Antibacterial coating process of carlo fiber textile fabric
Through the antibacterial coating process of Carolus fiber textile fabrics, photocatalytic activation and natural antibacterial agents are used to solve the problem that natural fiber textiles are prone to breed bacteria in humid environments, achieve efficient and long-lasting antibacterial effects, extend service life and Meet health and environmental standards.
Patent Information
- Application Number
- CN202410826673.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-08
AI Technical Summary
Natural fiber textiles are prone to breed bacteria and mold in humid environments, leading to problems with hygienic performance and service life. Existing antibacterial treatment methods are not long-lasting and damage the physical properties of the fibers.
An antibacterial coating process for Carolus fiber textile cloth is adopted, including soaking in sodium hydroxide solution to separate the fibers, hydrogen peroxide treatment to remove impurities, softening treatment, UV photocatalytic activation of TiO2, and mixing of silver ions, nano-copper particles, and citrus Extracts, tea polyphenols and other ingredients form an antibacterial solution, which is evenly soaked and dried to solidify the coating.
Significantly improve the antibacterial properties of fibers, form a long-lasting antibacterial barrier, extend the service life of textiles, reduce odor and disease risks caused by bacterial growth, and use environmentally friendly materials, which are safe, non-toxic, and comply with health and environmental standards.
Smart Images

Figure CN118745657A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of textile technology, and in particular to an antibacterial coating process for a karos fiber textile cloth. Background Art
[0002] In recent years, with the increasing awareness of health and environmental protection, natural fibers are increasingly used in textiles. Luffa cylindrica, a widely planted cucurbitaceae plant, has good mechanical strength and biocompatibility, and its fiber is widely used in the manufacture of eco-friendly textiles. However, natural fiber textiles often face the problem of insufficient antibacterial properties in practical applications, which makes it easy to breed bacteria and mold in humid environments, affecting the hygiene and service life of textiles. Therefore, how to maintain the natural characteristics of the fiber while improving its antibacterial properties has become a technical problem that needs to be solved urgently in the current textile industry.
[0003] Existing antibacterial treatment methods often have many shortcomings, such as the antibacterial agent is easy to fall off, the antibacterial effect is not lasting, and the physical properties of the fiber are damaged during the treatment process. Therefore, it is particularly necessary to develop an antibacterial coating process that is efficient, durable and has less impact on the physical properties of the fiber. Summary of the invention
[0004] Based on the above purpose, the present invention provides an antibacterial coating process for Carlos fiber textile fabric.
[0005] An antibacterial coating process for Carlos fiber textile fabric comprises the following steps:
[0006] S1: Slice the raw material of the kiwano and soak it in a sodium hydroxide solution to separate the fibers;
[0007] S2: washing the fiber obtained in S1 in clean water and treating it with a hydrogen peroxide solution to remove impurities and pigments in the fiber;
[0008] S3: softening the fibers treated in S2;
[0009] S4: exposing the fiber softened in S3 to ultraviolet light and using TiO2 for photocatalytic activation to enhance the antibacterial activity of the fiber;
[0010] S5: mixing silver ions, nano copper particles, citrus extract, tea polyphenols, chitosan, hyaluronic acid and natural flavors in deionized water in a predetermined ratio, and homogenizing them using an ultrasonic oscillator to form a stable antibacterial solution;
[0011] S6: Evenly immerse the fiber treated in S4 in the antibacterial solution in S5, so that the antibacterial agent is evenly attached to the fiber surface;
[0012] S7: drying the fiber in S6 in an oven to cure the antibacterial coating by heat treatment;
[0013] S8: Conduct antimicrobial performance test and physical property inspection on the treated fibers.
[0014] Furthermore, the S1 specifically includes:
[0015] S11: Slice the kiwi fruit raw material into slices with a thickness of 5-10 mm;
[0016] S12: placing the slices in S11 into a sodium hydroxide solution, wherein the concentration of the sodium hydroxide solution is 5-10%;
[0017] S13: controlling the soaking temperature to be 50-70° C. and the soaking time to be 1-3 hours to separate the fibers;
[0018] S14: During the soaking process, stir every 30 minutes.
[0019] Furthermore, the S2 specifically includes:
[0020] S21: placing the fiber obtained in S1 in clean water and washing it three times, each washing time being 10-15 minutes;
[0021] S22: placing the cleaned fiber in a 5% hydrogen peroxide solution, controlling the pH value of the hydrogen peroxide solution to be 5-7, maintaining a constant temperature of 40-50° C. during the treatment process, and the treatment time is 1-2 hours;
[0022] S23: After the treatment is completed, the fiber is washed again with clean water, twice, and each washing time is 10-15 minutes.
