Water-based grease-resistant woodworking adhesive and preparation method thereof
Through the emulsion compounding and dispersion process of water-based anti-grease woodworking adhesive, combined with components such as polyvinyl alcohol, silica sol and functional VAE emulsion, the problem of oily resin secretion affecting wood processing is solved, and high-strength, heat-resistant wood is realized Bonding effect.
Patent Information
- Application Number
- CN202411130464.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-08-16
AI Technical Summary
During wood processing, the secretion of oily resin affects the bonding performance of wood, leading to problems such as weak bonding and glue opening. Especially in high-temperature environments, resin penetration leads to surface contamination of wood and affects the quality of wood products.
Water-based anti-grease woodworking adhesive is used, containing components such as polyvinyl alcohol solution, alkaline silica sol, functional VAE emulsion, high-performance latex, oil affinity agent and inorganic reinforcement. It is prepared through an emulsion compound dispersion process to improve the adhesive quality. With excellent permeability and adhesion, it can effectively dissolve and absorb oily resin on the wood surface.
Significantly improves the permeability and adhesion of the adhesive, enhances the colloid strength after curing, solves the problem of weak bonding and cracking of oily wood, improves wood processing performance and surface quality, and is suitable for high temperature environments.
Smart Images

Figure BDA0004997671190000051 
Figure BDA0004997671190000061 
Figure BDA0004997671190000072
Abstract
Description
Technical Field
[0001] The invention relates to a water-based anti-grease woodworking adhesive and a preparation method thereof, in particular to an adhesive suitable for bonding wood processing that is prone to secrete oily resin and a preparation method thereof. Background Art
[0002] The wood structures of tung oil tree, eucalyptus, olive wood, yellow fir, coconut wood, larch, nanmu, silver fir and Chinese fir have normal resin channels, which are easy to secrete oily resins and essential oils, and are rich in resin. During the processing and utilization of wood, high content of resin and essential oils will affect the subsequent sawing, sanding, gluing and painting of wood, and once the ambient temperature is high, the resin will penetrate into the surface of the wood and contaminate the wood products. In addition, this type of wood needs to be effectively treated with resin during the bonding process, so as to improve its processing performance and surface quality and expand its application range.
[0003] In the process of processing wood products, processes such as pressing, plywood, assembly, and veneer are usually used. Various woods are connected by adhesives to form wood products. Due to the structural problems of some woods, after a certain period of time or under the influence of external temperature, humidity, and environment, it will secrete resin, and the resin will penetrate between the glue layer and the interface of the wood. The resin is generally in the form of oil, which not only has low strength and no adhesion, but also has poor solubility with the glue layer. It is dispersed between the wood and the glue layer, affecting the adhesion of the adhesive to the wood. Therefore, wood with high oil content is prone to debonding and cracking at the glued place after bonding, which seriously affects the quality of wood products. Summary of the invention
[0004] In view of the shortcomings of the current water-based woodworking adhesive in the bonding process for oily wood, such as weak bonding and debonding, the present invention provides a water-based anti-grease woodworking adhesive.
[0005] In addition, the present invention also provides a method for preparing the water-based anti-grease woodworking adhesive.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:
[0007] A water-based anti-grease woodworking adhesive comprises the following components in percentage by weight:
[0008] 25-32% polyvinyl alcohol solution, 5-8% alkaline silica sol solution, 10-15% functional EVA emulsion, 15-24% high-performance latex, 0.1-2% pH regulator, 0.2-2% oil affinity agent, 0.05-0.1% penetration enhancer, 10-20% inorganic reinforcing material, 0.2-0.6% additives, and 5-20% water.
[0009] As a further solution of the present invention, the polyvinyl alcohol solution is RS series or BP series polyvinyl alcohol, with a content of 20 wt% aqueous solution, and the polyvinyl alcohol model is one or more of BP17, RS217, and RS120.
[0010] As a further solution of the present invention, the alkaline silica sol is a silica sol solution with a silicon dioxide content of 30% and an average particle size of less than 30 nm.
[0011] As a further solution of the present invention, the inorganic reinforcing material is one or more of 4000 mesh calcined calcined terrene, 1000 mesh heavy calcium carbonate, 1200 mesh light calcium carbonate, and titanium dioxide.
