Modified copper slag and preparation method and application thereof
By pulverizing, calcining and quenching the copper slag, and doping it with metal ions, a modified copper slag is formed, which solves the problem of the existing copper slag having poor catalytic removal effect of nitric oxide in the Fenton reaction, and achieves a low dosage , long-lasting catalytic effect, promoting resource utilization and environmental protection of industrial solid waste.
Patent Information
- Application Number
- CN202410763922.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
AI Technical Summary
The existing copper slag is not effective in catalytically removing nitric oxide from flue gas in the Fenton reaction. The catalyst dosage is large and the denitrification duration is short.
By crushing, calcining and quenching the copper slag, it is doped with metal ions to form modified copper slag, which increases surface defects and metal oxides and improves catalytic activity.
It achieves the catalytic effect of small dosage and long denitrification duration, improves the stability of the catalyst and Fenton reaction ability, promotes the resource utilization of industrial solid waste, and reduces resource waste and environmental pollution.
Smart Images

Figure CN118745522A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental protection and industrial solid waste resource utilization, and specifically relates to a modified copper slag and a preparation method and application thereof. Background Art
[0002] With the continuous development of the copper smelting industry, a large amount of low-priced copper slag is produced. The leaching of heavy metals in the copper slag will cause serious damage to the environment and threaten human life. Non-ferrous smelting will produce flue gas and acid tail gas. Nitric oxide in the flue gas or tail gas will pollute the air and form acid rain, so it is necessary to remove the nitrogen monoxide in the flue gas or tail gas.
[0003] Copper slag mainly contains substances such as ferrous silicate and ferroferric oxide. Before modification, the active components are relatively few. When applied to Fenton reaction denitrification (removal of nitrogen monoxide in flue gas), the catalytic effect is not good. Therefore, copper slag needs to be modified. At present, the modification methods of copper slag for Fenton reaction include: adding calcium oxide to copper slag and calcining (Jiacheng Bao, Ping Ning, Fei Wang, et al. Thermal modification of copper slag via phase transformation for simultaneous removal of SO2 and NO x From acid-making tail gas[J].Chemical Engineering Journal, 2021, 425:131646.), the phase structure of the original copper slag is effectively transformed by CaO calcination, resulting in a reduction in the content of Fe(I)-containing substances including Fe3O4, Fe2SiO4 and metal sulfides. However, the use of the above-mentioned modified copper slag (catalyst) for catalytic Fenton reaction denitrification still has the problem of large catalyst dosage and short denitrification duration. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a modified copper slag and its preparation method and application. The catalyst prepared by quenching and modifying the copper slag in the present invention is used for removing nitrogen monoxide from flue gas by Fenton reaction, with small dosage and long denitrification duration.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing modified copper slag, comprising the following steps:
[0007] The copper slag is crushed and screened to obtain copper slag particles;
[0008] calcining the copper slag particles to obtain calcined copper slag;
[0009] Keeping the calcination temperature, adding the calcined copper slag into a metal salt solution for quenching to obtain a mixed solution;
[0010] The mixed liquid is separated into solid and liquid, and the obtained solid is washed and dried to obtain the modified copper slag.
[0011] Preferably, after the quenching treatment, the method further comprises: repeating the calcining treatment and the quenching treatment; the calcining treatment and the quenching treatment are repeated 1 to 7 times.
[0012] Preferably, the particle size of the copper slag particles is less than 200 mesh.
[0013] Preferably, the calcination temperature is 500-1000° C., and the holding time is 15-120 minutes.
[0014] Preferably, the metal salt in the metal salt solution includes one or more of ferric nitrate, cobalt nitrate and manganese nitrate.
[0015] Preferably, the concentration of the metal salt solution is 0.05-4 mol / L.
[0016] Preferably, the temperature of the metal salt solution is 0-30°C.
[0017] Preferably, the washing includes washing with deionized water and washing with anhydrous ethanol; the drying temperature is 80 to 100° C. and the drying time is 6 to 12 hours.
[0018] The present invention also provides modified copper slag obtained by the preparation method described in the above technical solution.
[0019] The present invention also provides the use of the modified copper slag described in the above technical solution in catalytic oxidation of nitrogen monoxide.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] The present invention provides a method for preparing modified copper slag, comprising the following steps: calcining copper slag particles to obtain calcined copper slag; maintaining the calcination temperature and putting the calcined copper slag into a metal salt solution for quenching to obtain the modified copper slag. The present invention quenches and modifies the copper slag in a metal salt solution, and metal ions can be doped into the copper slag. At the same time, the formation of metal oxides on the surface of the copper slag and the crystallization of silicates can increase surface defects, which can be used for Fenton reaction to remove nitrogen monoxide in flue gas, and the denitrification duration is long.