[0023] Furthermore, the S3 specifically includes:
[0024] S31: placing the fiber treated by S2 in a softener solution containing 2-5% phytosterol, the solution temperature is controlled at 30-40° C.; and soaking the fiber for 30-60 minutes;
[0025] S32: During the soaking process, stir every 10 minutes;
[0026] S33: After soaking, take out the fiber, rinse it with clean water, and wash it twice, each washing time is 10-15 minutes to remove the residual softener.
[0027] Furthermore, the S4 specifically includes:
[0028] S41: evenly spreading the fibers softened in S3 in an ultraviolet light irradiation device;
[0029] S42: setting the wavelength of ultraviolet light to 200-400 nanometers and controlling the irradiation time to 15-30 minutes;
[0030] S43: During the ultraviolet light irradiation process, a TiO2 solution is sprayed on the fiber surface, wherein the concentration of the TiO2 solution is 0.5-1.5%;
[0031] S44: After the photocatalytic treatment is completed, the fiber is left to stand for 10-20 minutes to ensure that TiO2 is fixed on the fiber surface.
[0032] Furthermore, the S5 specifically includes:
[0033] S51: adding each component to deionized water in sequence, wherein the silver ion solution accounts for 0.015% of the total amount of deionized water, the nano copper particles account for 0.007% of the total amount of deionized water, the citrus extract accounts for 0.007% of the total amount of deionized water, the tea polyphenols account for 0.005% of the total amount of deionized water, the chitosan accounts for 0.08% of the total amount of deionized water, the hyaluronic acid accounts for 0.03% of the total amount of deionized water, and the natural flavor accounts for 0.008% of the total amount of deionized water;
[0034] S52: After adding each ingredient, use a stirrer to stir for 5-10 minutes to ensure that the ingredients are initially mixed evenly;
[0035] S53: placing the preliminarily mixed solution in an ultrasonic oscillator, and setting the oscillation frequency to 20-40 kHz and the oscillation time to 30-60 minutes to form a stable antibacterial solution;
[0036] S54: After shaking, let the antimicrobial solution stand for 30 minutes to eliminate bubbles and ensure that the solution is stable.
[0037] Furthermore, the concentration of the silver ion solution is 100-200 ppm, the concentration of the nano copper particles is 50-100 ppm, the concentration of the citrus extract is 50-100 ppm, the concentration of the tea polyphenols is 30-70 ppm, the concentration of the chitosan is 0.5-1%, the concentration of the hyaluronic acid is 0.1-0.5%, and the concentration of the natural flavor is 0.05-0.1%.
[0038] Furthermore, the S6 specifically includes:
[0039] S61: placing the fiber treated in S4 in an antibacterial solution tank, wherein the temperature of the antibacterial solution is controlled at 30-40° C.; and the fiber is immersed in the antibacterial solution for 2-4 hours;
[0040] S62: During the soaking process, stir the antibacterial solution every 20 minutes to ensure that the fibers are evenly exposed to the antibacterial solution;
[0041] S64: After soaking, take out the fiber and hang it to dry for 30 minutes to remove excess antibacterial solution;
[0042] S65: The fibers after hanging and drying are centrifuged using a low-speed centrifuge at a speed of 500-1000 rpm for 5-10 minutes to completely remove excess solution on the fiber surface.
[0043] Furthermore, the S7 specifically includes:
[0044] S71: Spread the fibers treated in S6 evenly on the grid of the oven, and ensure that the fibers do not overlap;
[0045] S72: preheat the oven to 100-120°C and maintain a constant temperature;
[0046] S73: Place the fiber in a preheated oven for 1-2 hours to ensure that the antimicrobial coating is fully cured;
[0047] S74: After drying, the fiber is taken out and cooled at room temperature for 30-60 minutes to restore it to normal temperature and stabilize the structure.
[0048] Furthermore, the S8 specifically includes:
[0049] S81: Conduct an antibacterial performance test, specifically, cut the treated fiber sample into 1cmx1cm sheets; and place the fiber sample on a culture medium containing a standard strain in a sterile environment, and culture the culture medium at 37°C for 24 hours, wherein the standard strain includes Staphylococcus aureus or Escherichia coli; determine the antibacterial performance by counting the diameter of the inhibition zone around the fiber sample, and the standard diameter of the inhibition zone is 10-15mm;
[0050] S82: Perform strength test, specifically use an electronic tensile testing machine to perform tensile test according to GB / T3923.1 standard; record the breaking strength of the fiber sample, the standard breaking strength is 150-200MPa;
[0051] S83: Conduct abrasion resistance test according to GB / T21196 standard, use a rotary abrasion machine to perform 1000 abrasion cycles; record the mass loss of the fiber sample, the standard mass loss should be less than 5%;
[0052] S84: Hygroscopicity test: The hygroscopicity test is carried out in accordance with GB / T21655.1 standard. The fiber sample is placed in a constant humidity environment and the weight change after 24 hours is measured. The standard hygroscopicity rate is 8-12%.
