Packaging material for lithium ion battery
Through pressure treatment and material improvement of the hot-welded resin layer of the lithium-ion battery packaging material, the problem of reduced strength of the two-side seals caused by electrolyte penetration was solved, the electrolyte resistance and structural stability of the battery were improved, and the battery was ensured high performance and safety.
Patent Information
- Application Number
- CN202410758592.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
AI Technical Summary
During the electrolyte penetration process of existing lithium-ion battery packaging materials, the adsorption capacity of the thermally bonded resin layer causes the efficiency and strength of the two side seals to decrease, and separation occurs between the thermally bonded resin layer and the middle metal layer, affecting the battery's performance. Use performance.
By using an indentation device to pressurize the thermally welded resin layer, the difference range of the maximum indentation depth is limited, and the material composition of the resin layer is improved to increase crystallinity and density to block the penetration of electrolyte.
It improves the electrolyte resistance and structural strength of lithium-ion battery packaging materials, ensures that the peel strength of the two side seals is close to the initial heat seal strength, reduces the corrosion of the electrolyte on the thermal bonding resin layer and the middle metal layer, and improves Improve battery safety and efficiency.
Smart Images

Figure CN118745323A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery packaging materials, in particular to a lithium ion battery packaging material. Background Art
[0002] Soft-pack lithium-ion batteries have flexible appearance design, so they gradually occupy the main market of lithium-ion batteries. Among them: Since soft-pack lithium-ion batteries are usually composed of metal and resin layers, they are also called metal composite films. Among them: The production process of soft-pack batteries usually includes: (1) lamination; (2) welding of tabs to form battery cells; (3) forming of metal composite films; (4) placing battery cells in the pits after the metal composite films are formed and pre-packaging; (5) injecting electrolyte and sealing; (6) standing at high temperature or room temperature; (7) formation; (8) evacuation and sealing on both sides to basically form the soft-pack battery. Among them, when performing steps (5) to (8), the hot-melt resin layer of the metal composite film will be in full contact with the electrolyte. Since the hot-melt resin layer is mainly composed of polyethylene, polypropylene, polybutylene, or elastomer; and the hot-bonding resin layer is mainly composed of polypropylene resin modified by maleic anhydride, methacrylic acid, etc., the hot-melt resin layer and the hot-bonding resin layer composed of the above raw materials both have a certain ability to absorb the electrolyte, and the electrolyte will penetrate into the hot-melt resin layer and the hot-bonding resin layer in sequence, and finally contact and corrode the intermediate metal layer.
[0003] In addition, when the electrolyte penetrates into the hot-melt resin layer and the heat-bonding resin layer, a part of the heat energy will be used for the volatilization of the electrolyte during the process of sealing the two sides of the metal composite film. Therefore, when the electrolyte penetration is higher, the efficiency and strength of the two-side sealing are worse, and the peel strength is greatly reduced. In addition, when the electrolyte penetration is high, more serious swelling will occur between the hot-melt resin layer and the heat-bonding resin layer. When the electrolyte evaporates due to heat, holes originally used to store the electrolyte will remain in the hot-melt resin layer and the heat-bonding resin layer, and gaps will be left at the interface between the middle metal layer and the heat-bonding resin layer, resulting in poor sealing on both sides, a significant reduction in peel strength, and separation between the heat-bonding resin layer and the middle metal layer, or between the heat-bonding resin layer and the hot-melt resin layer, which greatly increases the defect rate of lithium-ion batteries.
[0004] In summary, it is necessary to prevent the electrolyte from penetrating into the heat-melting resin layer to ensure the strength of the metal composite film for two-side sealing, and to improve the bonding stability between the middle metal layer, the heat-bonding resin layer, and the heat-melting resin layer to prevent stratification therebetween, so as to ensure the performance of the soft-pack lithium-ion battery. Summary of the invention
[0005] The purpose of the present invention is to improve the physical and chemical properties of the heat-melting resin layer to reduce the permeability of the electrolyte to the heat-melting resin layer and to enhance the strength of the metal composite film when sealing on both sides.
[0006] In order to achieve the above-mentioned purpose, the present invention provides a packaging material for lithium-ion batteries, characterized in that it includes a heat-melting resin layer, wherein: using an indentation device under ambient conditions, after the surface of the heat-melting resin layer is pressurized by a pressurized head under a pressurized condition for a preset time, the maximum penetration depth of the pressurized head into the heat-melting resin layer is h1, wherein the length of h1 is 2.0% to 12.0% of the thickness of the heat-melting resin layer; and after the heat-melting resin layer is soaked in an electrolyte, using the indentation device under the ambient conditions, after the surface of the heat-melting resin layer soaked in the electrolyte is pressurized by the pressurized head under the pressurized condition for the preset time, the maximum penetration depth of the pressurized head into the heat-melting resin layer is h2, wherein the length of h2 is 2.0% to 12.0% of the thickness of the heat-melting resin layer, and the difference range of h1 and h2 is -2.0% to +2.0%.
[0007] More preferably, the environmental conditions include: a temperature of 25°C and a relative humidity of 50%; and / or the pressurizing conditions include: a load of 10 mN, a vibration frequency of 220 Hz, and an amplitude of 2 nm; and / or the pressurizing time is 40 s; and / or the indenter is a Berkovich indenter of a regular triangular pyramid type.
