Functional polyester-covered cotton fabric as well as preparation method and application thereof
Through the synergistic finishing of nano-zinc oxide and fluorine-free waterproofing agent on the polyester cover cotton fabric, combined with the cooling finishing agent, a hydrophobic and anti-UV layer is formed, which solves the problem of insufficient UV protection and moisture conductivity of the traditional polyester cover cotton fabric and realizes It ensures the excellent moisture conduction and cooling properties of the fabric, and ensures environmental protection and long-lasting performance.
Patent Information
- Application Number
- CN202410942555.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-15
AI Technical Summary
Traditional polyester-cotton fabrics have deficiencies in UV protection and moisture conductivity, and the cooling function is not effective in high-humidity environments. The commonly used waterproofing agents, fluorinated compounds, are not environmentally friendly and the effect is reduced after washing.
Nano-zinc oxide and fluorine-free waterproofing agent are used to synergistically finish the fabric surface. Combined with the cooling finishing agent, a hydrophobic and anti-UV layer is formed through coating technology to improve the fabric's moisture conductivity and anti-UV properties, and the cooling effect is enhanced through the impregnation method.
It achieves good anti-UV function of the fabric, enhances the one-way moisture conduction performance and cooling effect, and at the same time overcomes the problem that the function of conventional cooling functional finishing agents weakens after the number of washing times increases, and the use of fluorine-free waterproofing agent is environmentally friendly.
Smart Images

Figure HDA0004944612250000011 
Figure HDA0004944612250000012 
Figure HDA0004944612250000021
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, in particular to a functional polyester-covered cotton fabric and a preparation method and application thereof. Background Art
[0002] As people's living standards improve, the demand for textile functionality is growing, and the research and development of textiles with multifunctional finishing has become a development benchmark for the textile industry. Polyester-covered cotton fabric, a fabric interwoven with polyester and cotton fibers, combines the advantages of polyester and cotton fibers and has the characteristics of wear resistance, easy washing, and wrinkle resistance. However, the outdoor performance of traditional polyester-covered cotton fabric is average, its protection against ultraviolet effects is average, and its hygroscopic effect is quite different from that of cotton fabrics. It has no cooling or cooling function and cannot alleviate the discomfort caused by high temperature weather.
[0003] However, the research on fabrics with anti-ultraviolet function mainly focuses on the addition of ultraviolet absorbers and the use of nanotechnology, such as the improvement of fabrics' anti-ultraviolet ability. In terms of ultraviolet absorbers, there are many substances with excellent anti-ultraviolet performance, such as benzophenone derivatives and benzotriazole derivatives. However, the use of ultraviolet absorbers may affect the comfort of fabrics. In nanotechnology, especially the nano zinc oxide finishing process, it provides a new direction for the development of anti-ultraviolet fabrics. When nano zinc oxide is applied to natural fibers, such as cotton, linen, silk, etc., its anti-ultraviolet effect has been widely studied and recognized. Compared with polyester fiber (PET) and polyamide fiber (such as nylon), there are relatively few studies on the functional finishing of nano zinc oxide. This is due to the differences in chemical structure and physical properties between synthetic fibers and natural fibers. Existing one-way moisture conduction products usually add moisture absorption and perspiration aids to the fabric, as well as some waterproofing agents or waxes to achieve the purpose of one-way moisture conduction. At present, these waterproofing agents contain some fluorine compounds, which are not environmentally friendly, and the effect is reduced after repeated washing. There are two main methods for preparing existing cooling functional fabrics: one is to use cooling functional fibers for weaving, and the other is to use cooling functional finishing processes. Cooling functional fibers are mostly prepared by physical or chemical modification of chemical fibers, but their breathability and sweat-wicking ability are limited, and wearing them in high humidity conditions will still cause a strong sense of stuffiness; the function of cooling functional finishing agents will weaken with the increase in the number of washings.
[0004] Therefore, it is necessary to provide a method for preparing a functional polyester-covered cotton fabric that simultaneously meets the requirements of moisture conduction, cooling and UV protection to solve the above problems. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing a functional polyester-covered cotton fabric, and the obtained functional polyester-covered cotton fabric has good anti-ultraviolet function, enhanced unidirectional moisture conduction performance, and also has a cooling effect.
