Preparation method and application of metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for hydrogen production through water electrolysis

By preparing metal ruthenium-doped nickel-molybdenum nitride nanorod catalysts, the problem of high hydrogen evolution overpotential of non-noble metal catalysts in water electrolysis for hydrogen production has been solved, and a low-cost and efficient electrochemical reaction has been achieved, which is suitable for water electrolysis and sewage treatment. .

CN118745581APending Publication Date: 2024-10-08衢州市浙工大生态工业创新研究院
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410732951.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing non-precious metal catalysts have problems such as high hydrogen evolution overpotential and low power utilization efficiency in the electrolysis of water for hydrogen production, making it difficult to increase hydrogen production in alkaline electrolytes.

Method used

Using metal ruthenium doped nickel molybdenum nitride nanorod catalyst, by dissolving nickel salt and molybdenum salt in deionized water-ethylene glycol mixed solvent, preparing a salt solution, and preparing nickel molybdenum oxide through ultrasound and hydrothermal reaction. It is then roasted to obtain nickel-molybdenum nitride, and finally doped with ruthenium metal to form a catalyst with a nanorod structure.

Benefits of technology

It achieves low hydrogen evolution overpotential, improves the electrochemical reaction activity and chemical stability of the catalyst, reduces costs, increases the specific surface area, improves charge transport and proton diffusion efficiency, and is suitable for hydrogen production by electrolysis of water, sewage treatment and scale Industrial water electrolysis process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745581A_ABST
    Figure CN118745581A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for hydrogen production through water electrolysis, and the preparation method of the catalyst comprises the following steps: taking nickel salt and molybdenum salt as raw materials, taking ethylene glycol and water as solvents, adding a flaky carrier substrate, and preparing a nickel-molybdenum oxide precursor catalyst by adopting a hydrothermal method; the preparation method comprises the following steps: preparing a nickel-molybdenum nitride nanorod electrocatalyst, roasting the nickel-molybdenum nitride nanorod electrocatalyst in mixed gas of NH3 and N2 to obtain the nickel-molybdenum nitride nanorod electrocatalyst, and roasting the nickel-molybdenum nitride nanorod electrocatalyst and ruthenium salt in a tubular furnace to obtain the metal ruthenium doped nickel-molybdenum nitride nanorod catalyst. The catalyst is used for water electrolysis hydrogen production reaction, and in a 1 M Na2CO3 solution, the overpotential reaching 10 mA / cm < 2 > current density is only 43 mV. The preparation process of the catalyst is green and economical, the reaction process is simple and easy to operate, the catalyst cost is low, and the overpotential of the hydrogen evolution reaction is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material chemistry and electrocatalysis technology, and in particular to a metal ruthenium-doped nickel-molybdenum nitride material used for electrolysis of water to produce hydrogen, a preparation method thereof, and an application thereof as a catalyst for electrocatalytic hydrogen production. Background Art

[0002] Hydrogen (H2) is a renewable and environmentally friendly energy source that is expected to replace traditional fossil fuels. At present, industrial hydrogen production uses a large amount of fossil energy, which not only violates the concept of environmentally friendly development, but also causes serious pollution to the environment. In contrast, among various hydrogen production technologies, water electrolysis is regarded as an effective way to produce high-purity (>99.9%) hydrogen. In order to improve the efficiency of hydrogen production by water electrolysis, people usually use precious metals such as palladium (Pd) and platinum (Pt) to prepare catalysts. Since precious metals are scarce in the earth's crust and are expensive, the industry hopes to use low-cost materials to replace precious metal catalysts. However, non-precious metal catalysts have the problems of high hydrogen evolution overpotential and low electrical energy utilization efficiency in the application of water electrolysis to produce hydrogen. Therefore, it is of great significance to develop efficient catalysts that can accelerate electron transfer and reduce reaction energy barriers.

[0003] In recent years, many non-precious metal catalysts have been reported to be used for hydrogen production by water electrolysis, including transition metal compounds and their alloys, and these materials have been shown to have excellent hydrogen evolution performance. NiMo metal materials exhibit similar adjustable electronic state characteristics to Pt. In an alkaline environment, this material exhibits excellent HER kinetics and is therefore considered an ideal substitute for Pt. Although there have been a large number of related studies, there are still certain challenges in achieving increased hydrogen production in alkaline electrolytes. Summary of the invention

[0004] The purpose of the present invention is to address the above-mentioned problems existing in the prior art and to provide a method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water and its application. The process for preparing the catalyst is green and economical, the reaction process is simple and easy to operate, the catalyst cost is low, and the overpotential of the hydrogen evolution reaction is low.