[0008] More preferably, the heat-welding resin layer has a crystallinity of 20% to 40%, and / or a number average molecular weight of 80,000 to 150,000, and / or a melting point of 120° C. to 150° C.
[0009] More preferably, it further includes: a heat-bonding resin layer, one side of which is bonded to one side of the heat-melting resin layer; and an intermediate metal layer, one side of which is bonded to the other side of the heat-bonding resin layer, so that the heat-bonding resin layer is located between the intermediate metal layer and the heat-melting resin layer.
[0010] More preferably, it further comprises: an outer base resin layer, which is arranged on the other side of the intermediate metal layer, so that the intermediate metal layer is located between the thermal adhesive resin layer and the outer base resin layer.
[0011] More preferably, the thermal adhesive resin layer has a crystallinity of 3% to 15%, and / or a number average molecular weight of 60,000 to 120,000, and / or a molecular weight distribution of 1.0 to 2.0.
[0012] More preferably, the thickness of the heat-welding resin layer is ≤50 μm, 1 μm≤h1≤5 μm, 1 μm≤h2≤5 μm, and the difference between h1 and h2 ranges from -1.0 μm to +1.0 μm.
[0013] More preferably, 1.5 μm≤h1≤3.5 μm, 1.5 μm≤h2≤3.5 μm, and the difference between h1 and h2 ranges from -0.25 μm to +0.25 μm.
[0014] More preferably, after the hot melt resin layer is acted upon by electrolyte vapor, the indentation device is used under the environmental conditions to pressurize the surface of the hot melt resin layer after the action of electrolyte vapor under the pressurized conditions for the preset time. The maximum penetration depth of the indenter into the hot melt resin layer is h3, wherein the length of h3 is 2.0% to 12.0% of the thickness of the hot melt resin layer, and the difference between h1 and h3 is in the range of -1.5% to +1.5%.
[0015] More preferably, the thickness of the heat-welding resin layer is ≤50 μm, 1 μm≤h3≤5 μm, and the difference between h1 and h3 ranges from -0.5 μm to +0.5 μm.
[0016] More preferably, 1.5 μm≤h3≤3.5 μm, and the difference between h1 and h3 ranges from -0.15 μm to +0.15 μm.
[0017] More preferably, after the two ends of the lithium ion battery packaging material are attached to each other with the hot melt resin layer and pressurized and heat-sealed, a first melt bond is formed on the lithium ion battery packaging material, wherein: when the thickness of the hot melt resin layer is 5μm to 25μm, the peel strength of the first melt bond is A1, and A1≥80N; and when the thickness of the hot melt resin layer is 25μm to 50μm, the peel strength of the first melt bond is B1, and B1≥100N.
[0018] More preferably, after soaking the lithium ion battery packaging material in electrolyte, take it out and wipe it dry, and then affix the two ends of the lithium ion battery packaging material with the hot melt resin layer and pressurize and heat seal it to form a second melt bond on the lithium ion battery packaging material, wherein: when the thickness of the hot melt resin layer is 5μm to 25μm, the peel strength of the second melt bond is A2, wherein A2≥70N, and (A1-A2) / A1×100%≤30%; and when the thickness of the hot melt resin layer is 25μm to 50μm, the peel strength of the second melt bond is B2, wherein B2≥100N, and (B1-B2) / B1×100%≤20%.
[0019] More preferably, the composition of the heat-welding resin layer includes: polyolefin or acid-modified polyolefin.
[0020] More preferably, the polyolefin is one or more selected from homopolypropylene, polypropylene block copolymer, polypropylene random copolymer, low-density polyethylene, medium-density polyethylene, and high-density polyethylene.
[0021] More preferably, the temperature of the electrolyte is 85° C., and the heat-welding resin layer is immersed in the electrolyte for 7 days.
[0022] More preferably, the temperature of the electrolyte vapor is 85° C., and the heat-welding resin layer is allowed to react with the electrolyte vapor for 7 days.
[0023] More preferably, the pressure heat sealing is performed at a temperature of 190° C. and a pressure of 1.0 MPa for 3 seconds to form the first melt-bonded portion on the lithium-ion battery packaging material.
[0024] More preferably, the temperature of the electrolyte is 85° C., and the lithium ion battery packaging material is immersed in the electrolyte for 7 days; and the pressure heat sealing is performed at a temperature of 190° C. and a pressure of 1.0 MPa for 3 seconds to form the second melt-bonded portion on the lithium ion battery packaging material.