[0006] The invention also provides the functional polyester-covered cotton fabric.
[0007] The invention also provides application of the functional polyester-covered cotton fabric.
[0008] The first aspect of the present invention provides a method for preparing the above-mentioned nano yarn unidirectional moisture-conducting fabric, the preparation method comprising the following steps:
[0009] The preparation method comprises the following steps:
[0010] S1, treating a polyester-covered cotton fabric substrate in a cool finishing agent;
[0011] S2, mixing the nano zinc oxide and the dispersant and subjecting them to ultrasonic treatment to obtain a nano zinc oxide dispersion;
[0012] S3, mixing the nano zinc oxide dispersion and the thickener, and coating the mixture on the first surface of the fabric substrate treated in step S1;
[0013] S4, mixing the mixed solution obtained in step S3 with the fluorine-free waterproofing agent, and coating the mixture on the first surface of the fabric substrate treated in step S3.
[0014] The preparation method according to the first aspect of the present invention has at least the following beneficial effects:
[0015] The present invention adopts coating technology to synergistically finish a nano zinc solution dispersion and a fluorine-free waterproofing agent on the surface of a fabric, giving a hydrophobic structure to one side of the fabric, improving the difference in hydrophilic wetting structures inside and outside the fabric, coating a nano zinc oxide dispersion on the other side, giving the fabric anti-ultraviolet performance, and achieving a cooling effect on the fabric by an immersion method. At the same time, a nano zinc solution dispersion, a fluorine-free waterproofing agent and a thickener are synergistically used on the surface of the fabric to form an anti-ultraviolet layer and a unidirectional moisture-conducting layer, the overall performance and stability of the coating are improved, while overcoming the problem that the function of the cooling function finishing agent will be weakened with an increase in the number of washings.
[0016] According to some embodiments of the present invention, in step S1, the weight of the fabric substrate is 180-220 g / m 2 The warp density is 280-320 strands / 10cm, and the weft density is 240-280 strands / 10cm.
[0017] Preferably, in step S1, the weight of the fabric substrate is 200 g / m 2The warp density is 300 strands / 10cm, and the weft density is 260 strands / 10cm.
[0018] According to some embodiments of the present invention, in step S1, the cool finishing agent is COOL-MAX contact cool finishing agent.
[0019] According to some embodiments of the present invention, in step S1, the concentration of the cool finishing agent is 5 to 11 wt %.
[0020] Preferably, in step S1, the concentration of the cool finishing agent is 7-9 wt%.
[0021] According to some embodiments of the present invention, in step S1, the soaking time is 20 to 35 minutes.
[0022] According to some embodiments of the present invention, in step S1, the soaking temperature is 50-80°C.
[0023] According to some embodiments of the present invention, in step S2, the dispersant is polynaphthalenesulfonate sodium salt (NNO).
[0024] According to some embodiments of the present invention, in step S2, the concentration of the dispersant is 0.6-1.0 g / L.
[0025] According to some embodiments of the present invention, in step S2, the mass ratio of the nano zinc oxide to the dispersant is 1:0.4-0.7.
[0026] According to some embodiments of the present invention, in step S2, the ultrasonic treatment time is 5 to 15 minutes.
[0027] According to some embodiments of the present invention, in step S2, the frequency of the ultrasonic treatment is 10 to 30 KHZ.
[0028] Preferably, in step S2, the frequency of the ultrasonic treatment is 20 KHZ.
[0029] According to some embodiments of the present invention, in step S2, the power of the ultrasonic treatment is 400-600W.
[0030] Preferably, in step S2, the power of the ultrasonic treatment is 500W.
[0031] According to some embodiments of the present invention, in step S3, the thickener is PTF.
[0032] According to some embodiments of the present invention, in step S3, the concentration of the thickener is 2-4 wt %.
[0033] Preferably, in step S3, the concentration of the thickener is 3 wt %.
[0034] According to some embodiments of the present invention, in step S3, the mass ratio of the nano zinc oxide dispersion to the thickener is 23-27:2.