[0005] The technical solution adopted by the present invention is as follows:

[0006] A method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolyzing water comprises the following steps:

[0007] 1) dissolving nickel salt and molybdenum salt in a deionized water-ethylene glycol mixed solvent to prepare a salt solution for standby use;

[0008] 2) adding a sheet-shaped carrier substrate to the salt solution of step 1), and subjecting the substrate to ultrasonic treatment at room temperature to fully contact the substrate with the solution; then pouring the substrate and the solution into a reaction kettle, sealing the reaction kettle, and completely immersing the substrate in the salt solution for a hydrothermal reaction;

[0009] 3) After the reaction is completed, the substrate is naturally cooled, taken out, rinsed, and dried to obtain a nickel-molybdenum oxide electrocatalyst;

[0010] 4) placing the nickel-molybdenum oxide electrocatalyst in a tubular furnace, introducing a mixed gas of N2 and NH3 for calcination, thereby obtaining a nickel-molybdenum nitride electrocatalyst;

[0011] 5) placing the nickel-molybdenum-nitride electrocatalyst downstream of the tubular furnace, placing an excess of Ru precursor upstream of the tubular furnace, introducing argon gas for calcination, so that Ru is volatilized during the calcination process and doped on the nickel-molybdenum-nitride electrocatalyst, and obtaining a metal ruthenium-doped nickel-molybdenum-nitride nanorod catalyst.

[0012] Furthermore, in step 1), the nickel salt is at least one of nickel nitrate, nickel chloride, nickel acetylacetonate or nickel acetate, and the molybdenum salt is at least one of phosphomolybdic acid, sodium molybdate and ammonium molybdate; and the carrier is one of nickel foam, carbon felt and carbon cloth.

[0013] Further, in step 1), the molar ratio of nickel salt to molybdenum salt is 0.5-2:1, preferably 1-1.2:1; in step 2), the size area of ​​the sheet carrier substrate is 1 cm 2 The total molar amount of the nickel salt and the molybdenum salt in step 1) is 0.5-2 mmol, preferably 1-1.2 mmol.

[0014] Furthermore, in step 1), the volume ratio of deionized water to ethylene glycol is 0.3-1.0:1, preferably 0.5-0.6:1, and the concentration of nickel salt in the deionized water-ethylene glycol mixed solvent is 0.01-0.05 mmol / mL, preferably 0.02-0.04 mmol / mL.

[0015] Furthermore, in step 2), the temperature of the hydrothermal reaction is 120-160° C., preferably 130-140° C., and the reaction time is 8-15 h, preferably 10-12 h.

[0016] Furthermore, in step 4), in the mixed gas of N2 and NH3, the volume fraction of NH3 is 20-60%, preferably 40-50%.

[0017] Furthermore, in step 4), the calcination temperature is 400-450° C., and the calcination time is 2-2.5 h.

[0018] Furthermore, in step 5), the calcination temperature is 300-350° C., and the calcination time is 1-2 h, preferably 2 h.

[0019] The present invention also provides application of the catalyst in a water electrolysis hydrogen production reaction.

[0020] The beneficial effects of the present invention are as follows:

[0021] The invention provides a method for preparing a metal ruthenium-doped nickel-molybdenum-nitride nanorod catalyst for producing hydrogen by electrolysis of water, wherein the electrode material prepared by the method has good catalytic activity, electrical conductivity, and chemical stability: the metal ruthenium-doped nickel-molybdenum-nitride catalyst material has a simple process of combining with a carrier material, a strong combination, and a long service life, and can meet the requirements of green energy conservation and environmental protection. Moreover, the metal ruthenium-doped nickel-molybdenum-nitride is a nanorod structure, which can effectively increase the specific surface area of ​​the catalyst material and accelerate charge transfer and proton diffusion, thereby improving the electrochemical reaction activity of the catalyst. Therefore, the metal ruthenium-doped nickel-molybdenum-nitride electrode used for producing hydrogen by electrolysis of water of the present invention and the preparation method thereof have broad application prospects in hydrogen evolution industry, sewage treatment, and large-scale industrial water electrolysis processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM image of NiMoO4 / NF in step (4) of Example 1.

[0023] Figure 2 This is the SEM image of Ru-NiMoN / NF in step (6) of Example 1.