[0025] Compared with the prior art, the present invention has the following effects: the present invention limits the difference range of the maximum depth of the hot-melt resin layer before and after the electrolyte is immersed, so that the hot-melt resin layer has excellent electrolyte resistance stability. Since the hot-melt resin layer can effectively block the penetration of liquid or gas electrolyte, it will not cause corrosion of the hot-bonding resin layer or the intermediate metal layer. Moreover, since the electrolyte will not penetrate into the hot-bonding resin layer and the hot-melt resin layer, when the lithium-ion battery packaging material is heat-sealed or two-side sealed, the heat energy in the heat-sealing process will not be lost, so the efficiency, yield and peel strength of the heat sealing and two-side sealing can be ensured, and the peel strength of the two-side sealing can be ensured to be similar to the strength of the initial heat sealing. In addition, the present invention improves the material composition of the hot-melt resin layer, so that the proportion of the crystalline region contained in its structure increases, which can more effectively prevent the penetration of the electrolyte. In summary, by adjusting the physical and chemical properties of the heat-welding resin layer, the lithium-ion battery packaging material of the present invention has excellent electrolyte resistance and stable structural strength, thereby ensuring the performance and safety of the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 is a planar structural diagram for illustrating the structural features of the lithium ion battery packaging material of the present invention;
[0027] Figures 2A to 2B A series of plan views illustrating locations where fusion bonding of packaging materials for lithium-ion batteries is performed;
[0028] Figures 3A to 3DIt is a series of plan views used to illustrate the process of top sealing and side sealing of packaging materials for lithium-ion batteries. DETAILED DESCRIPTION
[0029] In order to make the above and / or other purposes, effects, and features of the present invention more clearly understood, preferred embodiments are specifically described below in detail:
[0030] The object of the present invention is to provide a lithium ion battery packaging material 1, characterized in that: Figure 1 As shown, it includes a hot-melt resin layer 2, wherein: using an indentation device under ambient conditions, after the indenter is pressed on the surface of the hot-melt resin layer 2 under the pressurized condition for a preset time, the maximum penetration depth of the indenter on the hot-melt resin layer 2 is h1, wherein the length of h1 is 2.0% to 12.0% of the thickness of the hot-melt resin layer 2; and after the hot-melt resin layer 2 is soaked in electrolyte, using the indentation device under the ambient conditions, after the indenter is pressed on the surface of the hot-melt resin layer 2 soaked in electrolyte under the pressurized condition for the preset time, the maximum penetration depth of the indenter on the hot-melt resin layer 2 is h2, wherein the length of h2 is 2.0% to 12.0% of the thickness of the hot-melt resin layer 2, and the difference range of h1 and h2 is -2.0% to +2.0%. Specifically, the smaller the difference between the maximum indentation depths h1 and h2 measured before and after the hot-melt resin layer 2 is immersed in the electrolyte, the more stable the electrolyte resistance of the hot-melt resin layer 2 is, so that when it contacts the electrolyte, the electrolyte is not easy to penetrate the hot-melt resin layer 2, and the hot-melt resin layer 2 and the intermediate metal layer 4, or the thermal adhesive resin layer 3 are prevented from being delaminated, and the peel strength of the two side seals of the lithium-ion battery packaging material 1 after immersion is avoided. In a preferred embodiment, the lithium-ion battery packaging material 1 is a metal composite film. In another preferred embodiment, the indentation device is a nanoindenter, but is not limited thereto. In another preferred embodiment, the temperature of the electrolyte is 85°C, and the hot-melt resin layer 2 is immersed in the electrolyte for 7 days.
[0031] More preferably, in order to accurately evaluate the performance of the hot-melt resin layer 2, so that the difference in the maximum penetration depth before and after immersion can be used as an indicator for measuring the electrolyte resistance of the hot-melt resin layer 2, the environmental conditions include: a temperature of 25°C and a relative humidity of 50%; and / or the pressurization conditions include: a load of 10mN, a vibration frequency of 220HZ, and an amplitude of 2nm; and / or the pressurization time is 40s; and / or the indenter is a Berkovich indenter of a regular triangular pyramid type, but is not limited to this. In a preferred embodiment, since the hot-melt resin layer 2 contains crystalline areas and non-crystalline areas, the non-crystalline areas are very easy for the electrolyte to pass through. In order to avoid the electrolyte from penetrating into the hot-melt resin layer 2 in large quantities, which causes stratification in the lithium-ion battery packaging material 1, the hot-melt resin layer 2 has a crystallinity of 20% to 40%, and / or a number average molecular weight of 80,000 to 150,000, and / or a melting point of 120°C to 150°C, but is not limited to this.
[0032] More preferably, in order to improve the stability of the overall structure of the lithium ion battery packaging material 1, Figure 1 As shown, it further comprises: a heat-bonding resin layer 3, one side of which is bonded to one side of the heat-melting resin layer 2; and an intermediate metal layer 4, one side of which is bonded to the other side of the heat-bonding resin layer 3, so that the heat-bonding resin layer 3 is located between the intermediate metal layer 4 and the heat-melting resin layer 2. In a preferred embodiment, it further comprises: an outer substrate resin layer 5, which is arranged on the other side of the intermediate metal layer 4, so that the intermediate metal layer 4 is located between the heat-bonding resin layer 3 and the outer substrate resin layer 5. In another preferred embodiment, in order to make the heat-bonding resin layer 3 closely bonded to the intermediate metal layer 4 and the heat-melting resin layer 2 respectively, so as to improve the stability of the structure of the overall lithium-ion battery packaging material 1, the crystallinity of the heat-bonding resin layer 3 is 3% to 15%, and / or the number average molecular weight is 60,000 to 120,000, and / or the molecular weight distribution is 1.0 to 2.0, but it is not limited thereto.
