Aluminum alloy with high strength and high anode appearance and processing technology thereof
By adjusting the aluminum alloy composition and process, combined with homogenization treatment, extrusion, quenching, aging and deformation processing, the problem of balancing strength and anodizing effect of existing aluminum alloys is solved, and a high-strength and high-bright anode appearance is achieved. Aluminum alloy materials are suitable for consumer electronics such as smartphones.
Patent Information
- Application Number
- CN202410757373.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-10-08
AI Technical Summary
It is difficult to balance the strength and anodizing effect of existing aluminum alloys for smartphones. The 6 series aluminum alloy has low strength and the 7 series aluminum alloy has poor corrosion resistance, making it difficult to meet the appearance and strength requirements.
By adjusting the aluminum alloy composition, including the contents of Zn, Mg, Si, Cu, Mn, Fe, Cr, and Ti, and using homogeneous treatment, extrusion, quenching, aging and deformation processing techniques, the yield strength and anodization of the material are controlled. Effect.
The material has achieved high strength and high-brightness anode appearance. The yield strength reaches ≥460MPa and the high-brightness anode Gu value is ≥500. It is suitable for consumer electronic aluminum materials.
Smart Images

Figure BDA0004889885260000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of aluminum alloys, and in particular to an aluminum alloy with high strength and high anode appearance and a processing technology thereof. Background Art
[0002] The aluminum alloys used in existing smartphones are mainly 6-series and 7-series aluminum alloys. The 6-series aluminum alloy has a better anodizing effect, but its strength is relatively low. For example, the yield strength of 6063 aluminum alloy is about 230MPa. The yield strength of the 6013 aluminum alloy with higher strength is about 380MPa; the 7-series aluminum has high strength, but the anodizing effect is poor, especially the high-brightness anode is seriously numb and has poor corrosion resistance, and the anode is easy to fall off. With the development trend of thin and light mobile phones, the strength requirements for the mobile phone middle frame are getting higher and higher. The newly developed aluminum alloy must meet both the strength requirements and the anode appearance requirements. Due to its poor corrosion resistance, the 7-series aluminum alloy is easy to corrode the grain boundary during the high-brightness anode process, so the appearance is slightly poor and it is not corrosion-resistant. The higher-strength 6-series aluminum alloys, such as 6013 or 6056 aluminum alloys, have a yield strength of about 380MPa. To increase the strength, it is necessary to increase the degree of alloying, which will cause the material to be numb at the high-brightness anode. Therefore, it is necessary to develop a new alloy that has both higher strength (similar to 7 series aluminum alloy) and better high-brightness anode effect (similar to 6 series aluminum alloy). Summary of the invention
[0003] The purpose of the present invention is to provide a high-strength and high-anodic appearance aluminum alloy and a processing technology thereof in view of the deficiencies in the prior art.
[0004] The purpose of the present invention is achieved through the following technical solutions:
[0005] First, the present invention provides an aluminum alloy with high strength and high anode appearance, which includes, by mass percentage, Zn 0.001-1.2wt.%, Mg 0.5-1.2wt.%, Si 0.5-0.8wt.%, Cu 0.6-1.8wt.%, Mn≤0.2wt.%, Fe≤0.2wt.%, Cr≤0.2wt.%, Ti≤0.1wt.%, and the remaining components are Al and unavoidable impurities.
[0006] Secondly, the present invention provides a processing technology for high-strength and high-anodic appearance aluminum alloy, comprising the following steps:
[0007] Weigh raw materials according to the mass percentage of each element in the aluminum alloy composition, and perform smelting and casting to obtain an ingot;
[0008] Homogenizing the ingot;
[0009] Extruding the homogenized material;
[0010] Quenching the extruded material;
[0011] Perform aging treatment on the extruded material after quenching;
[0012] The extruded material after aging treatment is deformed, and the deformation amount is controlled within 5-30%.
[0013] Furthermore, the homogenizing treatment of the ingot specifically includes: heating the ingot from room temperature to 500-520°C at a heating rate of 50-100°C / h and keeping it warm for 4-8h, then heating it to 525-540°C at a heating rate of 10-30°C / h and keeping it warm for 8-12h, and then heating it to 545-570°C at a heating rate of 10-30°C / h and keeping it warm for 4-12h.
[0014] Furthermore, the extrusion of the homogenized material specifically includes: feeding the homogenized ingot into the extrusion barrel of the extruder for extrusion, with a rod temperature of 530-570° C., an extrusion material outlet temperature of 510-540° C., and an extrusion speed of 3-12 m / min.