[0053] Beneficial effects of the present invention:
[0054] The present invention effectively improves the antibacterial property of the fiber by adding a photocatalytic activation step and using natural antibacterial agents such as silver ions and tea polyphenols during the fiber treatment process, and can form a long-lasting antibacterial barrier on the fiber surface, thereby significantly extending the service life of the textile and reducing the risk of odor and disease caused by bacterial growth. In addition, the antibacterial agents used are all environmentally friendly materials, which are not only effective but also safe and non-toxic, and meet the high standards of modern textiles for health and environmental protection.
[0055] The present invention ensures that the natural feel and comfort of the fiber are not affected through a unique antibacterial coating formula and process flow. The use of additives such as hyaluronic acid and natural flavors not only enhances the moisture retention and softness of the fiber, but also provides a more pleasant use experience. This antibacterial coating process that comprehensively considers functionality and user experience makes fiber products more competitive in the market and meets consumers' demand for high-quality daily necessities. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only for the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0057] Figure 1 A schematic diagram of an antibacterial coating process according to an embodiment of the present invention;
[0058] Figure 2 Schematic diagram of the process of photocatalytic activation using TiO2 according to an embodiment of the present invention. DETAILED DESCRIPTION
[0059] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0060] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The words "first", "second" and similar words used in the present invention do not indicate any order, quantity or importance, but are only used to distinguish different components. The words "include" or "comprise" and similar words mean that the elements or objects appearing before the word include the elements or objects listed after the word and their equivalents, without excluding other elements or objects.
[0061] Example 1
[0062] like Figure 1-Figure 2 As shown, a process for antibacterial coating of Carlos fiber textile fabric comprises the following steps:
[0063] S1: Slice the raw material of the kiwano and soak it in a sodium hydroxide solution to separate the fibers;
[0064] S2: washing the fiber obtained in S1 in clean water and treating it with a hydrogen peroxide solution to remove impurities and pigments in the fiber;
[0065] S3: Softening the fibers after S2 treatment to make them softer and more absorbent;
[0066] S4: exposing the fiber softened in S3 to ultraviolet light and using TiO2 for photocatalytic activation to enhance the antibacterial activity of the fiber;
[0067] S5: mixing silver ions, nano copper particles, citrus extract, tea polyphenols, chitosan, hyaluronic acid and natural flavors in deionized water in a predetermined ratio, and homogenizing them using an ultrasonic oscillator to form a stable antibacterial solution;
[0068] S6: Evenly immerse the fiber treated in S4 in the antibacterial solution in S5, so that the antibacterial agent is evenly attached to the fiber surface;
[0069] S7: drying the fiber in S6 in an oven to cure the antibacterial coating by heat treatment;
[0070] S8: Conduct antimicrobial and physical property tests on the treated fibers to ensure their antimicrobial effects and test their strength and durability.
[0071] S1 specifically includes:
[0072] S11: Slice the kiwifruit raw material into slices with a thickness of 8 mm;
[0073] S12: placing the slices in S11 into a sodium hydroxide solution, the concentration of the sodium hydroxide solution being 8%;
[0074] S13: controlling the soaking temperature to 60° C. and the soaking time to 2 hours to separate the fibers;
[0075] S14: During the soaking process, the mixture is stirred every 30 minutes to ensure that the melon raw material is fully in contact with the sodium hydroxide solution.
[0076] S2 specifically includes:
[0077] S21: The fiber obtained in S1 is placed in clean water and washed three times, each washing time is 13 minutes;
[0078] S22: placing the cleaned fiber in a 5% hydrogen peroxide solution, controlling the pH value of the hydrogen peroxide solution to be 6, maintaining a constant temperature of 45° C. during the treatment process, and the treatment time is 1.5 hours;
[0079] S23: After the treatment is completed, the fiber is washed again with clean water, twice, and each washing time is 13 minutes.
[0080] S3 specifically includes:
[0081] S31: placing the fiber treated with S2 in a softener solution containing 3% phytosterols, the solution temperature being controlled at 35° C.; and soaking the fiber for 45 minutes to ensure that the softener fully penetrates the fiber;
[0082] S32: During the soaking process, stir every 10 minutes to ensure that the fibers are evenly exposed to the softener solution;
[0083] S33: After soaking, the fiber is taken out and rinsed with clean water for two times, each time for 13 minutes, to remove the residual softener.