[0033] More preferably, in order to ensure the electrolyte resistance of the heat-melting resin layer 2 and prevent the electrolyte from easily penetrating into the heat-melting resin layer 2, the thickness of the heat-melting resin layer 2 is ≤50μm, 1μm≤h1≤5μm, 1μm≤h2≤5μm, and the difference between h1 and h2 is in the range of -1.0μm to +1.0μm, but not limited thereto. Preferably, 1.5μm≤h1≤3.5μm, 1.5μm≤h2≤3.5μm, and the difference between h1 and h2 is in the range of -0.25μm to +0.25μm, but not limited thereto.
[0034] More preferably, when the hot-melt resin layer 2 contacts the electrolyte, the vapor formed after the electrolyte evaporates may also penetrate into the hot-melt resin layer 2. In order to ensure that the vapor electrolyte does not destroy the structure of the hot-melt resin layer 2 and affect the peel strength of the lithium-ion battery packaging material 1 after heat sealing, the hot-melt resin layer 2 is acted on by the electrolyte vapor, and the indentation device is used under the environmental conditions to pressurize the surface of the hot-melt resin layer 2 after the electrolyte vapor is acted on for the preset time under the pressurized conditions. The maximum penetration depth of the indenter into the hot-melt resin layer 2 is h3, wherein the length of h3 is 2.0% to 12.0% of the thickness of the hot-melt resin layer 2, and the difference between h1 and h3 is in the range of -1.5% to +1.5%. In a preferred embodiment, in order to ensure the resistance of the heat-melting resin layer 2 to electrolyte vapor, the thickness of the heat-melting resin layer 2 is ≤50μm, 1μm≤h3≤5μm, and the difference between h1 and h3 ranges from -0.5μm to +0.5μm, but not limited thereto. In another preferred embodiment, wherein: 1.5μm≤h3≤3.5μm, and the difference between h1 and h3 ranges from -0.15μm to +0.15μm, but not limited thereto. In another preferred embodiment, the temperature of the electrolyte vapor is 85°C, and the heat-melting resin layer 2 is exposed to the electrolyte vapor for 7 days.
[0035] More preferably, by limiting the maximum penetration depth of the heat-welding resin layer 2, the initial heat-sealing strength of the lithium-ion battery packaging material 1 can be ensured. Specifically: Figure 2A As shown, after the two ends of the lithium ion battery packaging material 1 are attached to each other with the heat-melting resin layer 2 and pressurized and heat-sealed, a first melt-bonded portion 6 is formed on the lithium ion battery packaging material 1, wherein: when the thickness of the heat-melting resin layer 2 is 5μm to 25μm, the peel strength of the first melt-bonded portion 6 is A1, and A1≥80N; and when the thickness of the heat-melting resin layer 2 is 25μm to 50μm, the peel strength of the first melt-bonded portion 6 is B1, and B1≥100N. In a preferred embodiment, when the two ends of the lithium ion battery packaging material 1 are attached to each other, the heat-melting resin layers 2 are attached face to face. In another preferred embodiment, the first melt-bonded portion 6 is formed on the lithium ion battery packaging material 1 by pressurizing and heat-sealing at a temperature of 190°C and a pressure of 1.0MPa for 3 seconds.
[0036] More preferably, by limiting the maximum penetration depth of the heat-welding resin layer 2, the two-side sealing strength of the lithium-ion battery packaging material 1 can be ensured, and the peel strength of the two-side sealing is similar to the peel strength of the initial heat seal. Specifically: Figure 2BAs shown, after the lithium ion battery packaging material 1 is soaked in electrolyte, it is taken out and wiped dry, and then the two ends of the lithium ion battery packaging material 1 are attached to each other with the hot melt resin layer 2 and pressurized and heat-sealed, a second melt bonding point 7 is formed on the lithium ion battery packaging material 1, wherein: when the thickness of the hot melt resin layer 2 is 5μm to 25μm, the peel strength of the second melt bonding point 7 is A2, wherein A2≥70N, and (A1-A2) / A1×100%≤30%; and when the thickness of the hot melt resin layer 2 is 25μm to 50μm, the peel strength of the second melt bonding point 7 is B2, wherein B2≥100N, and (B1-B2) / B1×100%≤20%. In a preferred embodiment, the second melt bonding point 7 is at a different position from the first melt bonding point 6 to avoid mutual interference of test results. In another preferred embodiment, the temperature of the electrolyte is 85° C., and the lithium ion battery packaging material 1 is immersed in the electrolyte for 7 days; and the pressure heat sealing is performed at a temperature of 190° C. and a pressure of 1.0 MPa for 3 seconds to form the second melt-bonded area 7 on the lithium ion battery packaging material 1.
[0037] More preferably, the composition of the heat-melting resin layer 2 includes: polyolefin or acid-modified polyolefin. In a preferred embodiment, the polyolefin is selected from: one or more of homopolypropylene, polypropylene block copolymer, polypropylene random copolymer, low-density polyethylene, medium-density polyethylene, and high-density polyethylene, but not limited thereto.