[0035] Preferably, in step S3, the mass ratio of the nano zinc oxide dispersion to the thickener is 25:2.
[0036] According to some embodiments of the present invention, in step S3, the coating has a thickness of 450-550 μm.
[0037] According to some embodiments of the present invention, in step S4, the fluorine-free waterproofing agent is PSY CONC.
[0038] According to some embodiments of the present invention, in step S4, the concentration of the fluorine-free waterproofing agent is 13-17 wt %.
[0039] Preferably, in step S4, the concentration of the fluorine-free waterproofing agent is 15 wt %.
[0040] According to some embodiments of the present invention, in step S4, the mass ratio of the mixed liquid to the fluorine-free waterproofing agent is 23-27:2.
[0041] Preferably, in step S4, the mass ratio of the mixed liquid to the fluorine-free waterproofing agent is 25:2.
[0042] The second aspect of the present invention provides a functional polyester-covered cotton fabric, the functional polyester-covered cotton fabric comprising:
[0043] Fabric substrate;
[0044] A cooling layer impregnated on the fabric substrate;
[0045] A UV protection layer coated on one side of the first surface of the fabric substrate;
[0046] A unidirectional moisture conducting layer is coated on the second surface of the fabric substrate.
[0047] The third aspect of the present invention provides the use of the functional polyester-cotton fabric in the preparation of textile products.
[0048] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0050] Figure 1is a preparation process diagram of the functional polyester-covered cotton fabric in Example 1 of the present invention;
[0051] Figure 2 This is a graph showing the effect of different concentrations of dispersants on the nano zinc oxide dispersion in Test Example 1 of the present invention;
[0052] Figure 3 This is a graph showing the effect of different ultrasonic times on the nano zinc oxide dispersion in Test Example 1 of the present invention;
[0053] Figure 4 : is a graph showing the effect of different concentrations of fluorine-free waterproofing agents on the contact angle of fabrics in Test Example 2 of the present invention;
[0054] Figure 5 1 is a graph showing the effect of different concentrations of fluorine-free waterproofing agents on the moisture absorption properties of fabrics in Test Example 2 of the present invention;
[0055] Figure 6 : is a graph showing the effect of the number of times the unidirectional moisture conducting layer is coated on the contact angle of the fabric in Test Example 3 of the present invention;
[0056] Figure 7 This is a graph showing the effect of the number of times the unidirectional moisture conducting layer is coated on the moisture absorption performance of the fabric in Test Example 3 of the present invention;
[0057] Figure 8 This is a graph showing the effect of the number of times the UV protection layer is applied on the UV protection performance in Test Example 4 of the present invention;
[0058] Fig. 9 is a graph showing the effect of the cool feeling finishing agent on the cool feeling coefficient in Test Example 5 of the present invention;
[0059] Fig.10 is a graph showing the effect of immersion temperature on the coolness coefficient in Test Example 5 of the present invention;
[0060] Fig.11 Graph showing the effect of immersion time on the coolness coefficient in Test Example 5 of the present invention. DETAILED DESCRIPTION
[0061] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0062] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0063] When a numerical range is disclosed herein, the above range is considered to be continuous and includes the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0064] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of the present invention.
[0065] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0066] Reagents and instruments used in the examples of the present invention:
[0067] Nano ZnO: Shanghai Mecoxlin Biochemical Technology Co., Ltd.;
[0068] Anhydrous sodium carbonate: Guangzhou brand chemical reagent;
[0069] Dispersant NNO: Shanghai Mecoxlin Biochemical Technology Co., Ltd.;
[0070] Cool finishing agent COOL-MAX: Anbo Chemical Co., Ltd.
[0071] Thickener PTF: Foshan Chuanhua Fulian Fine Chemical Co., Ltd.;
[0072] High-concentration fluorine-free waterproof PSY CONC: Shanghai Fuke New Materials Co., Ltd.;
[0073] Electric constant temperature air drying oven: DHG-9070A, Shanghai Jinghong Experimental Equipment Co., Ltd.