[0084] S4 specifically includes:
[0085] S41: evenly spread the fibers softened in S3 in an ultraviolet light irradiation device to keep the fibers flat;
[0086] S42: setting the wavelength of the ultraviolet light to 300 nanometers and controlling the irradiation time to 20 minutes;
[0087] S43: During the ultraviolet light irradiation process, a TiO2 solution is sprayed on the fiber surface, and the concentration of the TiO2 solution is 0.8%;
[0088] S44: After the photocatalytic treatment is completed, the fiber is left to stand for 15 minutes to ensure that TiO2 is fixed on the fiber surface.
[0089] S5 specifically includes:
[0090] S51: In deionized water, the components are added in sequence: silver ion solution accounts for 0.015% of the total amount of deionized water, nano copper particles account for 0.007% of the total amount of deionized water, citrus extract accounts for 0.007% of the total amount of deionized water, tea polyphenols account for 0.005% of the total amount of deionized water, chitosan accounts for 0.08% of the total amount of deionized water, hyaluronic acid accounts for 0.03% of the total amount of deionized water, and natural flavor accounts for 0.008% of the total amount of deionized water;
[0091] S52: After adding each ingredient, use a stirrer to stir for 8 minutes to ensure that the ingredients are initially mixed evenly;
[0092] S53: placing the preliminarily mixed solution in an ultrasonic oscillator, and setting the oscillation frequency to 30 kHz and the oscillation time to 45 minutes to form a stable antibacterial solution;
[0093] S54: After shaking, let the antimicrobial solution stand for 30 minutes to eliminate bubbles and ensure that the solution is stable.
[0094] The concentration of silver ion solution is 150ppm, the concentration of nano copper particles is 75ppm, the concentration of citrus extract is 75ppm, the concentration of tea polyphenols is 50ppm, the concentration of chitosan is 0.8%, the concentration of hyaluronic acid is 0.3%, and the concentration of natural flavor is 0.08%.
[0095] S6 specifically includes:
[0096] S61: placing the fiber treated by S4 in an antibacterial solution tank, wherein the temperature of the antibacterial solution is controlled at 35° C.; and controlling the fiber to be immersed in the antibacterial solution for 3 hours to ensure that the fiber fully absorbs the antibacterial solution;
[0097] S62: During the soaking process, stir the antibacterial solution every 20 minutes to ensure that the fibers are evenly exposed to the antibacterial solution;
[0098] S64: After soaking, take out the fiber and hang it to dry for 30 minutes to remove excess antibacterial solution;
[0099] S65: The fibers after hanging and drying were centrifuged using a low-speed centrifuge at a speed of 700 rpm for 8 minutes to completely remove excess solution on the fiber surface.
[0100] S7 specifically includes:
[0101] S71: Spread the fibers treated in S6 evenly on the grid of the oven, and ensure that the fibers do not overlap;
[0102] S72: preheat the oven to 110° C. and maintain a constant temperature;
[0103] S73: Place the fiber in a preheated oven for 1.5 hours to ensure that the antimicrobial coating is fully cured;
[0104] S74: After drying, the fiber is taken out and cooled at room temperature for 45 minutes to restore it to normal temperature and stabilize the structure.
[0105] S8 specifically includes:
[0106] S81: Conduct an antibacterial performance test, specifically, cut the treated fiber sample into 1cmx1cm sheets; and place the fiber sample on a culture medium containing a standard strain in a sterile environment, and culture the culture medium at 37°C for 24 hours, the standard strain including Staphylococcus aureus; determine the antibacterial performance by counting the diameter of the inhibition zone around the fiber sample, the diameter of the inhibition zone is 15mm;
[0107] S82: Perform strength test, specifically use an electronic tensile testing machine to perform tensile test according to GB / T3923.1 standard; record the breaking strength of the fiber sample, the standard breaking strength is 200MPa;
[0108] S83: Conduct abrasion resistance test according to GB / T21196 standard, use a rotary abrasion machine to perform 1000 abrasion cycles; record the mass loss of the fiber sample, the mass loss is 2%;
[0109] S84: Hygroscopicity test: specifically, the hygroscopicity test is carried out in accordance with GB / T21655.1 standard. The fiber sample is placed in a constant humidity environment and the weight change after 24 hours is measured. The hygroscopicity rate is 10%.