[0038] The main purpose of the present invention is to avoid the significant decrease in the sealing strength of the two sides of the metal composite film after chemical formation, and to avoid the separation between the heat-bonding resin layer 3 and the intermediate metal layer 4, or between the heat-bonding resin layer 3 and the heat-melting resin layer 2. Specifically, the components of the heat-melting resin layer 2 mainly include: polypropylene, polyethylene, polybutylene, elastomer, and / or processing aids, and form a crystalline region and a non-crystalline region, wherein: since the non-crystalline region is very easy to allow the electrolyte to pass through, the heat-melting resin layer 2 has a certain ability to absorb the electrolyte. In addition, the components of the heat-melting resin layer 2 have a certain amount of low molecular weight components, mainly elastomers and / or other small molecule additives that help processing. Since the low molecular weight components are very easy to dissolve in the electrolyte, the heat-melting resin layer 2 is easily corroded by the electrolyte, and the compactness of the heat-melting resin layer 2 is further reduced, making it easier for the electrolyte to pass through the heat-melting resin layer 2. Among them, in order to prevent the electrolyte from corroding the hot-melt resin layer 2 and prevent the intermediate metal layer 4 from being corroded by the electrolyte, the present invention adopts a hot-melt resin with a relatively high proportion of crystalline regions in the composition, and reduces the content of low molecular weight components therein, so as to reduce the permeability and corrosion of the electrolyte to the hot-melt resin layer 2, and improve the two-side sealing performance of the metal composite film, so that the two-side sealing can be completed. Specifically, the two-side sealing strength of the metal composite film of the present invention is less than the initial heat sealing strength, and the heat-bonding resin layer 3 and the intermediate metal layer 4, and / or the heat-bonding resin layer 3 and the hot-melt resin layer 2 are tightly connected, and are not easy to separate or delaminate.
[0039] The present invention tests the hardness, Young's modulus, and maximum indentation depth of the hot-melt resin layer 2 by an indentation device, wherein: the hot-melt resin layer 2 with a high proportion of the crystalline region exhibits high hardness, large Young's modulus, and shallow maximum indentation depth. When the hot-melt resin layer 2 with a high proportion of the crystalline region is soaked in the electrolyte, the electrolyte has a weak ability to penetrate it, so the hardness, Young's modulus, and maximum indentation depth of the hot-melt resin layer 2 change slightly. In addition, since the content of low molecular weight components contained in the hot-melt resin layer 2 is low, the hot-melt resin layer 2 has few components that can be dissolved by the electrolyte. Combined with the characteristics of its high proportion of the crystalline region, the hot-melt resin layer 2 has a high density and good resistance to electrolyte penetration and corrosion. Therefore, the hot-melt resin layer 2 has a small change in hardness, Young's modulus, and maximum indentation depth before and after the immersion, and has excellent stability.
[0040] The indentation device is mainly used to study the mechanical properties of materials on micro-nano structures. It uses an indenter of a certain shape to press into the material at a uniform rate or a non-uniform rate. In this case, a certain load P is usually applied to the indenter, and within a fixed time, the indenter reaches the maximum depth it can reach. At this time, the maximum indentation depth parameter value h of the tested material, the projected area A of the contact area between the indenter and the material, and the nanoindentation hardness parameter H of the material can be obtained according to the test results of the load P and the projected area A. At the same time, the physical property index of the material can be obtained: Young's modulus parameter E, where the calculation method of each parameter is shown in the following formulas (1) to (3):
[0041] (1) H = P / A
[0042] (2)
[0043] (3)1 / E r =(1-v 2 ) / E+(1-v i 2 ) / E i
[0044] Where: In formula (1), H is hardness, P is load force, and A is contact projection area; in formula (2), S is stiffness, β is a constant related to the indenter geometry, and E r is the simplified Young's modulus, which is the modulus data directly obtained by the machine; in formula (3), E is the Young's modulus of the test material, E i is the Young's modulus of the indenter, v i is the Poisson’s ratio of the indenter, and v is the Poisson’s ratio of the test material.
[0045] According to the above formulas (1) to (3), the larger the maximum indentation depth h of the material, the larger the contact projection area A, the smaller the hardness H, and the smaller the Young's modulus E, wherein: the change trend of the hardness H with the maximum indentation depth h is isotropic with the change trend of the Young's modulus E with the maximum indentation depth h. The Young's modulus of polymer materials is an inherent property of polymer materials, which is related to their molecular chain structure, molecular weight and its distribution, crosslinking degree, crystallinity, orientation, etc. The molecular chain structure, molecular weight and its distribution of the hot-melt resin layer 2 are similar. Since there is no problem of crosslinking degree, its hardness H and Young's modulus E are mainly related to its crystallinity, orientation, the elastomers existing between the chain segments, and the state of the small molecule additives.
[0046] The present invention requires that the hot melt resin layer 2 has a higher hardness H, a higher Young's modulus E, and a lower maximum indentation depth h before the electrolyte is injected. In addition, the present invention tests the hardness H, Young's modulus E, and the maximum indentation depth h of the hot melt resin layer 2 after chemical formation, and evaluates the electrolyte resistance performance of the hot melt resin layer 2 according to the difference in the changes of the three parameters before and after. Among them: among the three parameters of hardness H, Young's modulus E, and maximum indentation depth h, the hardness H parameter usually changes with the instrument model and test conditions, the change difference of Young's modulus E is small, and only the change difference of the maximum indentation depth h is most suitable for evaluating the change of the hot melt resin layer 2 before and after chemical formation, so the present invention mainly limits the maximum indentation depth h of the hot melt resin layer 2.