[0015] Furthermore, the quenching of the extruded material specifically includes: the extruded aluminum alloy profile is subjected to online water mist quenching treatment at the outlet of the extrusion die, the quenching cooling rate is 40-100°C / s, the temperature of the aluminum alloy profile out of the quenching zone should be ≤180°C, and then air cooled to room temperature.
[0016] Furthermore, the aging treatment of the quenched extruded material specifically includes: placing the quenched extruded material in an aging furnace, keeping it at 175-190° C. for 6-12 hours, and then cooling it naturally.
[0017] Furthermore, the deformation treatment includes cold rolling treatment, drawing treatment or stretching treatment.
[0018] Furthermore, the cold rolling treatment specifically includes: at room temperature of 10-35°C, using a two-roll tube mill to perform a cold rolling on the extruded material after aging treatment, the feed speed of the two-roll tube mill during the cold rolling process is 15-40r / min, and cold rolling deformation is performed to the finished product thickness, and the single-pass deformation amount of the cold rolling treatment is 5-30%.
[0019] Furthermore, the stretching treatment specifically includes: passing the extruded material after aging treatment through a stretching machine within 6 hours to generate a 5-30% stretching deformation, ensuring that the straightness of the product during the drawing treatment is ≤1mm / m.
[0020] Furthermore, the drawing process specifically includes: using a drawing die with decreasing aperture, and the die working belt length is 5-10mm; drawing the extruded material after aging treatment, rolling the blank head before drawing, the rolling head length is controlled within 300mm, the drawing speed is 8-15m / min, and the single-pass drawing deformation is controlled at 5-30%.
[0021] When the main alloying elements in aluminum alloy are Mg and Si, Mg2Si phase or precursor will be formed in the system. The larger its volume fraction, the higher the strength of the material. At the same time, Mg2Si phase exists in two forms. One is the nano-level Mg2Si phase as a strengthening phase; the other is the micron or submicron level Mg2Si, which has no strengthening effect and will cause the material's bright anode to become numb, which needs to be eliminated through composition or process control. The Mg content is 0.5-1.2wt.%, and the Si content is 0.5-0.8wt.%. Within this range, the existence and volume fraction of Mg2Si can be better controlled.
[0022] The Cu element can also play a strengthening role. The Cu element is generally dissolved in the matrix to form a solid solution strengthening effect, or combined with Mg, Si, and Al elements to form a strengthening phase - Q phase. More importantly, the Cu element interacts strongly with the dislocation nucleus, which can significantly improve the work hardening ability of the material, thereby providing a basis for improving the mechanical properties of the material during subsequent cold processing. However, if the Cu content is too high, it will lead to the formation of a low melting point phase in the system or promote the formation of a coarse Mg2Si phase, which will cause the high-brightness anode to become numb. The Cu content should be 0.6-1.8wt.%.
[0023] Zn element mainly plays the role of solid solution strengthening and improving material aging kinetics, and its content is 0.001-1.2wt.%. Excessive addition of Zn will cause the corrosion resistance of the material to decrease.
[0024] The addition of Mn element is mainly used to control the grain size, and its content is preferably ≤0.2wt.%. Too much will form fibrous crystals, affecting the appearance of the high-brightness anode; Ti element is mainly used to refine the cast grains, and its content is ≤0.1wt.%. Too much will cause the black line of the anode to rise undesirably;
[0025] Fe and Cr are impurity elements in the alloy. Excessive presence will reduce the brightness of the material's high-brightness anode, but if the amount is limited, the material cost will increase significantly. Therefore, their content is ≤0.2wt.%.
[0026] The processing technology of the above aluminum alloy is to homogenize the ingots of the above composition, keep them at 500-520℃ for 4-8h, then heat them to 525-540℃ for 8-12h, and then heat them to 545-570℃ for 4-12h; the purpose of multi-stage homogenization of the material is to eliminate different types of second phases in the organization, so as to improve the mechanical properties of the material and the appearance effect of anodizing; the homogenized material is extruded at a rod temperature of 530-570℃ to ensure that the material has a high quenching temperature, and the material performance can be improved by aging later; after the extruded material is quenched, it is aged at 175-190℃ for 6-12h, so that the strengthening phase is fully and evenly precipitated, the strength of the material is improved, or the material has different work hardening capabilities; the material after aging treatment is deformed by 5-30%, including cold rolling, drawing, stretching, etc., to further improve the mechanical properties of the material, and the control of the deformation amount is mainly based on the work hardening capability of the material.
