Preparation method and application of ultralow-iridium-content catalyst for PEM membrane electrode

By using a cerium salt and chloroiridic acid solution for thermal reaction in a PEM hydrolysis tank to prepare an ultra-low iridium content catalyst, the problem of limited selection of catalyst materials in a protonated strong acid environment is solved, and high oxygen evolution reaction activity and stability are achieved. It reduces the usage of Ir and promotes the large-scale development of PEM technology.

CN118745582APending Publication Date: 2024-10-08YANGZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410862910.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The protonated strong acid environment of the existing PEM hydrolysis tank limits the selection of membrane electrode catalyst materials, resulting in high loading of Ir and Pt, increasing costs and hindering the large-scale development of PEM technology.

Method used

The ultra-low iridium content catalyst is prepared through the thermal reaction of cerium salt and chloroiridic acid solution to form IrOx cluster-doped cerium oxide powder. The structure is ultra-fine IrOx clusters with a particle size of <5nm anchored in the CeO2 lattice. Reduce the amount of Ir and improve catalytic performance.

Benefits of technology

It achieves high oxygen evolution reaction activity and stability of low Ir content catalysts, reduces the usage of Ir, has low cost, simple process, and is suitable for large-scale production. The membrane loading capacity is much smaller than that of commercial membrane electrodes, which promotes the cost reduction of PEM components. Increase efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745582A_ABST
    Figure CN118745582A_ABST
Patent Text Reader

Abstract

The invention discloses a catalyst with ultralow Ir content for a PEM membrane electrode as well as a preparation method and application of the catalyst. The catalyst with the ultralow Ir content is high in oxygen evolution reaction activity and good in stability, the performance of the catalyst is remarkably superior to that of a commercial IrO2 catalyst, the raw material cost is low, the process is simple, time and energy are saved, pollution is avoided, and large-scale production can be achieved. According to the preparation method of the ultralow-iridium-content catalyst for the PEM membrane electrode, the dosage of precious metal Ir is reduced, the catalytic performance is improved, Ir-based catalyst product iteration is expected to be achieved, and cost reduction and efficiency improvement of a PEM assembly are promoted.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalytic materials, and specifically relates to a preparation method and application of an ultra-low iridium content catalyst for a PEM membrane electrode. Background Art

[0002] At present, hydrogen has attracted widespread attention as an ideal new energy carrier that is expected to replace fossil fuels. Water electrolysis hydrogen production technology has also attracted attention. Proton exchange membrane (PEM) water electrolysis hydrogen production technology has the advantages of high operating current density, compact structure, low energy consumption, high efficiency, and high gas purity. It is an ideal large-scale green hydrogen production technology. In particular, PEM electrolyzers have fast response speeds, wide load ranges, and can flexibly match fluctuating inputs. They are unique in coupling with renewable power systems such as photovoltaics and wind turbines.

[0003] However, the protonated strong acid environment (pH ~ 2) of the PEM hydrolyzer limits the choice of membrane electrode catalyst materials. Currently, only precious metal-based IrO2 and Pt can serve as anode and cathode catalysts, respectively, with Ir and Pt loadings as high as 2-5 mg / cm 2 and 1-3 mg / cm 2 , accounting for ~16% of the total PEM system cost, is an important factor hindering the cost reduction and efficiency improvement of PEM equipment. In particular, Ir resources are extremely scarce and expensive, which greatly restricts the large-scale development of the PEM industry. Developing high-performance catalysts with low Ir content is a key task in the development of PEM technology. Summary of the invention

[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0005] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0006] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a catalyst with ultra-low iridium content for PEM membrane electrodes.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0008] The cerium salt and the chloroiridic acid solution are mixed to obtain a raw material mixed solution;

[0009] The raw material mixture undergoes a thermal reaction;

[0010] After naturally cooling to room temperature, the powder sample was taken out, and after washing and drying, an ultra-low iridium content catalyst for PEM membrane electrode was obtained.

[0011] As a preferred solution of the method for preparing the ultra-low iridium content catalyst for PEM membrane electrode of the present invention, the cerium salt is one of Ce(NO3)3·6H2O or CeCl3·6H2O.