[0022] Furthermore, the present invention can regulate the microscopic morphology of the copper slag surface and the number of doped metal ions through multiple quenching treatments, effectively improve the Fenton reaction ability of the catalyst and have good catalytic stability, which has a positive effect on promoting the resource utilization of industrial solid waste.
[0023] The present invention prepares modified copper slag by quenching and doping copper slag. The preparation method is novel, simple, low-cost, and has good repeatability. It has a good effect for denitrification. The present invention is expected to make full use of the high temperature when copper slag is produced during copper smelting, reduce the waste of resources, save costs, and has important significance for environmental protection. It can improve the economic benefits of enterprises and is conducive to large-scale application of enterprises. The present invention can make full use of the chemical properties of copper slag, regulate the surface of copper slag, and make copper slag resource-utilized, thereby improving the utilization rate of resources in the copper smelting industry and greatly improving the serious impact on the surrounding environment caused by the large amount of copper slag accumulation.
[0024] The present invention can not only efficiently utilize copper slag as a resource, but also solve the problem of removing nitrogen monoxide from industrial flue gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 This is a flow chart of a method for preparing a denitration catalyst by quenching and doping copper slag in an embodiment;
[0027] Figure 2 It is a graph of denitration efficiency of catalysts of Examples 1 to 3 and a comparative example;
[0028] Figure 3 The XRD patterns of the catalyst materials prepared in the comparative example and examples 1 to 3;
[0029] Figure 4 This is a graph showing the denitration efficiency of the catalyst of Example 4. DETAILED DESCRIPTION
[0030] The present invention provides a method for preparing modified copper slag, comprising the following steps:
[0031] The copper slag is crushed and screened to obtain copper slag particles;
[0032] calcining the copper slag particles to obtain calcined copper slag;
[0033] Keeping the calcination temperature, adding the calcined copper slag into a metal salt solution for quenching to obtain a mixed solution;
[0034] The mixed liquid is separated into solid and liquid, and the obtained solid is washed and dried to obtain the modified copper slag.
[0035] In the present invention, unless otherwise specified, the materials and equipment used are commercially available products in the art.
[0036] The invention crushes and screens the copper slag to obtain copper slag particles; and calcines the copper slag particles to obtain calcined copper slag.
[0037] In the present invention, the particle size of the copper slag particles is preferably less than 200 meshes. The present invention has no special requirements for the method of crushing and screening the copper slag, and the method commonly used by those skilled in the art can be used.
[0038] In the present invention, the copper slag is preferably collected from the bottom-blown slag of a mining enterprise in Jiangxi Province, and the copper slag preferably includes iron silicate, copper oxide and ferrosoferric oxide. After the crushing and screening, washing is preferably performed, and the washing is preferably performed with deionized water, and the number of washings is preferably 3 times, and the function of the washing is to remove soluble salts in the copper slag.
[0039] In the present invention, the calcination temperature is preferably 500-1000°C, more preferably 800°C, and the holding time is preferably 15-120 minutes, more preferably 60 minutes. The calcination temperature and time of the present invention increase the lattice oxygen in the copper slag, change the crystal form, and facilitate lattice distortion during rapid cooling (quenching).
[0040] After obtaining the calcined copper slag, the present invention maintains the calcination temperature and puts the calcined copper slag into a metal salt solution for quenching to obtain a mixed solution; the mixed solution is separated into solid and liquid, and the obtained solid is washed and dried to obtain the modified copper slag.
[0041] In the present invention, the metal salt solution preferably includes a carbonate solution, a bicarbonate solution or a nitrate solution; the metal of the metal salt solution preferably includes one or more of iron, cobalt and manganese. The metal salt in the metal salt solution preferably includes one or more of iron nitrate, cobalt nitrate and manganese nitrate, and the concentration of the metal salt solution is preferably 0.05-4 mol / L, more preferably 0.1, 0.5, 1, 2 or 3 mol / L. The concentration of the metal salt solution described in the present invention can increase the denitration duration of the modified copper slag, and further increasing the concentration of the metal salt solution cannot significantly increase the denitration duration of the modified copper slag.
[0042] In the present invention, the temperature of the metal salt solution is preferably 0-30° C., more preferably 25° C. During the quenching process, lattice distortion is caused, oxygen vacancies are generated, other metal ions are doped, and iron and the doped metal form oxides.
[0043] In the present invention, after the quenching treatment, the method preferably further comprises: repeating the calcining treatment and the quenching treatment; the calcining treatment and the quenching treatment are preferably repeated 1 to 7 times, more preferably 1 to 2 times.