[0027] Through the above composition and process control, the yield strength of the material can be ≥460MPa, the Gu value of the high-brightness anode can be ≥500, and it has a good high-brightness anode appearance;
[0028] The present invention adjusts the content of main elements and controls the process so that the material has both high strength and high anode appearance, and is suitable for the application field of consumer electronic aluminum materials. DETAILED DESCRIPTION
[0029] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0030] Example 1
[0031] The aluminum alloy composition is calculated by mass percentage as follows: Mg 0.5wt.%, Si 0.8wt.%, Mn 0.2wt.%, Cr0.2wt.%, Cu 1.8wt.%, Ti 0.1wt.%, Fe 0.2wt.%, Zn 0.001wt.%, inevitable impurities ≤0.5wt.%, and the balance is Al;
[0032] The ingot with the above composition is homogenized, and the ingot is heated from room temperature to 500°C at a heating rate of 80°C / h and kept at this temperature for 8 hours, then heated to 540°C at a heating rate of 30°C / h and kept at this temperature for 8 hours, and then heated to 570°C at a heating rate of 30°C / h and kept at this temperature for 4 hours;
[0033] The homogenized material is extruded, the rod temperature is 570℃, the extrusion material outlet temperature is 540℃, and the extrusion speed is 12m / min;
[0034] The extruded aluminum alloy profile is subjected to online water mist quenching treatment at the exit of the extrusion die. The quenching cooling rate is 80℃ / s. The temperature of the aluminum alloy profile out of the quenching zone should be ≤180℃, and then air cooled to room temperature.
[0035] After quenching, the extruded material is subjected to aging treatment at 175°C for 12 hours;
[0036] The extruded material after aging treatment is passed through a stretching machine for 3 hours to produce a 5% tensile deformation, ensuring that the straightness of the product during the drawing process is ≤1mm / m.
[0037] Example 2
[0038] The aluminum alloy composition is calculated by mass percentage as follows: Mg 1.2wt.%, Si 0.5wt.%, Mn 0.05wt.%, Cr0.01wt.%, Cu 0.6wt.%, Ti 0.006wt.%, Fe 0.05wt.%, Zn 1.2wt%, inevitable impurities total ≤0.5wt.%, and the balance is Al;
[0039] The difference from Example 1 is that the ingot with the above composition is homogenized, kept at 520°C for 4 hours, then heated to 525°C for 12 hours, and then heated to 545°C for 12 hours; the homogenized material is extruded, the rod temperature is 530°C, the extrusion material outlet temperature is 510°C, and the extrusion speed is 3m / min; after the extrusion material is quenched, it is aged at 190°C for 6 hours; then, at room temperature of 20°C, the extrusion material after the aging treatment is cold rolled by a two-roll tube mill, the feed speed of the two-roll tube mill during the cold rolling process is 30r / min, and the cold rolling deformation is performed to the finished product thickness, and the single-pass deformation of the cold rolling treatment is 10%.
[0040] Example 3
[0041] The aluminum alloy composition is calculated by mass percentage as follows: Mg 0.9wt.%, Si 0.7wt.%, Mn 0.04wt.%, Cr0.01wt.%, Cu 1.4wt.%, Ti 0.008wt.%, Fe 0.06wt.%, Zn 0.12wt.%, inevitable impurities ≤0.5wt.%, and the balance is Al;
[0042] The difference from Example 1 is that the ingot with the above composition is homogenized, kept at 510°C for 6 hours, then heated to 535°C for 10 hours, and then heated to 560°C for 8 hours; the homogenized material is extruded, the rod temperature is 550°C, the extrusion material outlet temperature is 520°C, and the extrusion speed is 10m / min; after the extrusion material is quenched, it is aged at 185°C for 7 hours; a drawing die with decreasing aperture and a working band length of 6mm is used to draw the extruded material after aging treatment, and the billet is rolled before drawing, the rolling head length is controlled within 300mm, the drawing speed is 8m / min, and the single-pass drawing deformation is controlled at 30%.
[0043] Comparative Example 1
[0044] The aluminum alloy composition is calculated by mass percentage as follows: Mg 1.6wt.%, Si 0.4wt.%, Mn 0.5wt.%, Cr0.25wt.%, Cu 0.35wt.%, Ti 0.15wt.%, Fe 0.19wt.%, inevitable impurities ≤0.5wt.%, and the balance is Al;
[0045] The processing technology of the aluminum alloy in Comparative Example 1 is consistent with that in Example 1.