[0047] Since the crystalline area of the hot melt resin layer 2 of the present invention accounts for a high proportion, a high initial hardness and a low maximum penetration depth can be obtained. In addition, since the crystalline area in the hot melt resin layer 2 of the present invention accounts for a high proportion, the electrolyte has weak permeability to the hot melt resin layer 2; and the content of low molecular weight components in the hot melt resin layer 2 is low, so there are few components that can be dissolved by the electrolyte, and the electrolyte has weak permeability to the hot melt resin layer 2. Therefore, the immersion liquid has little effect on the physical and chemical properties of the hot melt resin layer 2, and the changes in the two parameters of hardness and maximum penetration depth are not obvious. Specifically, the maximum penetration depth of the hot melt resin layer 2 of the present invention after chemical formation has a small change range compared to the initial maximum penetration depth, and the hardness is almost unchanged, with good stability.
[0048] The heat-bonding resin layer 3 is used to bond the intermediate metal layer 4 to the heat-melting resin layer 2. Its main components include: maleic anhydride, and / or methacrylic acid, etc. modified polypropylene resin. Since its components have more polar groups than the heat-melting resin layer 2, it improves the ability of the heat-melting resin layer 2 to adsorb electrolyte, which is not conducive to the two-side sealing. Among them, the role of the polar group in the heat-bonding resin layer 3 is to generate a valence bond with the passivation layer, thereby improving the bonding ability between the heat-bonding resin layer 3 and the intermediate metal layer 4, and between the heat-melting resin layer 2 and the intermediate metal layer 4. The present invention can reduce the penetration of the electrolyte and block the combination of the polar group and the electrolyte by improving the compactness of the heat-melting resin layer 2 under the premise that there are a certain number of polar groups in the heat-bonding resin layer 3. In a preferred embodiment, modified PP with a higher melting point can be used to make the thermal adhesive resin layer 3. Due to its higher melting point, longer polymer chain segments in the thermal adhesive resin layer 3, narrower molecular weight distribution and tighter arrangement, and the arrangement is not easily affected by electrolyte corrosion, it can further hinder the penetration of the electrolyte, promote complete sealing of the two sides after formation, and reduce the probability of separation between the thermal adhesive resin layer 3 and the intermediate metal layer 4.
[0049] 《The following describes the method for measuring the parameters of the heat-sealed resin layer 2》
[0050] 1. First, the initial parameters of the heat-welding resin layer 2 of the metal composite film, such as ① nanoindentation hardness, ② Young's modulus and ③ maximum indentation depth, were tested.
[0051] Under the environmental conditions of temperature of 25°C and relative humidity of 50%, an indentation device is used to press a Berkovich indenter of a right triangular pyramid into the surface of the heat-melting resin layer 2, wherein the load of the indenter is constant at 10Mn, and during the indenter insertion process, a vibration frequency of 220HZ and an amplitude of 2nm are applied to the indenter through piezoelectric ceramics, and the indentation is stopped when the indentation time reaches 40s, thereby obtaining the main parameters of the heat-melting resin layer 2 such as ① maximum indentation depth, ② nanoindentation hardness, and ③ Young's modulus.
[0052] Second, if Figure 3A As shown, using some steps of battery production, a forming machine is used to punch holes in the metal composite film to form a space of a certain size that can accommodate the power core, and the metal composite film with the space is heat-sealed with the metal composite film without the holes, wherein one side is left as a liquid injection port, and after a certain volume of electrolyte is injected into the liquid injection port, the top seal is performed to seal the metal composite film, and a heat-sealed package is obtained. The heat-sealed package is placed at a temperature of 85°C for 7 days and then taken out, and the hot-melt resin layer 2 that is fully in contact with the electrolyte and the hot-melt resin layer 2 that is not in contact with the electrolyte, that is, only corroded by the electrolyte vapor, are tested respectively to obtain: the nanoindentation hardness, Young's modulus, and maximum indentation depth of the hot-melt resin layer 2 after being immersed in an electrolyte at 85°C for 7 days; and the nanoindentation hardness, Young's modulus, and maximum indentation depth of the hot-melt resin layer 2 after being corroded by the electrolyte vapor at 85°C for 7 days.
[0053] 3. Next, test the two-side sealing performance of the metal composite film.
[0054] Cut the metal composite film into certain sizes, such as Figure 3A As shown in FIG. 1 , deep punching is first performed, and then the sheet is folded in half along the MD direction, and the two folded edges are heat-sealed, leaving only the injection port in the TD direction; and as shown in FIG. Figures 3B to 3C As shown, a certain volume of electrolyte is injected from the injection port, and then the top is sealed to obtain a heat-sealed package. The heat-sealed package is placed at a temperature of 60°C for 7 days and then taken out. Figure 3D As shown, two side seals are performed in the area where the heat-melting resin layer 2 is in full contact with the electrolyte, and the strength of the two side seals is tested by a tensile testing machine.
[0055] Among them, when the two sides are not sealed well, it usually manifests as low strength. In addition, if the following situations occur during the test: (a) after the heat-sealed part is pulled open, the PP films on both sides (heat-melting resin layer 2) are intact, it means that the two sides are not sealed completely; or (b) after the heat-sealed part is pulled open, the PP film is separated from the aluminum foil (middle metal layer 4), it means that the electrolyte has corroded the heat-melting resin layer 2 and the heat-adhesive resin layer 3 more seriously.