[0012] As a further solution of the present invention, the functional VAE emulsion is a VAE emulsion with a Tg of 10-25° C. and capable of self-crosslinking.
[0013] As a further embodiment of the present invention, the high-performance latex is at least one of anionic carboxylated styrene-butadiene latex and aqueous polyurethane emulsion.
[0014] As a further embodiment of the present invention, the pH regulator is one or more of ammonia water, trisodium phosphate, sodium hydroxide, and triethanolamine.
[0015] As a further embodiment of the present invention, the oil affinity agent is dimethylformamide or a ketone solvent, such as acetone.
[0016] As a further embodiment of the present invention, the penetration enhancer is an ethanol or propylene glycol solution of tetrahydropiperine.
[0017] As a further embodiment of the present invention, the auxiliary agent includes a defoamer, a bactericide, a dispersant, a thickener, etc. In a preferred embodiment, the auxiliary agent includes a mixture of Rhodia mineral oil defoamer DF691, isothiazolinone bactericide, polycarboxylate sodium salt dispersant SN-5040, carboxymethyl cellulose thickener, etc.
[0018] The adhesive of the present invention mainly uses high-performance polyvinyl alcohol solvent as the primary adhesive colloid, and compound functional VAE emulsion and high-performance latex as the main body of the adhesive. At the same time, high-permeability silica sol and penetration promoter are added to increase the penetration and adhesion of the colloid to wood. The grease affinity agent added to the colloid can effectively dissolve the oily resin secreted by the wood. The inorganic reinforcing material added to the formula mainly plays a role in increasing the curing speed and improving the overall strength of the colloid. The adhesive of the present invention has the advantages of being able to dissolve grease on the surface of wood, strong permeability, strong adhesion to wood, high strength after curing, simple to use, and convenient to produce. Due to its excellent performance, it is particularly suitable for having a very good bonding effect on wood that is easy to secrete oily resin. Compared with ordinary water-based woodworking glue, it has strong pertinence and a very obvious bonding effect on oily wood.
[0019] The preparation method of the water-based anti-grease woodworking adhesive of the present invention is an emulsion compounding and dispersing method, which is carried out in a heatable dispersing kettle and comprises the following steps:
[0020] 1) Preparation of polyvinyl alcohol aqueous solution
[0021] Add water to a stirring kettle, slowly add polyvinyl alcohol powder while stirring, heat to above 90°C, keep warm for 60 minutes to completely dissolve it, and obtain a polyvinyl alcohol solution for standby use;
[0022] 2) Dispersed powder
[0023] The polyvinyl alcohol solution is cooled to below 60°C in the dispersion kettle, some additives are added, and after rapid dispersion for 15 minutes, the inorganic reinforcing material is added to the dispersion kettle for dispersion, and samples are taken to detect whether the dispersion is uniform. After dispersion, the pH regulator is added in small amounts and multiple times to adjust the pH value of the material to 8.0-8.5, and the dispersed powder is obtained for standby use;
[0024] 3) Mixed emulsion
[0025] Add functional VAE emulsion and high-performance latex into a stirring kettle, add the remaining additives and penetration enhancers while stirring, slowly add silica sol solution into the stirring kettle after 15 minutes while stirring, add it all in about 30 minutes, add pH adjuster to adjust pH value to 8.0-8.5, and obtain emulsion mixture for standby use;
[0026] 4) Add the emulsion mixture to the dispersed powder, add water, disperse at high speed, take samples to check whether it is evenly dispersed, take samples to test viscosity, solid content, etc., filter and package the material after the indicators are qualified.