[0012] As a preferred solution of the method for preparing the ultra-low iridium content catalyst for PEM membrane electrode of the present invention, the concentration of chloroiridic acid in the raw material mixed solution is 0-0.16 mol / L.

[0013] As a preferred solution of the method for preparing the ultra-low iridium content catalyst for PEM membrane electrode of the present invention, the concentration of chloroiridic acid in the raw material mixed solution is 0.08-0.16 mol / L.

[0014] As a preferred embodiment of the method for preparing the ultra-low iridium content catalyst for PEM membrane electrode of the present invention, wherein: Ce in the raw material mixture is 3+ The molar ratio of iridium chloride to chloroiridic acid is 1:0 to 0.16.

[0015] As a preferred solution of the method for preparing the ultra-low iridium content catalyst for PEM membrane electrode of the present invention, the thermal reaction temperature is 200-250°C.

[0016] As a preferred solution of the method for preparing the ultra-low iridium content catalyst for PEM membrane electrode of the present invention, the thermal reaction time is 3 to 7 hours.

[0017] Another object of the present invention is to overcome the deficiencies in the prior art and provide a PEM membrane electrode ultra-low iridium content catalyst prepared by the preparation method. x Cluster-doped cerium oxide powder, the structure is ultrafine IrO with particle size less than 5nm x The clusters are anchored in the CeO2 lattice, where IrO x Iridium oxide.

[0018] As a preferred embodiment of the ultra-low iridium content catalyst for PEM membrane electrode of the present invention, the mass proportion of Ir in the ultra-low iridium content catalyst for PEM membrane electrode is 2-7 wt.%.

[0019] Another object of the present invention is to overcome the shortcomings of the prior art and provide an application of the ultra-low iridium content catalyst for PEM membrane electrode, characterized in that the ultra-low iridium content catalyst powder for PEM membrane electrode is added to a solvent with a volume ratio of isopropanol, pure water and Nafion adhesive of 1:1:0.02-0.03 at a mass ratio of 1-5%, and the slurry is sprayed on the proton membrane, and after hot pressing, it is used as an anode for hydrogen production in a proton exchange membrane water electrolyzer.

[0020] Beneficial effects of the present invention:

[0021] (1) The low Ir content catalyst of the present invention has high oxygen evolution reaction activity and good stability, and its performance is significantly superior to that of commercial IrO2 catalysts.

[0022] (2) The low Ir content catalyst of the present invention has low raw material cost, simple process, time-saving and energy-saving, no pollution, and can be produced on a large scale. In addition, the mass proportion of Ir is only 4wt.%, and the estimated membrane loading (based on the membrane-loaded catalyst amount of 10mg / cm 2 Calculation) is only 0.4mg / cm 2 , which is much smaller than the 2-5 mg / cm in current commercial membrane electrodes. 2 of Ir loading.

[0023] (3) The preparation method of the ultra-low iridium content catalyst for PEM membrane electrode in the present invention not only reduces the amount of precious metal Ir used, but also improves the catalytic performance, which is expected to achieve the iteration of Ir-based catalyst products and promote the cost reduction and efficiency improvement of PEM components. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0025] Figure 1 This is a schematic diagram of the preparation of the catalyst in Example 1 of the present invention.

[0026] Figure 2 This is a scanning electron microscope photograph of the catalyst in Example 1 of the present invention.

[0027] Figure 3 The energy dispersive spectrum and element content of the catalyst in Example 1 of the present invention.

[0028] Figure 4 This is the X-ray diffraction spectrum of the catalyst in Example 1 of the present invention.

[0029] Figure 5This is a spherical aberration corrected transmission electron microscope photograph of the catalyst in Example 1 of the present invention.

[0030] Figure 6 This is a polarization curve diagram of the deposition oxygen evolution reaction of catalysts with different Ir contents in Example 2 of the present invention.

[0031] Figure 7 It is the polarization curve of the deposition oxygen evolution reaction of the low Ir content catalyst in Comparative Example 1 of the present invention, the commercial IrO2 catalyst and the CeO2 substrate.

[0032] Figure 8 It is a chronopotentiometric curve diagram of the low Ir content catalyst and the commercial IrO2 catalyst in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0033] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0034] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0035] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0036] Unless otherwise specified, the raw materials used in the present invention are all commercially available in the art.