[0056] In addition, in the above test, when the tensile testing machine is used for the heat seal strength test, the test conditions are as follows: the heat seal part is cut to a width of 15 mm, the distance between the upper and lower clamps of the tensile testing machine is maintained at 50±1 mm, the stretching rate is set to 300 mm / min, and the test stroke is 30 mm. After the test is completed, the maximum tensile force value during the entire stroke is taken as the peel strength of the heat seal part.
[0057] In summary, the initial hardness of the heat-melting resin layer 2 of the present invention is high. After being corroded by the electrolyte, the hardness and maximum penetration depth of the heat-melting resin layer 2 do not change significantly, and the sealing performance of both sides is good.
[0058] As shown in the following Table 1, Examples 1 to 5 of the lithium ion battery packaging material 1 are provided to illustrate the evaluation results of the electrolyte resistance performance of the lithium ion battery packaging material 1 corresponding to the heat-adhesive resin layer 3 and the heat-melting resin layer 2 under different performance conditions. Among them, since the various performance parameters of the heat-adhesive resin layer 3, the various performance parameters of the heat-melting resin layer 2, and the maximum pressing depth of the heat-melting resin layer 2 are all within the range defined by the present invention, the peel strength of the two side seals of the lithium ion battery packaging material 1 of Examples 1 to 5 can be ensured, and the delamination and floating of the lithium ion battery packaging material 1 after being immersed in the electrolyte for a long time at high temperature can be avoided.
[0059] Table 1. Examples 1 to 5 of the present invention
[0060]
[0061] In addition, as shown in the following Table 2, comparative examples 1 to 6 of the lithium ion battery packaging material 1 are provided respectively to illustrate the evaluation results of the electrolyte resistance performance of the lithium ion battery packaging material 1 corresponding to the heat-bonding resin layer 3 and the heat-melting resin layer 2 under different performance conditions, wherein: since the crystallinity of the heat-bonding resin layer 3, the crystallinity of the heat-melting resin layer 2, the ratio of the maximum indentation depth h1 of the heat-melting resin layer 2 to the thickness of the heat-melting resin layer 2, the difference between h1 and h2, or the difference between h1 and h3 in the comparative examples are not within the range defined by the present invention, the peel strength of the two side seals of the lithium ion battery packaging materials 1 of comparative examples 1 to 6 decreases greatly, and there is a high probability that they will be delaminated and floated after being immersed in electrolyte for a long time at high temperature.
[0062] Table 2. Comparative Examples 1 to 4 of the present invention
[0063]
[0064] Compared with the prior art, the present invention has the following effects: the present invention limits the difference range of the maximum depth of the hot-melt resin layer 2 before and after the electrolyte is immersed, so that the hot-melt resin layer 2 has excellent electrolyte resistance stability. Since the hot-melt resin layer 2 can effectively block the penetration of liquid or gas electrolyte, it will not cause corrosion of the hot-bonding resin layer 3 or the intermediate metal layer 4. Moreover, since the electrolyte will not penetrate into the hot-bonding resin layer 3 and the hot-melt resin layer 2, when the lithium-ion battery packaging material 1 is heat-sealed or two-side sealed, the heat energy in the heat-sealing process will not be lost, so the efficiency, yield and peel strength of the heat sealing and two-side sealing can be ensured, and the peel strength of the two-side sealing can be ensured to be similar to the strength of the initial heat sealing. In addition, the present invention further improves the material composition of the hot-melt resin layer 2, so that the proportion of the crystalline region contained in its structure increases, which can more effectively prevent the penetration of the electrolyte. In summary, by adjusting the physical and chemical properties of the heat-welding resin layer 2 , the lithium-ion battery packaging material 1 of the present invention has excellent electrolyte resistance and stable structural strength, thereby ensuring the performance and safety of the lithium-ion battery.
[0065] However, what is described above is only a preferred embodiment of the present invention, but it cannot be used to limit the patent protection scope of the present invention; therefore, all simple equivalent changes and modifications made according to the patent protection scope of the present invention and the contents of the specification still fall within the patent protection scope of the present invention.
Claims
1. A packaging material for lithium-ion batteries, It is characterized in that Comprising a heat-welding resin layer, wherein: Using an indentation device under ambient conditions, after applying pressure to the surface of the heat-melting resin layer for a preset time, the maximum penetration depth of the indentation into the heat-melting resin layer is h1, wherein the length of h1 is 2.0% to 12.0% of the thickness of the heat-melting resin layer; and After the hot melt resin layer is soaked in electrolyte, the indentation device is used under the environmental conditions to pressurize the surface of the hot melt resin layer soaked in electrolyte under the pressurization conditions for the preset time. The maximum penetration depth of the indenter into the hot melt resin layer is h2, wherein the length of h2 is 2.0% to 12.0% of the thickness of the hot melt resin layer, and the difference between h1 and h2 ranges from -2.0% to +2.0%.
2. The lithium ion battery packaging material according to claim 1, Features: The environmental conditions include: a temperature of 25° C. and a relative humidity of 50%; and / or The pressurizing conditions include: a load of 10 mN, a vibration frequency of 220 Hz, and an amplitude of 2 nm; and / or The pressurization time is 40s; and / or The indenter is a Berkovich indenter in a regular triangular pyramid shape.