[0027] Compared with the existing water-based woodworking glue on the market, the present invention has the following special effects:
[0028] The colloid of the present invention is added with silica sol, which greatly improves the permeability, adhesion and strength of the colloid after curing. The particle size of silica sol is extremely small, generally between 7-40nm, and the dispersibility and permeability are excellent, and it can penetrate into the deep tissue of wood; and the silica sol is added to the latex, and after drying and curing, it can become a solid gel structure, which will produce greater adhesion. (2) The dissolving liquid of tetrahydropiperine is added to the woodworking glue as a strong permeation promoter of the colloid. Tetrahydropiperine is a substance extracted from plants with a strong permeation promoter. It can increase the fluidity of the oil secreted from the wood, promote the diffusion of various active molecules in the colloid between the oil and wood fiber, so that the colloid molecules can better combine with the wood fiber, and enhance the adhesion of the adhesive. (3) The added functional VAE emulsion has a relatively high glass transition temperature and can be self-crosslinked. It has very high cohesion and adhesion. After curing, it has good water resistance and good compatibility with fillers, which can greatly improve the comprehensive performance of the woodworking colloid. (4) The resin and essential oil secreted from the wood are oily substances. The presence of this oil will obviously affect the combination of wood and emulsion. In the present invention, an appropriate amount of dimethylformamide (DMF) or ketone solvent is added as an oil affinity agent. In the molecular structure of DMF, a double-bonded oxygen, a hydrogen and a nitrogen are connected to the carbon, and the nitrogen is connected to two methyl groups. The DMF of this molecular structure is not only stable in nature, but also a highly polar solvent that can be dissolved in water and most solvents. It also has a strong affinity and solubility for organic matter. When the adhesive is attached to the wood, the oil affinity agent will extract the oily substance, thereby reducing its influence, so that the latex is better combined with the wood surface. DETAILED DESCRIPTION
[0029] In order to allow those skilled in the art to understand the present invention more clearly and intuitively, the present invention will be further described below.
[0030] The water-based anti-grease woodworking adhesive of the present invention comprises the following components in percentage by weight:
[0031] 25-32% polyvinyl alcohol solution, 5-8% alkaline silica sol solution, 10-15% functional EVA emulsion, 15-24% high-performance latex, 0.1-2% pH regulator, 0.2-2% oil affinity agent, 0.05-0.1% penetration enhancer, 10-20% inorganic reinforcing material, 0.2-0.6% additives, and 5-20% water.
[0032] The polyvinyl alcohol solution is RS series or BP series polyvinyl alcohol, with a content of 20 wt % in aqueous solution, and the polyvinyl alcohol model is one or more of BP17, RS217, and RS120.
[0033] Alkaline silica sol is a silica sol solution with a silicon dioxide content of 30% and an average particle size of less than 30nm, such as Zhongfa silica sol AJN-830.
[0034] The inorganic reinforcing material is one or more of 4000-mesh calcined calcined terrene, 1000-mesh heavy calcium carbonate, 1200-mesh light calcium carbonate and titanium dioxide.
[0035] Functional VAE emulsion is a VAE emulsion with a Tg of 10-25°C and self-crosslinking, such as Dalian Chemical VAE emulsion DA-691.
[0036] The high-performance latex is at least one of anionic carboxylated styrene butadiene latex or water-based polyurethane emulsion, such as BASF 417 carboxylated styrene butadiene latex and Wanhua Chemical 1645 polyurethane emulsion.
[0037] The pH regulator is one or more of ammonia water, trisodium phosphate, sodium hydroxide, and triethanolamine.
[0038] The oil affinity agent is dimethylformamide or a ketone solvent, such as acetone.
[0039] The penetration enhancer is a solution of tetrahydropiperine in ethanol or propylene glycol.
[0040] The additives include: a mixture of Rhodia mineral oil defoamer DF691, isothiazolinone fungicide, polycarboxylate sodium salt dispersant SN-5040, carboxymethyl cellulose thickener, etc., prepared in a mass ratio of 1:1:1:1.
[0041] Example 1
[0042] The water-based anti-grease woodworking adhesive of the present embodiment comprises the following components in percentage by weight:
[0043]
[0044] The preparation method of the water-based anti-grease woodworking adhesive comprises the following steps:
[0045] Step 1: Add 80 parts by weight of water into a stirring kettle, slowly add 20 parts by weight of polyvinyl alcohol BP17 powder while stirring, heat to 95°C, keep warm for 60 minutes to completely dissolve it, and obtain a 20% concentration of polyvinyl alcohol solution for standby use.