[0110] Example 2
[0111] S1: Slice the kiwifruit raw material into slices with a thickness of 5 mm, and put the slices into a sodium hydroxide solution with a concentration of 5%, a soaking temperature of 50° C., and a soaking time of 1 hour. During the soaking process, stir once every 30 minutes to separate the fibers;
[0112] S2: The fiber obtained in S1 is placed in clean water and washed three times, each washing time is 10 minutes, and the washed fiber is placed in a 5% hydrogen peroxide solution, the pH value of the hydrogen peroxide solution is controlled to be 5, and the temperature is kept constant at 40°C during the treatment process. The treatment time is 1 hour. After the treatment is completed, the fiber is washed again with clean water, washed twice, each washing time is 10 minutes;
[0113] S3: The fiber treated with S2 is placed in a softener solution containing 2% phytosterols, the solution temperature is controlled at 30°C, and the fiber is soaked for 30 minutes. During the soaking process, the fiber is stirred every 10 minutes. After the soaking is completed, the fiber is taken out and rinsed with clean water for two times, each washing time is 10 minutes, so as to remove the residual softener;
[0114] S4: The fibers softened in S3 are evenly spread in an ultraviolet irradiation device, the wavelength of the ultraviolet light is set to 200 nanometers, and the irradiation time is controlled to be 15 minutes. During the ultraviolet irradiation process, a 0.5% concentration of TiO2 solution is sprayed on the fiber surface. After the photocatalytic treatment is completed, the fiber is left to stand for 10 minutes to ensure that TiO2 is fixed on the fiber surface;
[0115] S5: Add each component to deionized water in sequence, the concentration of the silver ion solution is 100ppm, accounting for 0.015% of the total amount of deionized water; the concentration of nano copper particles is 50ppm, accounting for 0.007% of the total amount of deionized water; the concentration of citrus extract is 50ppm, accounting for 0.007% of the total amount of deionized water; the concentration of tea polyphenols is 30ppm, accounting for 0.005% of the total amount of deionized water; the concentration of chitosan is 0.5%, and chitosan accounts for 0.08% of the total amount of deionized water; the concentration of hyaluronic acid is 0.1%, and hyaluronic acid accounts for 0.03% of the total amount of deionized water; the concentration of natural flavor is 0.05%, and natural flavor accounts for 0.008% of the total amount of deionized water; and after adding each component, stir with a stirrer for 5 minutes, place the preliminarily mixed solution in an ultrasonic oscillator, and set the oscillation frequency to 20kHz and the oscillation time to 30 minutes. After the oscillation is completed, let the antibacterial solution stand for 30 minutes to eliminate bubbles and ensure the stability of the solution;
[0116] S6: placing the fiber treated in S4 in an antibacterial solution tank, the temperature of the antibacterial solution is controlled at 30°C; and controlling the fiber to be immersed in the antibacterial solution for 2 hours. During the immersion process, the antibacterial solution is stirred every 20 minutes. After the immersion, the fiber is taken out and hung to dry for 30 minutes to remove excess antibacterial solution. The fiber after hanging to dry is centrifuged in a low-speed centrifuge at a speed of 500 rpm for 5 minutes to completely remove excess solution on the fiber surface;
[0117] S7: Spread the fibers treated in S6 evenly on the grid of the oven, and make sure that the fibers do not overlap, preheat the oven to 100°C and maintain a constant temperature, place the fibers in the preheated oven, and dry them for 1 hour to ensure that the antibacterial coating is completely cured. After drying, take out the fibers and cool them at room temperature for 30 minutes to restore them to room temperature and stabilize the structure;
[0118] S8: Antibacterial performance test, cut the treated fiber sample into 1cm x 1cm sheets; and in a sterile environment, place the fiber sample on a culture medium containing Escherichia coli, and culture the culture medium at 37°C for 24 hours, and determine the antibacterial performance by counting the diameter of the inhibition zone around the fiber sample, and the diameter of the inhibition zone is 13mm; perform strength test, use an electronic tensile testing machine, and record the breaking strength of the fiber sample as 150MPa; perform wear resistance test, use a rotary abrasion machine for 1000 abrasion cycles, and record the mass loss of the fiber sample as 4%; hygroscopicity test, place the fiber sample in a constant humidity environment, measure the weight change after 24 hours, and the moisture absorption rate is 8%.