[0044] In the present invention, after the last quenching treatment, the mixed liquid is separated into solid and liquid, and the obtained solid is washed and dried. The washing preferably includes deionized water washing and anhydrous ethanol washing. The number of deionized water washing and anhydrous ethanol washing is preferably 3 times. The purpose of the washing is to wash away the residual metal salt solution; the drying temperature is preferably 80-100°C, and the time is preferably 6-12h; the drying is preferably forced air drying or vacuum drying.
[0045] The present invention also provides modified copper slag obtained by the preparation method described in the above technical solution.
[0046] In the present invention, the modified copper slag is a copper slag material doped with metal ions, including metal oxides.
[0047] The present invention also provides the use of the modified copper slag described in the above technical solution in catalytic oxidation of nitrogen monoxide.
[0048] In the present invention, the catalytic oxidation of nitric oxide is preferably a Fenton reaction, and the modified copper slag can generate free radicals to oxidize nitric oxide:
[0049] Fe 2+ +H2O2→Fe 3+ +(OH) - +OH
[0050] Fe 3+ +M 2+ →Fe 2+ +M 3+
[0051] OH·+NO→HNO2
[0052] According to the present invention, after the copper slag is quenched in a metal salt solution, the surface crystallization becomes irregular, forming some distortions and some active sites and oxygen vacancies, and the material composition becomes an oxide composed of multiple metals, with more active substances and more active sites, and higher catalytic denitrification efficiency.
[0053] In order to further illustrate the present invention, the modified copper slag provided by the present invention and its preparation method and application are described in detail below in combination with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0054] Figure 1This is a flow chart of the method for preparing a denitration catalyst by quenching and doping copper slag in an embodiment of the present invention. The copper slag is crushed and screened, washed with water, calcined and kept warm, and the calcined and kept warm copper slag is quickly poured into a metal salt solution for quenching. The copper slag can be filtered and quenched again, and then washed and dried to obtain a copper slag material doped with metal ions (denitration catalyst).
[0055] In the embodiment of the present invention, the copper slag used is from the bottom-blown slag (mainly including ferrous silicate, copper oxide, and ferrosoferric oxide) of a mining enterprise in Jiangxi Province. Table 1 is the XRF data of the original copper slag. The copper slag is crushed and sieved in a crusher to obtain copper slag particles below 200 mesh, which are then washed three times with deionized water.
[0056] Table 1 XRF data of original copper slag
[0057]
[0058] Example 1
[0059] The method steps of preparing denitration catalyst by quenching and doping copper slag are as follows:
[0060] 1) Prepare 50 mL of 0.1 mol / L manganese nitrate solution: weigh 1.79 g of concentrated manganese nitrate solution (mass fraction of manganese nitrate is 50%), add deionized water to dilute to 50 mL, stir at room temperature for 10 min until the solution is completely mixed, pour into a corundum crucible and keep the solution warm at 25°C.
[0061] 2) Weigh 2 g of copper slag particles and put them into another crucible. Heat them to 500°C in a muffle furnace at a rate of 5°C per minute and keep them warm for 1 hour. Then pour them directly into the prepared solution.
[0062] The obtained mixture was washed with deionized water and anhydrous ethanol three times respectively, filtered, and dried in an oven at 100° C. for 6 hours to obtain a denitration catalyst.
[0063] Example 2
[0064] The method steps of preparing denitration catalyst by quenching and doping copper slag are as follows:
[0065] 1) Prepare 50 mL of 0.1 mol / L ferric nitrate solution: weigh 1.21 g of ferric nitrate hexahydrate, add deionized water to dilute to 50 mL, stir at room temperature for 10 min until the solution is completely mixed, pour into a corundum crucible and keep the solution warm at 25 °C.
[0066] 2) Weigh 2 g of copper slag particles and put them into another crucible. Heat them to 800°C in a muffle furnace at a rate of 5°C per minute and keep them warm for 1 hour. Then pour them directly into the prepared solution.
[0067] The calcination and quenching treatment of step 2) was repeated twice.
[0068] The obtained mixture was washed with deionized water and anhydrous ethanol three times respectively, filtered, and dried in an oven at 100° C. for 6 hours to obtain a denitration catalyst.
[0069] Example 3
[0070] The method steps of preparing denitration catalyst by quenching and doping copper slag are as follows:
[0071] 1) Prepare 50 mL of 0.1 mol / L cobalt nitrate solution: weigh 1.445 g of cobalt nitrate hexahydrate, add deionized water to dilute to 50 mL, stir at room temperature for 10 min until the solution is completely mixed, pour into a corundum crucible and keep the solution warm at 25°C.
[0072] 2) Weigh 2 g of copper slag particles and put them into another crucible. Heat them to 800°C in a muffle furnace at a rate of 5°C per minute and keep them warm for 1 hour. Then pour them directly into the prepared solution.
[0073] Repeat the calcination and quenching treatment of step 2) once.