[0037] The commercial catalyst in the present invention was purchased from Anhui Masu Shui New Energy Technology Co., Ltd., which is IrO2 powder with an Ir content of >84.0wt.% and a membrane loading of 1.0mg. Ir / cm 2 .

[0038] The determination method for determining the catalytic activity of the material in the present invention is a three-electrode linear voltammetric scanning method, and the determination conditions are: at room temperature of 25°C, the electrolyte is a 0.5M H2SO4 solution, the reference electrode is silver / silver chloride, the counter electrode is a carbon rod, and the working electrode is the ultra-low iridium content catalyst prepared in the present invention. 4.8 mg of the low Ir content catalyst and 1.2 mg of acetylene black are weighed, dissolved in 300 μL of alcohol, 30 μL of naphthol solution and 300 μL of deionized water, and ultrasonically dissolved for 20 minutes to obtain a mixed solution. Take 3 μL of the mixed solution and drop it on the glassy carbon electrode, and dry it for 7 hours to obtain the working electrode.

[0039] The catalytic stability determination method in the present invention is: constant current chronopotentiometry.

[0040] Example 1

[0041] This embodiment provides a method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode. The catalyst preparation process is as follows: Figure 1 Specifically:

[0042] Weigh 200 mg Ce(NO3)3·6H2O and 10 μL 2 g / mL H2IrCl6·6H2O and dissolve them in 460 μL deionized water. Ultrasonicate for 10 minutes to fully dissolve the mixture to obtain a raw material mixture. 3+ The concentration of Ce in the raw material mixture is 1 mol / L, the concentration of H2IrCl6·6H2O is 0.08 mol / L, and the concentration of Ce in the raw material mixture is 1 mol / L. 3+ The molar ratio with H2IrCl6·6H2O is 1:0.08;

[0043] Pour the raw material mixture into the crucible, place the crucible in a muffle furnace and heat it to 220°C, and continue the thermal reaction for 5 hours;

[0044] After naturally cooling to room temperature, the powder sample in the crucible is taken out, and after washing and drying, an ultra-low iridium content catalyst for PEM membrane electrode is obtained.

[0045] The thermal preparation method is very simple and does not require stringent requirements such as high pressure, vacuum, and atmosphere. It can be easily mass-produced, and the manufacturing equipment is simple and the process cost is low.

[0046] Figure 2 This is a scanning electron microscope (SEM) image of the material. The prepared catalyst has a nanoparticle morphology. Figure 3 The energy dispersive spectrum (EDS) of the material and its elemental mapping diagram indicate that the catalyst contains Ce, Ir, and O elements, and each element is evenly distributed, among which the atomic proportion of Ir is about 1.31 at.%, and the mass proportion is about 4.14 wt.%.

[0047] Figure 4The X-ray diffraction spectrum (XRD) of the material shows that the prepared catalyst only shows the (111), (220), and (311) diffraction peaks of CeO2 crystals, and there is no XRD-distinguishable Ir metal or IrO2 crystalline phase. The iridium oxide is recorded as IrO x .

[0048] Figure 5 This is a spherical aberration corrected transmission electron microscopy (SAC-TEM) image. It can be seen that the ultrafine IrO with a particle size of less than 5nm x The clusters are dispersed and embedded in the CeO2 lattice.

[0049] Example 2

[0050] The difference between this embodiment and embodiment 1 is that the Ir content of the catalyst is 2 wt.% and 7 wt.%, and the other steps are the same as those in embodiment 1.

[0051] Figure 6 Figure 2 shows the polarization curves of the deposited oxygen evolution reaction of catalysts with different Ir contents. It can be seen that with the increase of Ir content, the activity of the oxygen evolution reaction gradually increases, but if the Ir content continues to increase, the activity will decrease, which may be due to the fact that IrO x The increase of clusters leads to the loss of active surface area. The optimum Ir content in the low Ir content catalyst is 4 wt.%.

[0052] Example 3

[0053] The difference between this embodiment and embodiment 1 is that the thermalization temperature is adjusted to 200°C and 250°C respectively, and the remaining steps are the same as those in embodiment 1. The effect of the thermalization temperature on the activity of the prepared low Ir content catalyst is investigated, and the results are shown in Table 1.