[0119] Example 3
[0120] S1: Slice the raw material of the kiwano to a thickness of 10 mm, and put the slices into a sodium hydroxide solution, wherein the concentration of the sodium hydroxide solution is 10%, the soaking temperature is controlled to be 70° C., and the soaking time is 3 hours. During the soaking process, stir once every 30 minutes to separate the fibers;
[0121] S2: The fiber obtained in S1 is placed in clean water and washed three times, each washing time is 15 minutes, and the washed fiber is placed in a 5% hydrogen peroxide solution, the pH value of the hydrogen peroxide solution is controlled to be 7, and the temperature is kept constant at 50°C during the treatment process. The treatment time is 2 hours. After the treatment is completed, the fiber is washed again with clean water, washed twice, each washing time is 15 minutes;
[0122] S3: placing the fiber treated with S2 in a softener solution containing 5% phytosterols, the solution temperature is controlled at 40°C, and the fiber is soaked for 60 minutes. During the soaking process, the fiber is stirred every 10 minutes. After the soaking is completed, the fiber is taken out and rinsed with clean water for two times, each washing time is 15 minutes, so as to remove the residual softener;
[0123] S4: The fibers softened in S3 are evenly spread in an ultraviolet irradiation device, the wavelength of the ultraviolet light is set to 400 nanometers, and the irradiation time is controlled to be 30 minutes. During the ultraviolet irradiation process, a 1.5% concentration of TiO2 solution is sprayed on the fiber surface. After the photocatalytic treatment is completed, the fiber is left to stand for 20 minutes to ensure that TiO2 is fixed on the fiber surface;
[0124] S5: adding each component to deionized water in sequence, wherein the concentration of the silver ion solution is 200ppm, accounting for 0.015% of the total amount of deionized water; the concentration of the nano copper particles is 100ppm, accounting for 0.007% of the total amount of deionized water; the concentration of the citrus extract is 100ppm, accounting for 0.007% of the total amount of deionized water; the concentration of the tea polyphenols is 70ppm, accounting for 0.005% of the total amount of deionized water; the concentration of chitosan is 1%, and chitosan accounts for 0.08% of the total amount of deionized water; the concentration of hyaluronic acid is 0.5%, and hyaluronic acid accounts for 0.03% of the total amount of deionized water; the concentration of the natural flavor is 0.1%, and the natural flavor accounts for 0.008% of the total amount of deionized water; and after adding each component, stirring with a stirrer for 10 minutes, placing the preliminarily mixed solution in an ultrasonic oscillator, and setting the oscillation frequency to 40kHz, the oscillation time to 60 minutes, after the oscillation is completed, the antibacterial solution is allowed to stand for 30 minutes to eliminate bubbles and ensure the stability of the solution;
[0125] S6: placing the fiber treated in S4 in an antibacterial solution tank, the temperature of the antibacterial solution is controlled at 40°C; and controlling the fiber to be immersed in the antibacterial solution for 4 hours. During the immersion process, the antibacterial solution is stirred every 20 minutes. After the immersion, the fiber is taken out and hung to dry for 30 minutes to remove excess antibacterial solution. The fiber after hanging to dry is centrifuged in a low-speed centrifuge at a centrifugal speed of 1000 rpm for 10 minutes to completely remove excess solution on the fiber surface;
[0126] S7: Spread the fibers treated in S6 evenly on the grid of the oven, and make sure that the fibers do not overlap. Preheat the oven to 120°C and keep the temperature constant. Place the fibers in the preheated oven for 2 hours to ensure that the antibacterial coating is completely cured. After the drying is completed, take out the fibers and cool them at room temperature for 60 minutes to restore them to room temperature and stabilize the structure.
[0127] S8: Antibacterial performance test, cut the treated fiber sample into 1cm x 1cm sheets; in a sterile environment, place the fiber sample on a culture medium containing Staphylococcus aureus, and culture the culture medium at 37°C for 24 hours, and determine the antibacterial performance by counting the diameter of the inhibition zone around the fiber sample, the diameter of the inhibition zone is 10mm; strength test, use an electronic tensile testing machine, record the breaking strength of the fiber sample as 200MPa; wear resistance test, use a rotary abrasion machine for 1000 abrasion cycles, and record the mass loss of the fiber sample as 5%; hygroscopicity test, place the fiber sample in a constant humidity environment, measure the weight change after 24 hours, the hygroscopicity rate is 12%.
[0128] Table 1 Comparison of finished product experimental data
[0129] Compare Projects Example 1 Example 2 Example 3 Diameter of inhibition zone (mm) 15 13 10 Strength (MPa) 200 150 200 Wear resistance mass loss (%) 2 4 5 Moisture absorption rate (%) 10 8 12 Drying time (hours) 1.5 1 2 Soaking time (hours) 3 2 4
[0130] As can be seen from Table 1 above, Example 1 exhibits the best antibacterial performance, and the diameter of the inhibition zone is the largest, reaching 15 mm, which shows that its antibacterial agent has the most significant effect on the fiber; the fiber strength of Example 1 and Example 3 is the same, both of which are 200 MPa, showing high mechanical strength; Example 1 performs best in the wear resistance test, with a mass loss of only 2%, indicating that its wear resistance is better than other examples; Example 2 has the lowest moisture absorption rate of 8%, which is suitable for applications that need to be kept dry; Example 2 has the shortest drying time and the total processing time is relatively short, which means that the efficiency is higher in the production process.