[0024] Figure 3 LSV curves of NiMoO4 / NF, NiMoN / NF of Example 1 and Ru-NiMoN / NF of Example 4.

[0025] Figure 4 ECSA curves of NiMoO4 / NF, NiMoN / NF of Example 1 and Ru-NiMoN / NF of Example 4.

[0026] Figure 5 The Ru-NiMoN / NF catalyst of Example 4 is at 10 mA / cm 2 Time diagram of stable operation under current density. DETAILED DESCRIPTION

[0027] The present invention will now be further described in detail with reference to the embodiments. The application of the present invention is not limited to the following embodiments, and any modifications made to the present invention will fall within the protection scope of the present invention.

[0028] Example 1 Synthesis of Ru-NiMoN / NF catalyst and its application in water electrolysis to produce hydrogen

[0029] (1) Add 1.8 mmol nickel nitrate and 1.7 mmol ammonium molybdate into 30 mL deionized water and dissolve them by ultrasonication;

[0030] (2) Add 50 mL of ethylene glycol and mix thoroughly by ultrasonication at room temperature for 20 min;

[0031] (3) Add nickel foam (NF) (size 3×3 cm) to the solution. 2 ), ultrasonically treat at room temperature for 10 min to allow the NF to fully contact the solution; pour the solution and NF into the inner lining of the reactor, immerse the carrier NF completely in the salt solution, seal the reactor, and hydroheat at 140°C for 12 h;

[0032] (4) After the reaction is completed, the NF is naturally cooled, and the NF is taken out and rinsed with deionized water and ethanol in sequence, and then placed in a vacuum drying oven at 60° C. for 12 h to obtain a NiMoO4 / NF electrocatalyst;

[0033] (5) The prepared NiMoO4 / NF catalyst was placed in a tubular furnace, introduced with a mixed gas of 80% N2+20% NH3, and calcined at 450°C for 2h to obtain a NiMoN / NF electrocatalyst.

[0034] (6) The above-mentioned NiMoN / NF electrocatalyst and 0.5 mmol of ruthenium acetylacetonate were placed in a tubular furnace respectively. The ruthenium acetylacetonate was placed in a porcelain boat and placed upstream of the tubular furnace. The nickel-molybdenum nitride electrocatalyst was placed downstream of the tubular furnace. Argon gas was introduced and the mixture was calcined at 300°C for 1 hour. After the calcination, the Ru-NiMoN / NF electrocatalyst was obtained.

[0035] (7) The prepared Ru-NiMoN / NF electrocatalyst was used as the working electrode, the platinum sheet as the counter electrode, and the Ag / AgCl as the reference electrode to test the hydrogen evolution performance of water electrolysis in 1M Na2CO3 aqueous solution. The specific method is as follows:

[0036] The above examples were tested at room temperature using a CHI760E electrochemical workstation for the Ru-NiMoN / NF catalytic electrode material. The electrolytic cell was a standard three-electrode system, with the Ru-NiMoN / NF electrocatalyst as the working electrode, the platinum sheet as the counter electrode, the Ag / AgCl as the reference electrode, and the electrolyte as a 1M Na2CO3 solution. The scan rate for all linear sweep voltammograms (LSV) was 5mV / s, and the potential scan range was -0.8V-0V vs.RHE. Test 10mA / cm 2 The potential of Ru-NiMoN / NF electrode material at a current density of 2.5447 W was used to determine its HER performance.

[0037] The catalyst morphology was investigated by SEM characterization. The SEM image of NiMoO4 / NF in step (4) of Example 1 is as follows: Figure 1 As shown, the SEM image of Ru-NiMoN / NF in step (6) is as follows Figure 2 As shown. Figure 1 It can be seen that the precursor catalyst NiMoO4 is uniformly loaded on the nickel foam substrate. Figure 2 As shown, Ru-NiMoN / NF becomes a nanorod structure, which can expose a large number of active sites, thereby increasing the effective contact between the catalyst and the electrolyte in the electrochemical reaction.

[0038] Example 2: Synthesis of Ru-NiMoN / NF catalyst and its application in water electrolysis to produce hydrogen

[0039] The synthesis steps of the Ru-NiMoN / NF catalyst in Example 2 were repeated as in Example 1, with the only difference being that "the calcination temperature in step (6) was replaced with 350° C.", and the other conditions remained unchanged.