[0054] Table 1 Comparison of the activity of low Ir content catalysts prepared at different thermalization temperatures

[0055]

[0056] As shown in Table 1, the thermalization temperature has a significant effect on the activity of the catalyst. When the temperature is 220°C, the overpotential of the catalyst is the lowest, which is 193 mV.

[0057] Example 4

[0058] The difference between this embodiment and embodiment 1 is that the heating time is adjusted to 3h and 7h respectively, and the remaining steps are the same as embodiment 1. The effect of heating time on the activity of the prepared low Ir content catalyst is investigated, and the results are shown in Table 2.

[0059] Table 2 Comparison of the activity of low Ir content catalysts prepared at different thermalization times

[0060]

[0061] It can be seen from Table 2 that the thermalization time has a significant effect on the activity of the catalyst. When the thermalization time is 5 h, the overpotential of the catalyst is as low as 193 mV.

[0062] Example 5

[0063] The difference between this embodiment and embodiment 1 is that the amount of H2IrCl6·6H2O added is adjusted to 0 μL, 5 μL, 15 μL, and 20 μL, respectively, and the corresponding concentrations of H2IrCl6·6H2O in the raw material mixture are 0, 0.04 mol / L, 0.08 mol / L, 0.12 mol / L, and 0.16 mol / L, and Ce in the raw material mixture is 3+ The molar ratio of Ir source to H2IrCl6·6H2O was 1:0, 1:0.04, 1:0.08, 1:0.12, and 1:0.16. The remaining steps and drug dosages were the same as in Example 1. The effect of different Ir source dosages on the activity of the low Ir content catalyst was investigated. The results are shown in Table 3.

[0064] Table 3 Comparison of the activity of low Ir content catalysts with different Ir source dosages

[0065]

[0066] It can be seen from Table 3 that the amount of H2IrCl6·6H2O input has a significant effect on the activity of the catalyst. When it is 10μL, the overpotential of the catalyst is as low as 193mV.

[0067] Example 6

[0068] The difference between this embodiment and embodiment 1 is that Ce(NO3)3·6H2O is replaced by CeCl3·6H2O, and the other steps are the same as those of embodiment 1. An ultra-low iridium content catalyst is prepared.

[0069] Example 7

[0070] This embodiment provides an application of a catalyst with a low Ir content, specifically:

[0071] The low Ir content catalyst powder prepared in Example 1 was added to a solvent with a volume ratio of isopropanol, pure water and Nafion binder of 1:1:0.02 at a mass ratio of 1%, and the slurry was sprayed on the proton membrane. After hot pressing, it was used as the anode, denoted as PEM membrane electrode, and the cathode was Pt / C, which was used for hydrogen production in a proton exchange membrane water electrolyzer.

[0072] Example 8

[0073] This embodiment provides an application of a catalyst with a low Ir content, specifically:

[0074] The low Ir content catalyst powder prepared in Example 1 was added into a solvent with a volume ratio of isopropanol, pure water and Nafion binder of 1:1:0.03 at a mass ratio of 5%, and the slurry was sprayed on the proton membrane. After hot pressing, it was used as the anode and Pt / C as the cathode for hydrogen production in a proton exchange membrane water electrolyzer.

[0075] Comparative Example 1

[0076] The catalytic performance of the low Ir content catalyst in Example 1 was compared with that of the commercial IrO2 catalyst. First, the Ir content of the catalyst prepared in Example 1 of the present invention is about 4 wt.%. If the membrane electrode coated catalyst is usually loaded with 10 mg / cm 2 Calculation method: membrane loading = (catalyst thickness × coating area) × iridium content. The membrane electrode loading of the catalyst of the present invention is only about 0.4 mg / cm 2 According to the statistics of data provided by different companies, the Ir loading of commercial membrane electrodes is 2-5wt.%. The Ir loading of the catalyst membrane electrode prepared by the present invention is much lower than that of commercial membrane electrodes.

[0077] Figure 7 The polarization curves of the deposition oxygen evolution reaction of the low Ir content catalyst of Example 1 of the present invention, the commercial catalyst and the CeO2 substrate. The lower the overpotential of the catalyst, the higher the catalytic activity of the material. The low Ir content catalyst has excellent oxygen evolution reaction activity at a current density of 10 mA / cm 2 The overpotential is only 193 mV, which is significantly better than the commercial IrO2 catalyst (~350 mV@10 mA / cm 2 ), while the CeO2 substrate has almost no catalytic activity, indicating that the low Ir content catalyst of Example 1 achieves efficient utilization of precious metals due to its ultrafine clusters.