[0131] Based on the above comparison, Example 1 performs best in most key performance indicators, especially in antibacterial performance and wear resistance, and is suitable for application in textiles that require high durability and hygiene. Although Example 2 has advantages in hygroscopicity and processing time, it is slightly inferior in antibacterial performance and wear resistance. Although Example 3 is on par with Example 1 in mechanical strength, it performs poorly in other performance indicators, especially in wear resistance and antibacterial performance.
[0132] Table 2 Comparison of other performance parameters
[0133] Compare Projects Example 1 Example 2 Example 3 Residual softener removal rate (%) 98 95 93 TiO2 fixation rate (%) 90 85 80 Silver ion content (ppm) 150 100 200 Nano copper particle content (ppm) 75 50 100 pH value control accuracy (range) 5.9-6.1 4.9-5.1 6.9-7.1 UV exposure time (minutes) 20 15 30 Hydrogen peroxide treatment time (hours) 1.5 1 2
[0134] It can be seen from Table 2 above that the residual softener removal rate of Example 1 is the highest, which is 98%, indicating that its fiber purity is the best; the TiO2 fixation rate of Example 1 is 90%, which is the highest, showing that its antibacterial active material has the best adhesion effect on the fiber surface; the silver ion and nano-copper particle contents of Example 3 are the highest, which are 200ppm and 100ppm respectively. Although the content is high, it will increase the cost and affect other properties in practical applications; the pH value control of Example 1 is the most accurate, ranging from 5.9 to 6.1, which is crucial to ensure the stability and performance consistency of the fiber; the ultraviolet light irradiation time of Example 2 is the shortest, which is 15 minutes, indicating that its photocatalytic treatment efficiency is high, but it affects the TiO2 fixation rate and antibacterial effect; the hydrogen peroxide treatment time of Example 2 is the shortest, which is only 1 hour, which means that its treatment efficiency is high, but it affects the final fiber purity and antibacterial effect.
[0135] Based on the above comparison, Example 1 performs best in key performance indicators such as residual softener removal rate, TiO2 fixation rate, and pH value control accuracy. Overall, it is still the best example and is suitable for applications with high requirements on fiber purity, antibacterial effect and stability.
[0136] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. An antibacterial coating process for Carlos fiber textile fabric, characterized in that: The following steps are involved: S1: Slice the raw material of the kiwano and soak it in a sodium hydroxide solution to separate the fibers; S2: washing the fiber obtained in S1 in clean water and treating it with a hydrogen peroxide solution to remove impurities and pigments in the fiber; S3: softening the fibers treated in S2; S4: exposing the fiber softened in S3 to ultraviolet light and using TiO2 for photocatalytic activation to enhance the antibacterial activity of the fiber; S5: mixing silver ions, nano copper particles, citrus extract, tea polyphenols, chitosan, hyaluronic acid and natural flavors in deionized water in a predetermined ratio, and homogenizing them using an ultrasonic oscillator to form a stable antibacterial solution; S6: Evenly immerse the fiber treated in S4 in the antibacterial solution in S5, so that the antibacterial agent is evenly attached to the fiber surface; S7: drying the fiber in S6 in an oven to cure the antibacterial coating by heat treatment; S8: Conduct antimicrobial performance test and physical property inspection on the treated fibers.
2. The antibacterial coating process of Carlos fiber textile fabric according to claim 1, characterized in that: The S1 specifically includes: S11: Slice the kiwi fruit raw material into slices with a thickness of 5-10 mm; S12: placing the slices in S11 into a sodium hydroxide solution, wherein the concentration of the sodium hydroxide solution is 5-10%; S13: controlling the soaking temperature to be 50-70° C. and the soaking time to be 1-3 hours to separate the fibers; S14: During the soaking process, stir every 30 minutes.
3. The antibacterial coating process of Carlos fiber textile fabric according to claim 1, characterized in that: The S2 specifically includes: S21: placing the fiber obtained in S1 in clean water and washing it three times, each washing time being 10-15 minutes; S22: placing the cleaned fiber in a 5% hydrogen peroxide solution, controlling the pH value of the hydrogen peroxide solution to be 5-7, maintaining a constant temperature of 40-50° C. during the treatment process, and the treatment time is 1-2 hours; S23: After the treatment is completed, the fiber is washed again with clean water, twice, and each washing time is 10-15 minutes.
4. The antibacterial coating process of a Carlos fiber textile fabric according to claim 1, characterized in that: The S3 specifically includes: S31: placing the fiber treated by S2 in a softener solution containing 2-5% phytosterol, the solution temperature is controlled at 30-40° C.; and soaking the fiber for 30-60 minutes; S32: During the soaking process, stir every 10 minutes; S33: After soaking, take out the fiber, rinse it with clean water, and wash it twice, each washing time is 10-15 minutes to remove the residual softener.