[0046] Step 2: Put the dissolved polyvinyl alcohol solution into the dispersion kettle, cool it to 55℃, add dispersant and defoamer, and disperse it quickly for 15 minutes. Then add heavy calcium carbonate into the dispersion kettle and disperse it for 30 minutes. Take samples to check whether it is evenly dispersed. After dispersion, add pH adjuster and adjust the pH value of the material to 8.0-8.5 in small amounts and multiple times to obtain dispersed powder for standby use.
[0047] Step 3: Add functional VAE emulsion and carboxyl styrene butadiene latex into the stirring kettle, add thickener, fungicide and tetrahydropiperine ethanol solution under stirring, slowly add silica sol solution into the stirring kettle after 15 minutes under stirring, and add it all in about 30 minutes. Add pH adjuster to adjust pH value to 8.0-8.5, and obtain emulsion mixture for standby use.
[0048] Step 4: Add the above emulsion mixture to the dispersed powder, add water, disperse at high speed for 30 minutes, take samples to check whether it is evenly dispersed, take samples to test viscosity, solid content, etc., filter and package the material after the indicators are qualified.
[0049] Example 2
[0050] The water-based anti-grease woodworking adhesive of the present embodiment comprises the following components in percentage by weight:
[0051]
[0052]
[0053] The preparation method of the water-based anti-grease woodworking adhesive comprises the following steps:
[0054] Step 1: Add 80 parts by weight of water into a stirring kettle, slowly add 20 parts by weight of polyvinyl alcohol RS217 powder while stirring, heat to 95°C, keep warm for 60 minutes to completely dissolve it, and obtain a 20% concentration of polyvinyl alcohol solution for standby use.
[0055] Step 2: Put the dissolved polyvinyl alcohol solution into the dispersion kettle, cool it to 50℃, add dispersant and defoamer, disperse it quickly for 15 minutes, then add heavy calcium carbonate into the dispersion kettle and disperse it for 30 minutes. Take samples to check whether it is evenly dispersed. After dispersion, add pH adjuster and adjust the pH value of the material to 8.0-8.5 in small amounts and multiple times to obtain dispersed powder for standby use.
[0056] Step 3: Add functional VAE emulsion and waterborne polyurethane emulsion into the stirring kettle, add thickener, fungicide and propylene glycol solution of tetrahydropiperine under stirring, slowly add silica sol solution into the stirring kettle after 15 minutes under stirring, and add it all in about 30 minutes. Add pH adjuster to adjust pH value to 8.0-8.5, and obtain emulsion mixture for standby use.
[0057] Step 4: Add the above emulsion mixture to the dispersed powder, add water, disperse at high speed for 30 minutes, take samples to check whether it is evenly dispersed, take samples to test viscosity, solid content, etc., filter and package the material after the indicators are qualified.
[0058] Embodiment 3:
[0059] The water-based anti-grease woodworking adhesive of the present embodiment comprises the following components in percentage by weight:
[0060]
[0061]
[0062] The preparation method of the water-based anti-grease woodworking adhesive comprises the following steps:
[0063] Step 1: Add 80 parts by weight of water into a stirring kettle, slowly add polyvinyl alcohol RS217 and RS120 powder while stirring, heat to 100°C, keep warm for 60 minutes to completely dissolve them, and obtain a 20% concentration of polyvinyl alcohol solution for standby use.
[0064] Step 2: Put the dissolved polyvinyl alcohol solution into the dispersion kettle, cool it to 55°C, add dispersant and defoamer, and disperse it quickly for 15 minutes. Then add kaolin and titanium dioxide into the dispersion kettle and disperse them for 30 minutes. Take samples to check whether they are evenly dispersed. After dispersion, add pH adjuster, add it in small amounts and multiple times to adjust the pH value of the material to 8.0-8.5, and obtain dispersed powder for standby use.
[0065] Step 3: Add functional VAE emulsion and carboxylated styrene butadiene latex into the stirring kettle, add the remaining additives and tetrahydropiperine propylene glycol solution under stirring, slowly add silica sol solution into the stirring kettle after 15 minutes under stirring, and add it all in about 30 minutes. Add pH adjuster to adjust the pH value to 8.0-8.5 to obtain the emulsion mixture for standby use.