[0078] Figure 8 The graphs are the chronopotentiometric curves of the low Ir content catalyst of Example 1 of the present invention and the commercial IrO2 catalyst. The pure IrO2 catalyst showed activity decay in the first 50 hours, while the low Ir content catalyst of Example 1 had excellent catalytic stability at 10 mA / cm 2 There was almost no activity decay after running for 240 h, indicating that the lattice-anchored active sites are helpful to improve the durability of the catalyst with low Ir content.

[0079] Comparative Example 2

[0080] The catalytic stability and activity of the low Ir content catalyst prepared in Example 1 are compared with those of the Ir-containing catalyst in the prior art, as shown in Table 4.

[0081] Table 4 Comparison of performance of different catalysts

[0082]

[0083]

[0084] As shown in Table 4, the catalytic activity and stability of the low Ir content catalyst prepared in Example 1 of the present invention in an acidic environment are significantly better than those of most iridium-based catalysts.

[0085] In summary, the low Ir content catalyst of the present invention has high oxygen evolution reaction activity and good stability, and its performance is significantly superior to that of commercial IrO2 catalyst. The temperature, time and Ir raw material dosage of the thermalization all have an impact on the activity of the catalyst. The optimal thermalization temperature is 220°C, the optimal time is 5h, and the optimal dosage of H2IrCl6·6H2O is 10μL (0.08mol / L), which can form ultrafine IrO2 with dispersed lattice anchoring. x clusters, otherwise active IrO x The decrease in the number of units or their aggregation will reduce the catalytic performance. The catalytic activity and stability of the catalyst material with low Ir content prepared in Example 1 of the present invention are superior to other catalysts in the prior art and commercial IrO2 catalysts.

[0086] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.

Claims

1. A method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode, characterized in that: include, The cerium salt and the chloroiridic acid solution are mixed to obtain a raw material mixed solution; The raw material mixture undergoes a thermal reaction; After naturally cooling to room temperature, the powder sample was taken out, and after washing and drying, an ultra-low iridium content catalyst for PEM membrane electrode was obtained.

2. The method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode according to claim 1, characterized in that: The cerium salt is one of Ce(NO3)3·6H2O or CeCl3·6H2O.

3. The method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode according to claim 1, characterized in that: The concentration of chloroiridic acid in the raw material mixed solution is 0-0.16 mol / L.

4. The method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode according to claim 1, characterized in that: The concentration of chloroiridic acid in the raw material mixed solution is 0.08-0.16 mol / L.

5. The method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode according to claim 1, characterized in that: Ce in the raw material mixture 3+ The molar ratio of iridium chloride to chloroiridic acid is 1:0 to 0.

16.

6. The method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode according to claim 1, characterized in that: The thermal reaction temperature is 200-250°C.

7. The method for preparing an ultra-low iridium content catalyst for a PEM membrane electrode according to claim 1, characterized in that: The thermal reaction time is 3 to 7 hours.

8. The ultra-low iridium content catalyst for PEM membrane electrode prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The ultra-low iridium content catalyst for the PEM membrane electrode is IrO x Cluster-doped cerium oxide powder, the structure is ultrafine IrO with particle size less than 5nm x The clusters are anchored in the CeO2 lattice, where IrO x Iridium oxide.

9. The ultra-low iridium content catalyst for PEM membrane electrode according to claim 8, characterized in that: The mass proportion of Ir in the ultra-low iridium content catalyst for PEM membrane electrode is 2-7 wt.%.

10. The use of the ultra-low iridium content catalyst for PEM membrane electrode according to claim 8, characterized in that: The ultra-low iridium content catalyst powder for PEM membrane electrode is added to a solvent with a volume ratio of isopropanol, pure water and Nafion adhesive of 1:1:0.02-0.03 at a mass ratio of 1-5%, and the slurry is sprayed on the proton membrane. After hot pressing, it is used as an anode for hydrogen production in a proton exchange membrane water electrolyzer.