[0074] Fabric UV resistance tester: NF2021, Ningbo Textile Instrument Factory;
[0075] Homogenizer: IKA T25, IKA, Germany;
[0076] Electronic balance: NBL254, Adam Equipment (Wuhan) Co., Ltd.
[0077] Contact angle measuring instrument: DSA25E, Kuss, Germany;
[0078] Nanoparticle size and zeta potential instrument: Y571B, Malvern Instruments Ltd.
[0079] Textile contact coolness coefficient tester: NF3031, Ningbo Textile Instrument Factory;
[0080] Example 1
[0081] This embodiment 1 provides a method for preparing a functional polyester-covered cotton fabric, comprising the following steps:
[0082] 1) Weigh 15 mL of COOL-MAX and pour it into 85 mL of distilled water. Soak the polyester-covered cotton fabric substrate in the COOL-MAX solution and soak it in a 60°C water bath for 30 minutes. Dry it in an oven at 80°C for 20 minutes, then take out the fabric and let it stand at room temperature for 1 hour.
[0083] 2) 1.5 g of nano ZnO and 0.08 g of NNO were added to a beaker, and then 100 mL of purified water was added, and ultrasonic dispersion was performed for 10 min, with an ultrasonic power of 500 W and an ultrasonic frequency of 20 KH, and then stirred for 10 min using a homogenizer to obtain a nano ZnO dispersion;
[0084] 3) Mix the nano ZnO dispersion and the thickener PTF with a concentration of 3wt% in a mass ratio of 25:2, mix under an electric stirrer to obtain an anti-ultraviolet finishing liquid, and use a coating roller to coat the single side surface of the polyester-covered cotton fabric three times, each coating is dried in an oven at 80°C for 20 minutes, and then continue coating. The thickness of the first coating is 500±50μm;
[0085] 4) The nano ZnO dispersion and 3 wt% thickener PTF mixed solution in step 3) are added with 15 wt% fluorine-free waterproof agent PSY CONC and mixed at a mass ratio of 25:2 under an electric stirrer to obtain a unilateral moisture-conducting finishing solution. A coating roller is used to coat the single side surface of the polyester-covered cotton fabric three times. Each coating is dried in an oven at 80° C. for 10 minutes, and then the coating is continued. The thickness of the other coating is 500±50 μm, and a polyester-covered cotton fabric with anti-ultraviolet, unilateral moisture-conducting and cooling functions is obtained. The process flow chart is as follows: Figure 1 shown.
[0086] Test Example 1
[0087] The particle size was measured using a nanoparticle size analyzer and a zeta potential analyzer.
[0088] The nano zinc oxide dispersion prepared with dispersant NNO concentrations of 0, 0.2, 0.4, 0.6, 0.8, 1.0, and 1.2 g / L was tested; when the dispersant concentration is too low, the dispersant molecules are not enough to completely cover the surface of Nano-Zno (nano zinc oxide) particles, resulting in stronger interaction between particles and easy aggregation into particles with large particle size. As the concentration of NNO increases, the molecules of the surfactant gradually adsorb on the surface of the particles, reducing the attraction between the particles, thereby reducing the average particle size and PDI. When the dispersant concentration is too high, too many dispersant molecules may increase the bond resistance between the particles, which in turn increases the mutual repulsion between the particles, causing the particles to re-aggregate, thereby increasing the average particle size and PDI. The bond repulsion between the dispersant and the Nano-Zno particles affects the dispersion effect. If the force between the dispersant and the particles is too strong or too weak, it may lead to poor dispersion effect, resulting in an increase in the average particle size and PDI. Therefore, when the dispersant concentration is within a limited range, the dispersant molecules form a uniform and stable dispersion layer on the surface of the Nano-Zno particles, and the interaction force between the particles is minimized, so the average particle size and PDI reach the minimum value. The results are as follows Figure 2 shown.