5. The antibacterial coating process of Carlos fiber textile fabric according to claim 1, characterized in that: The S4 specifically includes: S41: evenly spreading the fibers softened in S3 in an ultraviolet light irradiation device; S42: setting the wavelength of ultraviolet light to 200-400 nanometers and controlling the irradiation time to 15-30 minutes; S43: During the ultraviolet light irradiation process, a TiO2 solution is sprayed on the fiber surface, wherein the concentration of the TiO2 solution is 0.5-1.5%; S44: After the photocatalytic treatment is completed, the fiber is left to stand for 10-20 minutes to ensure that TiO2 is fixed on the fiber surface.
6. The antibacterial coating process of Carlos fiber textile fabric according to claim 1, characterized in that: The S5 specifically includes: S51: adding each component to deionized water in sequence, wherein the silver ion solution accounts for 0.015% of the total amount of deionized water, the nano copper particles account for 0.007% of the total amount of deionized water, the citrus extract accounts for 0.007% of the total amount of deionized water, the tea polyphenols account for 0.005% of the total amount of deionized water, the chitosan accounts for 0.08% of the total amount of deionized water, the hyaluronic acid accounts for 0.03% of the total amount of deionized water, and the natural flavor accounts for 0.008% of the total amount of deionized water; S52: After adding each ingredient, use a stirrer to stir for 5-10 minutes to ensure that the ingredients are initially mixed evenly; S53: placing the preliminarily mixed solution in an ultrasonic oscillator, and setting the oscillation frequency to 20-40 kHz and the oscillation time to 30-60 minutes to form a stable antibacterial solution; S54: After shaking, let the antimicrobial solution stand for 30 minutes to eliminate bubbles and ensure that the solution is stable.
7. The antibacterial coating process of Carlos fiber textile fabric according to claim 6, characterized in that: The concentration of the silver ion solution is 100-200ppm, the concentration of the nano copper particles is 50-100ppm, the concentration of the citrus extract is 50-100ppm, the concentration of the tea polyphenols is 30-70ppm, the concentration of the chitosan is 0.5-1%, the concentration of the hyaluronic acid is 0.1-0.5%, and the concentration of the natural flavor is 0.05-0.1%.
8. The antibacterial coating process of Carlos fiber textile fabric according to claim 1, characterized in that: The S6 specifically includes: S61: placing the fiber treated in S4 in an antibacterial solution tank, wherein the temperature of the antibacterial solution is controlled at 30-40° C.; and the fiber is immersed in the antibacterial solution for 2-4 hours; S62: During the soaking process, stir the antibacterial solution every 20 minutes to ensure that the fibers are evenly exposed to the antibacterial solution; S64: After soaking, take out the fiber and hang it to dry for 30 minutes to remove excess antibacterial solution; S65: The fibers after hanging and drying are centrifuged using a low-speed centrifuge at a speed of 500-1000 rpm for 5-10 minutes to completely remove excess solution on the fiber surface.
9. The antibacterial coating process of Carlos fiber textile fabric according to claim 1, characterized in that: The S7 specifically includes: S71: Spread the fibers treated in S6 evenly on the grid of the oven, and ensure that the fibers do not overlap; S72: preheat the oven to 100-120°C and maintain a constant temperature; S73: Place the fiber in a preheated oven for 1-2 hours to ensure that the antimicrobial coating is fully cured; S74: After drying, the fiber is taken out and cooled at room temperature for 30-60 minutes to restore it to normal temperature and stabilize the structure.
10. The antibacterial coating process of Carlos fiber textile fabric according to claim 1, characterized in that: The S8 specifically includes: S81: Conduct an antibacterial performance test, specifically, cut the treated fiber sample into 1cmx1cm sheets; and place the fiber sample on a culture medium containing a standard strain in a sterile environment, and culture the culture medium at 37°C for 24 hours, wherein the standard strain includes Staphylococcus aureus or Escherichia coli; determine the antibacterial performance by counting the diameter of the inhibition zone around the fiber sample, and the standard diameter of the inhibition zone is 10-15mm; S82: Perform strength test, specifically use an electronic tensile testing machine to perform tensile test according to GB / T3923.1 standard; record the breaking strength of the fiber sample, the standard breaking strength is 150-200MPa; S83: Conduct abrasion resistance test according to GB / T21196 standard, use a rotary abrasion machine to perform 1000 abrasion cycles; record the mass loss of the fiber sample, the standard mass loss should be less than 5%; S84: Hygroscopicity test: specifically, the hygroscopicity test is carried out in accordance with GB / T21655.1 standard. The fiber sample is placed in a constant humidity environment and the weight change after 24 hours is measured. The standard hygroscopicity rate is 8-12%.
Citation Information
Cited By
Calotropis gigantea fiber with antibacterial property and application thereof
CN121381229A