[0066] Step 4: Add the above emulsion mixture to the dispersed powder, add water, disperse at high speed for 30 minutes, take samples to check whether it is evenly dispersed, take samples to test viscosity, solid content, etc., filter and package the material after the indicators are qualified.
[0067] test:
[0068] The reference standard for wood bonding strength test: Determination method of wood breakage rate of glued surface LY / T2720-2016;
[0069] The reference standard for aging resistance test is: GB / T 8537-2008 "Test method for thermal aging of rubber products";
[0070] D4 water resistance test:
[0071] 1. Keep the sample in good condition for 7 days;
[0072] 2. Soak the sample in boiling water for 4 hours;
[0073] 3. Soak the sample in cold water at room temperature for 1 hour;
[0074] 4. Place the sample in an oven at 50±3℃ for at least 18 hours until the moisture content of the sample drops to the level before the test;
[0075] 5. Check the cracking rate of the glue line. The qualified standard is: the cracking rate is no more than 20%.
[0076] The test results of the adhesive properties obtained in Examples 1-3 are as follows:
[0077]
[0078] Note: √ means the wood is damaged or has passed the D4 water resistance test, and × means the glue has come off or has failed the D4 water resistance test.
[0079] The above test substrates used five different types of oil-rich wood, and three embodiments of the present invention and market brand adhesives were used for comparative experiments. This test used the conventional process of plywood, and the bonding strength, heat resistance, aging resistance and water resistance of the bonded samples were tested after complete curing. From the test results obtained, it can be seen that the water-based grease-resistant wood glue of the present invention shows excellent bonding performance when bonding wood that easily secretes oil. When the bonding strength test was carried out, all the wood was destroyed; the wood could pass the UV heat resistance and aging resistance test 7 days after bonding, and could also pass the D4 water resistance test smoothly.
[0080] In order to study the effects of high-permeability silica sol, penetration enhancer and oil affinity agent on adhesive, a comparative example was set up.
[0081] Comparative Example 1
[0082] The water-based anti-grease woodworking adhesive of this comparative example is different from that of Example 1 in that no highly permeable silica sol solution is added.
[0083] The water-based anti-grease woodworking adhesive of this comparative example comprises the following components in percentage by weight:
[0084]
[0085] Comparative Example 2
[0086] The water-based anti-grease woodworking adhesive of this comparative example is different from that of Example 1 in that no penetration enhancer is added.
[0087] The water-based anti-grease woodworking adhesive of this comparative example comprises the following components in percentage by weight:
[0088]
[0089] Comparative Example 3
[0090] The water-based anti-grease woodworking adhesive of this comparative example is different from that of Example 1 in that no grease affinity agent is added.
[0091] The water-based anti-grease woodworking adhesive of this comparative example comprises the following components in percentage by weight:
[0092]
[0093] The test results of adhesive properties obtained in Comparative Examples 1-3 are as follows:
[0094]
[0095] Note: √ means the wood is damaged or has passed the D4 water resistance test, and × means the glue has come off or has failed the D4 water resistance test.
[0096] Since Comparative Examples 1-3 lack high-permeability silica sol, penetration promoter or grease affinity agent, which have a great influence on the bonding ability, the lack of any one of them makes the bonding strength and heat resistance and aging resistance in the test results fail to pass and show "×". Among them, the Chinese fir passed all performance tests because the Chinese fir material is relatively soft, and only a small adhesive force is needed to make the wood pass the bonding strength test, and it is also easier to pass the heat resistance and aging resistance test. Since high-performance "VAE emulsion" is added to the formula, the water resistance is not affected and is shown as "√".
[0097] The above description of the embodiments is to facilitate the understanding and application of the present invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the embodiments herein, and improvements and modifications made to the present invention by those skilled in the art based on the disclosure of the present invention should be within the scope of protection of the present invention.