[0089] Nano zinc oxide dispersions prepared with ultrasonic times of 0, 5, 10, 15, 20, and 25 min were used for testing. Ultrasonic waves produce high-frequency vibrations and cavitation effects in the liquid, which can destroy the agglomeration structure between particles and make the nano ZnO particles more evenly dispersed in the solvent. The nanoparticles gradually broke with the increase of ultrasonic dispersion time, so the average values of the particle size and PDI gradually decreased. When the dispersion time reached 10 min, it was observed that the average particle size and PDI values reached the minimum value, which may be because the energy input of ultrasonic dispersion and the agglomeration force between particles reached a state of equilibrium. At this time, the energy of ultrasonic dispersion is sufficient to break the agglomeration between particles, but will not excessively destroy the stability of the particles, so the dispersion effect is the best. When the ultrasonic dispersion time is too long, the average particle size and PDI begin to increase. This may be because the ultrasonic dispersion for too long causes the particle surface to be damaged, or the stability between particles is destroyed, resulting in re-agglomeration. In addition, long-term ultrasonic dispersion may also cause the temperature of the solvent to rise, affecting the dispersion effect. The results are shown in Figure 2. Figure 3 shown.
[0090] Test Example 2
[0091] The contact angle test is in accordance with the national standard GB / T 30693-2014.
[0092] Functional polyester-covered cotton fabrics prepared with fluorine-free waterproofing agent concentrations of 0%, 5%, 10%, 15%, 20%, and 25% were tested. When the concentration of fluorine-free waterproofing agent was 15%, the growth rate of the contact angle of the coating surface slowed down, and the moisture absorption time was stable in the 40s range. At this time, the waterproofing agent factor adsorbed the fabric fiber structure to the maximum value, and the unidirectional moisture conduction effect reached the best. The results Figure 5 shown.
[0093] When the concentration of fluorine-free water repellent is too high, the contact angle of the coating surface is stable, but the hydrophobic angle of the hydrophilic surface also tends to increase slowly. This is because the fluorine-free water repellent can not only form a waterproof layer on the surface of the fabric, but also penetrate to the back of the fabric, resulting in a hydrophobic effect on both sides. However, this double-sided hydrophobic effect will affect the unidirectional moisture conduction of the fabric, that is, the direction of water transfer on the fabric is subject to certain restrictions, and the results are as follows: Figure 4 shown.
[0094] The influence of coating times on the unidirectional moisture-conducting layer: As the coating times increase, the contact angle of the hydrophobic layer increases, while the contact angle of the hydrophilic layer changes within a stable range. When the coating times reach 3 times, the contact angle of the hydrophobic layer increases slowly, but the contact angle of the hydrophilic layer continues to increase, and the moisture absorption and penetration time increases. The best coating times are 3 times.
[0095] When the number of coatings is less than 3 times, as the coating thickness increases, the thicker coating can form a smoother and more continuous surface, thereby providing better hydrophobic performance. Water droplets are more likely to form spheres on the surface and have a larger contact angle, and the contact angle of the hydrophilic layer is also increasing; when the number of coatings is greater than 3 layers, because the coating liquid is not dry enough, only one side is coated during the coating process, but there is also a phenomenon that the solution penetrates through the fabric to the other side, causing the water contact angle of the hydrophilic layer to increase and the moisture absorption time to be prolonged. Therefore, for the one-way moisture conduction effect, the high-concentration fluorine-free waterproof PSY CONC coating number is 3 layers, and the results are as follows Figure 6 and Figure 7 shown.
[0096] Test Example 4
[0097] The test of fabric anti-ultraviolet performance is in accordance with GB / T 18830-2009.
[0098] As the number of coatings increases, the UPF value shows an upward trend, and the transmittance UVA value continues to decrease. When the number of coatings reaches 3 layers, the UVA value reaches the standard value of 5%. As the number of coatings increases, the UPF and transmittance UVA values tend to be stable. When the number of coatings is less than 3 times, as the number of coatings increases, the average percentage of UVA gradually decreases, while the UPF value shows an upward trend, because the Nano-Zno valence band electrons absorb ultraviolet light and undergo transitions, thereby shielding ultraviolet light.