[0040] Example 3: Synthesis of Ru-NiMoN / NF catalyst and its application in water electrolysis to produce hydrogen

[0041] The synthesis steps of the Ru-NiMoN / NF catalyst in Example 3 are repeated in Example 2, except that "the amount of deionized water used in step (1) is 80 mL, and the step of adding ethylene glycol is omitted in step (2)," and the other conditions remain unchanged.

[0042] Example 4: Synthesis of Ru-NiMoN / NF catalyst and its application in water electrolysis to produce hydrogen

[0043] The synthesis steps of the Ru-NiMoN / NF catalyst in Example 4 were repeated in Example 2, except that the calcination time at 350° C. in step (6) was replaced with 1.5 h, and the other conditions remained unchanged.

[0044] Example 5: Synthesis of Ru-NiMoN / NF catalyst and its application in water electrolysis to produce hydrogen

[0045] The synthesis steps of the Ru-NiMoN / NF catalyst in Example 5 were repeated in Example 2, with the only difference being that the calcination time at 350° C. in step (6) was replaced with 2 h, and the other conditions remained unchanged.

[0046] Example 6: Synthesis of Ru-NiMoN / NF catalyst and its application in water electrolysis to produce hydrogen

[0047] The synthesis steps of Ru-NiMoN / NF catalyst in Example 6 are repeated as in Example 5, with the only difference being that "the gas introduced in step (5) is replaced by a 50% N2+50% NH3 mixed gas", and the other conditions remain unchanged.

[0048] Comparative Example 1: Synthesis of Ru-NiMoN / NF (hydrothermal preparation) catalyst and its application in water electrolysis to produce hydrogen

[0049] The synthesis steps of the Ru-NiMoN / NF catalyst in Control Example 1 were repeated as in Example 1, except that "2 mmol urea was also added in step (1), and the gas introduced in step (6) was replaced by N2", and the other conditions remained unchanged.

[0050] The Ru-NiMoN / NF electrocatalysts prepared in Examples 2-6 and Comparative Example 1 were used as working electrodes for testing, and the testing steps were repeated in Example 1. Test 10 mA / cm 2 The potential of Ru-NiMoN / NF electrode materials prepared under different conditions at a current density of , and the results are shown in Table 1. The HER performance is compared through the data in Table 1.

[0051] Table 1: Test results of hydrogen evolution reaction of Ru-NiMoN / NF catalysts prepared under different conditions

[0052]

[0053] By comparing Example 2 and Example 3, it can be found that the addition of ethylene glycol during hydrothermal treatment improves the hydrogen evolution performance of the catalyst. The catalysts of Examples 2 and 3 are weighed, and it is found that the weight of the catalyst of Example 2 is greater than the weight of the catalyst of Example 3, so ethylene glycol may increase the adhesion of the catalyst on the foam nickel substrate. By comparing Example 5 with the control experiment, it is found that the catalyst prepared by roasting method using NH3 as a nitrogen source has a lower hydrogen evolution overpotential, indicating that roasting is beneficial to improving the activity of the catalyst. And by screening the experimental conditions, it is concluded that when roasting with NH3+N2, the gas ratio is 80% N2+20% NH3 and when roasting with ruthenium acetylacetonate, the optimal roasting temperature is 350°C, and the time is 2h, and the obtained hydrogen evolution catalyst has the best effect.

[0054] In order to highlight the improvement of Ru doping on the performance of hydrogen evolution in water electrolysis, the performance of hydrogen evolution in water electrolysis was tested in 1M Na2CO3 solution. The NiMoO4 / NF and NiMoN / NF materials prepared in Example 1 and the Ru-NiMoN / NF catalytic electrode materials prepared in Example 4 were tested at room temperature using a CHI760E electrochemical workstation. The electrolytic cell was a standard three-electrode system, with NiMoO4 / NF, NiMoN / NF and Ru-NiMoN / NF electrocatalysts as working electrodes, platinum as the counter electrode, Ag / AgCl as the reference electrode, and the electrolyte was 1M Na2CO3 solution. The scan rate of all linear sweep voltammograms (LSV) was 5mV·s -1 The potential scanning range is -0.8V-0.1V vs. RHE. The LSV curves of NiMoO4 / NF, NiMoN / NF and Ru-NiMoN / NF materials are shown in Figure 3 The electrochemically active surface area (ECSA) was tested in the voltage range of 0.12 V to 0.28 V vs. RHE at scan rates of 20, 40, 60, 80, 100, and 120 mV s -1 , the ECSA curve is as follows Figure 4 shown.