Claims
1. A water-based anti-grease woodworking adhesive, characterized in that: The composition comprises the following weight percentages: 25-32% polyvinyl alcohol solution, 5-8% alkaline silica sol solution, 10-15% functional EVA emulsion, 15-24% high-performance latex, 0.1-2% pH regulator, 0.2-2% oil affinity agent, 0.05-0.1% penetration enhancer, 10-20% inorganic reinforcing material, 0.2-0.6% additives, and 5-20% water.
2. A water-based grease-resistant woodworking adhesive as claimed in claim 1, characterized in that: The polyvinyl alcohol solution is a polyvinyl alcohol aqueous solution with a content of 20wt%, and the polyvinyl alcohol model is one or more of BP17, RS217, and RS120.
3. A water-based grease-resistant woodworking adhesive as claimed in claim 1, characterized in that: The alkaline silica sol is a silica sol solution with a silicon dioxide content of 30% and an average particle size of less than 30 nm.
4. A water-based grease-resistant woodworking adhesive as claimed in claim 1, characterized in that: The inorganic reinforcing material is one or more of 4000-mesh calcined calcined terrene, 1000-mesh heavy calcium carbonate, 1200-mesh light calcium carbonate and titanium dioxide.
5. A water-based grease-resistant woodworking adhesive as claimed in claim 1, characterized in that: The functional VAE emulsion has a Tg of 10-25° C. and is self-crosslinkable.
6. A water-based grease-resistant woodworking adhesive as claimed in claim 1, characterized in that: The high-performance latex is at least one of anionic carboxyl styrene butadiene latex and water-based polyurethane emulsion.
7. A water-based grease-resistant woodworking adhesive as claimed in claim 1, characterized in that: The oil affinity agent is dimethylformamide or a ketone solvent.
8. The water-based grease-resistant woodworking adhesive according to claim 1, characterized in that: The penetration enhancer is an ethanol or propylene glycol solution of tetrahydropiperine.
9. A water-based grease-resistant woodworking adhesive as claimed in claim 1, characterized in that: The auxiliary agent comprises: a mixture of Rhodia mineral oil defoamer DF691, isothiazolinone bactericide, polycarboxylic acid sodium salt dispersant SN-5040, and carboxymethyl cellulose thickener.
10. The method for preparing the water-based grease-resistant woodworking adhesive according to any one of claims 1 to 9, characterized in that: The steps include: 1) Preparation of polyvinyl alcohol aqueous solution Add water to a stirring kettle, slowly add polyvinyl alcohol powder while stirring, heat to above 90°C, keep warm for 60 minutes to completely dissolve it, and obtain a polyvinyl alcohol solution for standby use; 2) Dispersed powder The polyvinyl alcohol solution is cooled to below 60°C in a dispersion kettle, some additives are added, and after rapid dispersion for 15 minutes, the inorganic reinforcing material is added to the dispersion kettle for dispersion, and sampling is performed to detect whether it is evenly dispersed. After dispersion, a pH regulator is added in small amounts and multiple times to adjust the pH value of the material to 8.0-8.5, and a dispersed powder is obtained for standby use; the pH regulator is one or more of ammonia water, trisodium phosphate, sodium hydroxide, and triethanolamine; 3) Mixed emulsion Add functional VAE emulsion and high-performance latex into a stirring kettle, add the remaining additives and penetration enhancers while stirring, slowly add silica sol solution into the stirring kettle after 15 minutes while stirring, and add it all in about 30 minutes, add pH adjuster to adjust pH value to 8.0-8.5, and obtain emulsion mixture for standby use; 4) Add the emulsion mixture to the dispersed powder, add water, disperse at high speed, take samples to check whether it is evenly dispersed, take samples to test viscosity, solid content, etc., filter and package the material after the indicators are qualified.
Citation Information
Patent Citations
Water-tolerant polyvinyl acetate wood adhesive and preparation method thereof
CN104403608A
Emulsion for rosewood two-component plate laminating glue and preparation method of emulsion
CN105885738A
One-component aqueous solid-wood joint board adhesive and preparation method thereof
CN110437772A
Water-soluble adhesive for repairing gypsum mold for manufacturing tire mold
JP2006225445A
Cited By
Durable sound insulation tile adhesive and preparation method thereof
CN121406246A
Durable soundproof ceramic tile adhesive and method for preparing the same
CN121406246B