[0074] The obtained mixture was washed with deionized water and anhydrous ethanol three times respectively, filtered, and dried in an oven at 100° C. for 6 hours to obtain a denitration catalyst.
[0075] Example 4
[0076] The difference from Example 1 is that the concentrations of the manganese nitrate solutions are 0.05 mol / L, 0.1 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, 3 mol / L and 4 mol / L, respectively; the calcination temperature is 800° C.; and the remaining steps are the same as in Example 1.
[0077] Comparative Example
[0078] The copper slag used comes from the bottom-blown slag of a mining enterprise in Jiangxi Province. The copper slag is crushed and sieved in a crusher to obtain copper slag particles below 200 mesh, which are washed three times with deionized water to obtain a copper slag catalyst.
[0079] Test Case
[0080] The denitration catalysts of Examples 1 to 3 and the copper slag catalyst of the comparative example were subjected to a Fenton denitration efficiency test as follows:
[0081] The denitration catalysts of Examples 1 to 3 and the copper slag catalyst of the comparative example were dispersed in 200 mL of a prepared H2O2 solution (2 mol / L) with a pH value of 9.5;
[0082] A nitric oxide mixed gas (NO concentration of 300ppm, O2 concentration of 10vol%, the rest of nitrogen, flow rate of 300mL / min) was continuously introduced into the above H2O2 solution, and magnetic stirring (1000r / min) was performed at 45°C. Gas collection began at the 15th minute (collection for 10 minutes), and then every half an hour. After each collection, the nitrogen oxide content was measured using a flue gas analyzer.
[0083] Figure 2 The figure is a graph of the denitration efficiency of the catalysts of Examples 1 to 3 and the comparative example, wherein Examples 1 to 3 correspond to Examples 1 to 3 respectively. The prepared Fenton iron mud catalyst exhibits good catalytic activity, and the denitration efficiency is significantly higher than that of the unmodified copper slag, and the denitration duration is significantly longer than that of the unmodified copper slag. At 75 minutes, the denitration efficiency of the modified copper slag of Examples 1 to 3 is in the range of 35 to 40%, while the denitration efficiency of the comparative copper slag is only about 15%.
[0084] Figure 3 The XRD patterns of the catalyst materials prepared in the comparative example and Examples 1 to 3 are shown in the figure. As can be seen from the figure, the corresponding metal ions are doped into the metal ions to form MFe2O4 oxides (M is the doped ions) after quenching in different metal salt solutions.
[0085] Figure 4 Graph showing the denitration efficiency of the catalyst of Example 4. At 75 minutes, the denitration efficiency of the modified copper slag of Example 4 is still within the range of 30-50%, which is significantly better than that of the copper slag of the comparative example.
[0086] Although the above-mentioned embodiments have made a detailed description of the present invention, they are only some embodiments of the present invention, rather than all embodiments. People can also obtain other embodiments based on the embodiments of the present invention without creative work, and these embodiments all fall within the scope of protection of the present invention.
Claims
1. A method for preparing modified copper slag, characterized in that: The following steps are involved: The copper slag is crushed and screened to obtain copper slag particles; calcining the copper slag particles to obtain calcined copper slag; Keeping the calcination temperature, adding the calcined copper slag into a metal salt solution for quenching to obtain a mixed solution; The mixed liquid is separated into solid and liquid, and the obtained solid is washed and dried to obtain the modified copper slag.
2. The preparation method according to claim 1, characterized in that: After the quenching treatment, the method further comprises: repeating the calcining treatment and the quenching treatment; the calcining treatment and the quenching treatment are repeated 1 to 7 times.
3. The preparation method according to claim 1, characterized in that: The particle size of the copper slag particles is less than 200 meshes.
4. The preparation method according to claim 1, characterized in that: The calcination treatment temperature is 500-1000° C., and the heat preservation time is 15-120 minutes.
5. The preparation method according to claim 1, characterized in that: The metal salt in the metal salt solution includes one or more of iron nitrate, cobalt nitrate and manganese nitrate.
6. The preparation method according to claim 5, characterized in that: The concentration of the metal salt solution is 0.05-4 mol / L.
7. The preparation method according to claim 1, 5 or 6, characterized in that: The temperature of the metal salt solution is 0-30°C.
8. The preparation method according to claim 1, characterized in that: The washing includes deionized water washing and anhydrous ethanol washing; the drying temperature is 80-100° C. and the drying time is 6-12 hours.
9. The modified copper slag obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the modified copper slag according to claim 9 in catalytic oxidation of nitrogen monoxide.
Citation Information
Cited By
Copper oxide catalyst as well as preparation method and application thereof
CN119258876A
Metal oxide nano material, surface modification method thereof and array type gas sensor
CN121800223A
Metal oxide nanomaterial, surface modification method thereof and array type gas sensor
CN121800223B