[0046] Comparative Example 2
[0047] The composition of the aluminum alloy in Comparative Example 2 is consistent with that in Example 1.
[0048] The processing technology of the aluminum alloy in Comparative Example 2 is different from that in Example 1 in that: the ingot with the above composition is homogenized and kept at 540°C for 12 hours, the homogenized material is extruded with a rod temperature of 570°C; after the extruded material is quenched, it is aged at 175°C for 8 hours.
[0049] Table 1 shows the properties and microstructure characteristics of the aluminum alloys in the embodiments and comparative examples.
[0050] Table 1
[0051]
[0052] As shown in Table 1, the present invention reasonably adjusts the content of each element in the aluminum alloy and the processing technology, so that the obtained aluminum alloy material has high strength and high anodizing effect, which is suitable for the large-scale production of consumer electronic aluminum materials.
[0053] According to the disclosure of the above description, those skilled in the art to which the present invention belongs may also make appropriate changes and modifications to the above embodiments. Therefore, the present invention is not limited to the specific embodiments disclosed and described above, and some modifications and changes to the present invention should also fall within the scope of protection of the claims of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A high-strength and high-anodic appearance aluminum alloy, characterized in that: Calculated by mass percentage, it includes: Zn 0.001-1.2wt.%, Mg 0.5-1.2wt.%, Si 0.5-0.8wt.%, Cu 0.6-1.8wt.%, Mn≤0.2wt.%, Fe≤0.2wt.%, Cr≤0.2wt.%, Ti≤0.1wt.%, and the remaining components are Al and inevitable impurities.
2. A processing technology for the high-strength and high-anodic appearance aluminum alloy according to claim 1, characterized in that: The steps include: Weigh raw materials according to the mass percentage of each element in the aluminum alloy composition, and perform smelting and casting to obtain an ingot; Homogenizing the ingot; Extruding the homogenized material; Quenching the extruded material; Perform aging treatment on the extruded material after quenching; The extruded material after aging treatment is deformed, and the deformation amount is controlled within 5-30%.
3. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 2 is characterized in that: The homogenizing treatment of the ingot specifically includes: heating the ingot from room temperature to 500-520°C at a heating rate of 50-100°C / h and keeping it warm for 4-8h, then heating it to 525-540°C at a heating rate of 10-30°C / h and keeping it warm for 8-12h, and then heating it to 545-570°C at a heating rate of 10-30°C / h and keeping it warm for 4-12h.
4. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 2 is characterized in that: The extrusion of the homogenized material specifically includes: sending the homogenized ingot into the extrusion barrel of the extruder for extrusion, the rod temperature is 530-570° C., the extrusion material outlet temperature is 510-540° C., and the extrusion speed is 3-12 m / min.
5. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 2 is characterized in that: The quenching of the extruded material specifically includes: the extruded aluminum alloy profile is subjected to online water mist quenching treatment at the outlet of the extrusion die, the quenching cooling rate is 40-100°C / s, the temperature of the aluminum alloy profile out of the quenching zone should be ≤180°C, and then air cooled to room temperature.
6. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 2 is characterized in that: The aging treatment of the quenched extruded material specifically includes: placing the quenched extruded material in an aging furnace, keeping it at 175-190° C. for 6-12 hours, and then cooling it naturally.
7. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 2 is characterized in that: The deformation process includes cold rolling, drawing or stretching.
8. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 7 is characterized in that: The cold rolling treatment specifically includes: at room temperature of 10-35°C, using a two-roll tube mill to perform a cold rolling on the extruded material after aging treatment, the feed speed of the two-roll tube mill during the cold rolling process is 15-40r / min, and cold rolling is performed to deform the extruded material to the finished product thickness, and the deformation amount of a single cold rolling process is 5-30%.
9. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 7 is characterized in that: The stretching treatment specifically includes: passing the extruded material after aging treatment through a stretching machine within 6 hours to generate a 5-30% stretching deformation, ensuring that the straightness of the product during the drawing treatment is ≤1mm / m.
10. The processing technology of the high-strength and high-anodic appearance aluminum alloy according to claim 7, characterized in that: The drawing process specifically includes: using a drawing die with decreasing aperture, the die working belt length is 5-10mm, drawing the extruded material after aging treatment, rolling the blank head before drawing, the rolling head length is controlled within 300mm, the drawing speed is 8-15m / min, and the single-pass drawing deformation is controlled within 5-30%.
Citation Information
Cited By
Heat exchanger and processing method therefor
WO2026145310A1