3. The lithium ion battery packaging material according to claim 1, Features: The heat-melting resin layer has a crystallinity of 20% to 40%, and / or a number average molecular weight of 80,000 to 150,000. and / or a melting point of 120°C to 150°C.
4. The lithium ion battery packaging material according to claim 1, It is characterized in that It also includes: a heat-bonding resin layer, one side of which is bonded to one side of the heat-melting resin layer; as well as One side of the intermediate metal layer is bonded to the other side of the thermal adhesive resin layer so that the thermal adhesive resin layer is located between the intermediate metal layer and the thermal fusion resin layer.
5. The lithium ion battery packaging material according to claim 4, It is characterized in that It further includes: an outer base resin layer, which is arranged on the other side of the intermediate metal layer, so that the intermediate metal layer is located between the thermal bonding resin layer and the outer base resin layer.
6. The lithium ion battery packaging material according to claim 4, Features: The thermal adhesive resin layer has a crystallinity of 3% to 15%, and / or a number average molecular weight of 60,000 to 120,000, and / or a molecular weight distribution of 1.0 to 2.
0.
7. The lithium ion battery packaging material according to claim 1, Features: The thickness of the heat-melting resin layer is ≤50 μm, 1 μm≤h1≤5 μm, 1 μm≤h2≤5 μm, and the difference between h1 and h2 ranges from -1.0 μm to +1.0 μm.
8. The lithium ion battery packaging material according to claim 7, It is characterized in that in: 1.5μm≤h1≤3.5μm, 1.5μm≤h2≤3.5μm, and the difference between h1 and h2 ranges from -0.25μm to +0.25μm.
9. The lithium ion battery packaging material according to claim 1, Features: After the hot melt resin layer is acted upon by electrolyte vapor, the indentation device is used under the environmental conditions to pressurize the surface of the hot melt resin layer after the action of electrolyte vapor under the pressurized conditions for the preset time. The maximum penetration depth of the indenter into the hot melt resin layer is h3, wherein the length of h3 is 2.0% to 12.0% of the thickness of the hot melt resin layer, and the difference between h1 and h3 is in the range of -1.5% to +1.5%.
10. The lithium ion battery packaging material according to claim 9, Features: The thickness of the heat-welding resin layer is ≤50 μm, 1 μm≤h3≤5 μm, and the difference between h1 and h3 ranges from -0.5 μm to +0.5 μm.
11. The lithium ion battery packaging material according to claim 10, It is characterized in that in: 1.5μm≤h3≤3.5μm, and the difference between h1 and h3 ranges from -0.15μm to +0.15μm.
12. The lithium ion battery packaging material according to claim 1, It is characterized in that After the two ends of the lithium ion battery packaging material are attached to each other with the heat-welding resin layer and heat-sealed under pressure, a first fusion bonding portion is formed on the lithium ion battery packaging material, wherein: When the thickness of the heat-welding resin layer is 5 μm to 25 μm, the peel strength of the first fusion bonding portion is A 1 , and A 1 ≥80N; and When the thickness of the heat-welding resin layer is 25 μm to 50 μm, the peel strength of the first fusion bonding portion is B 1 , and B 1 ≥100N.
13. The lithium ion battery packaging material according to claim 12, It is characterized in that After the lithium ion battery packaging material is soaked in electrolyte, it is taken out and wiped dry, and then the two ends of the lithium ion battery packaging material are attached to each other with the heat-welding resin layer and heat-sealed under pressure to form a second fusion bonding portion on the lithium ion battery packaging material, wherein: When the thickness of the heat-melting resin layer is 5 μm to 25 μm, the peel strength of the second melt-bonded portion is A 2 , where A 2 ≥70N, and (A 1 -A 2 ) / A 1 ×100%≤30%; and When the thickness of the heat-melting resin layer is 25 μm to 50 μm, the peel strength of the second melt-bonded portion is B 2 , where B 2 ≥100N, and (B 1 -B 2 ) / B 1 ×100%≤20%.
14. The lithium ion battery packaging material according to claim 1, It is characterized in that The composition of the heat-welding resin layer includes: polyolefin or acid-modified polyolefin.
15. The lithium ion battery packaging material according to claim 14, It is characterized in that The polyolefin is selected from one or more of homopolypropylene, polypropylene block copolymer, polypropylene random copolymer, low-density polyethylene, medium-density polyethylene, and high-density polyethylene.
16. The lithium ion battery packaging material according to claim 1, It is characterized in that The temperature of the electrolyte is 85° C., and the heat-welding resin layer is immersed in the electrolyte for 7 days.
17. The lithium ion battery packaging material according to claim 9, It is characterized in that The temperature of the electrolyte vapor was 85° C., and the heat-welding resin layer was allowed to react with the electrolyte vapor for 7 days.
18. The lithium ion battery packaging material according to claim 12, It is characterized in that The pressure heat sealing is performed at a temperature of 190° C. and a pressure of 1.0 MPa for 3 seconds to form the first melt-bonded portion on the lithium ion battery packaging material.
19. The lithium ion battery packaging material according to claim 13, It is characterized in that The temperature of the electrolyte is 85° C., and the lithium ion battery packaging material is immersed in the electrolyte for 7 days; The second melt-bonded portion is formed on the lithium ion battery packaging material by heat-sealing at a temperature of 190° C. and a pressure of 1.0 MPa for 3 seconds.