[0055] In by Figure 3 From the LSV curve, it can be seen that at a current density of 10 mA / cm 2 When the overpotential of NiMoO4 / NF, NiMoN / NF and Ru-NiMoN reaches 159, 114 and 43 mV respectively, Figure 4 It shows that Ru-NiMoN / NF has the largest electrochemical active surface area and has good electrocatalytic performance, indicating that Ru-NiMoN / NF has more active sites, which is beneficial to the electrocatalytic hydrogen evolution reaction.

[0056] In order to further verify the stability of the catalyst, the Ru-NiMoN / NF catalytic electrode material prepared in Example 4 was tested at 10 mA / cm -2 The time for stable operation under the current density of Figure 5 It can be seen that the catalyst can be -2 The continuous and stable hydrogen production can last up to 100 hours at the current density.

[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water, characterized in that The following steps are involved: 1) Dissolve nickel salt and molybdenum salt in a deionized water-ethylene glycol mixed solvent to prepare a salt solution for later use; 2) adding a sheet-shaped carrier substrate to the salt solution of step 1), and subjecting the substrate to ultrasonic treatment at room temperature to allow the substrate and the solution to be in full contact; then pouring the substrate and the solution into a reaction kettle, sealing the reaction kettle, and completely immersing the substrate in the salt solution for a hydrothermal reaction; 3) After the reaction is completed, the substrate is naturally cooled, taken out, rinsed, and dried to obtain a nickel-molybdenum oxide electrocatalyst; 4) placing the nickel-molybdenum oxide electrocatalyst in a tubular furnace, introducing a mixed gas of N2 and NH3 for calcination, thereby obtaining a nickel-molybdenum nitride electrocatalyst; 5) Placing the nickel-molybdenum nitride electrocatalyst downstream of the tubular furnace and the Ru precursor upstream of the tubular furnace, introducing argon gas for calcination, so that Ru is volatilized during the calcination process and doped into the nickel-molybdenum nitride electrocatalyst to obtain a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst.

2. The method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water as claimed in claim 1, characterized in that In step 1), the nickel salt is at least one of nickel nitrate, nickel chloride, nickel acetylacetonate or nickel acetate, and the molybdenum salt is at least one of phosphomolybdic acid, sodium molybdate and ammonium molybdate; and the carrier is one of nickel foam, carbon felt and carbon cloth.

3. The method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water as claimed in claim 1, characterized in that In step 1), the molar ratio of nickel salt to molybdenum salt is 0.5-2:1, preferably 1-1.2:1; In step 2) the size of the sheet carrier substrate is 1 cm 2 In step 1), the total molar amount of the nickel salt and the molybdenum salt is 0.5-2 mmol, preferably 1-1.2 mmol.

4. The method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water as claimed in claim 1, characterized in that In step 1), the volume ratio of deionized water to ethylene glycol is 0.3-1.0:1, preferably 0.5-0.6:1, and the concentration of nickel salt in the deionized water-ethylene glycol mixed solvent is 0.01-0.05 mmol / mL, preferably 0.02-0.04 mmol / mL.

5. The method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water as claimed in claim 1, characterized in that In step 2), the temperature of the hydrothermal reaction is 120-160° C., preferably 130-140° C., and the reaction time is 8-15 h, preferably 10-12 h.

6. The method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water as claimed in claim 1, characterized in that In step 4), in the mixed gas of N2 and NH3, the volume fraction of NH3 is 20-60%, preferably 40-50%.

7. The method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water as claimed in claim 1, characterized in that In step 4), the calcination temperature is 400-450°C and the calcination time is 2-2.5 h.

8. The method for preparing a metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water as claimed in claim 1, characterized in that In step 5), the calcination temperature is 300-350 ºC, and the calcination time is 1-2 h, preferably 2 h.

9. A metal ruthenium-doped nickel-molybdenum nitride nanorod catalyst for producing hydrogen by electrolysis of water, prepared according to the method of any one of claims 1 to 8.

10. Use of the catalyst as claimed in claim 9 in a hydrogen production reaction by electrolysis of water.

Citation Information

Cited By

  • Preparation method of non-noble metal doped nickel-molybdenum-nitrogen-carbon multi-element hydrogen evolution catalyst

    CN120060907A

  • Preparation method of manganese-doped nickel molybdate material and application of manganese-doped nickel molybdate material in preparation of nitrate through electro-catalytic ammoxidation

    CN120250059A

  • Lanthanum oxide doped molybdenum-based supported catalyst as well as preparation method and application thereof

    CN121228286A