • Three-angle full-matte scratch-resistant high-temperature matte black baking varnish for vehicle-mounted magnesium alloy material

    CN117903646A

  • Water-based acrylic amino baking varnish as well as preparation method and application thereof

    CN118271917A