[0099] When the number of coatings is 3, the UPF value has reached 192.4, far exceeding the UPF requirement of more than 50 stipulated in the national standard GB / T18830. At the same time, the transmittance UVA is 4.92%, which is less than the standard value of 5%, and also meets the national standard anti-ultraviolet standard. Continuing to increase the number of coatings, the fabric protection effect tends to be stable. Therefore, choosing three layers of coating is the best, which can not only achieve excellent anti-ultraviolet effect, meet the requirements of national standards, but also ensure the functionality of the fabric, taking into account its practicality and comfort. Figure 8 shown.
[0100] Test Example 5
[0101] The contact coolness coefficient test is in accordance with GB / T 35263-2017.
[0102] Concentration of cool finishing agent: The cool coefficient of polyester cotton will increase significantly with the increase of the concentration of cool finishing agent. When the concentration of cool finishing agent reaches 9%, the cool coefficient reaches the maximum value. As the concentration continues to increase, the cool coefficient gradually tends to a balanced state. When the concentration of cool finishing agent increases from 5% to 9%, the attachment and distribution of finishing agent molecules on the fabric gradually increase, which significantly improves the cool performance of the fabric. This is because the cool factor can be fixed to the inside of the fabric to form a more uniform and dense coating, thereby increasing the cool coefficient of the fabric. When the concentration of the finishing agent exceeds 9%, the increasing trend of the cool coefficient of the fabric begins to become less obvious. This may be because the finishing agent molecules on the surface and inside of the fabric are close to saturation and can no longer accommodate more finishing agent molecules. At this point, even if the finishing agent concentration continues to increase, it will not have a significant effect on the cool performance of the fabric. Therefore, the optimal finishing agent concentration is 9%. The results are as follows Fig. 9 shown.
[0103] Impregnation temperature: As the impregnation temperature increases, the coolness coefficient of the polyester cover cotton will increase significantly. When the finishing temperature reaches 60°C, the coolness coefficient reaches its maximum value. When the finishing temperature continues to increase, the coolness coefficient gradually decreases. When the finishing temperature is less than 60°C, the coolness coefficient continues to increase with the increase in temperature. This may be because the reaction and adsorption process of the cool finishing agent on the fabric is more active at high temperatures, allowing the effective ingredients to more fully combine with the fabric fibers. When the finishing temperature is greater than 60°C, excessively high processing temperatures may cause the mint essential oil components in the finishing agent to decompose or volatilize, and overheated water temperatures may damage the fibers, thereby affecting the cool effect. When the temperature is 60°C, the coolness coefficient reaches its maximum value. At this time, the cool factor of the finishing agent fully reacts and adsorbs with the fabric without causing decomposition or volatilization of the components. The results are as follows. Fig.10 shown.
[0104] Impregnation time: As the impregnation time increases, the coolness coefficient of the polyester cover cotton will gradually increase. When the impregnation time reaches 30 minutes, the coolness coefficient reaches its maximum value. As the impregnation time continues to increase, the coolness coefficient gradually tends to stabilize. When the impregnation time is less than 30 minutes, the finishing agent molecules have enough time to penetrate into the fabric, fully contact and react with the fibers, thereby forming a more uniform and stable coating. This causes the coolness coefficient of the fabric to gradually increase because more cool factors are fixed to the fabric, increasing its surface energy and coolness performance. When the impregnation time exceeds 30 minutes, the increasing trend of the fabric coolness coefficient will tend to be flat. This is because the finishing agent molecules have fully penetrated into the fabric at this time and have reached a saturated state with the fibers. Continuing to extend the impregnation time will not significantly increase the amount of finishing agent molecules attached to the fabric, so the coolness coefficient of the fabric tends to stabilize or slightly decrease. The results are as follows. Fig.11 shown.
[0105] In summary, the functional polyester-covered cotton fabric prepared by the preparation method of the present invention has a hydrophobic layer contact angle of 149.3° and a hydrophilic layer contact angle of 81.3°. After being immersed in a 9% cool finishing agent in a 60°C aqueous solution for 30 minutes, its cool feeling performance is improved from the original cool feeling coefficient of 0.064 to 0.219, and it has cool feeling performance. Compared with the untreated cotton fabric, the anti-ultraviolet performance is improved from 7.32 to 192.41, and the UVA transmittance is reduced from 22.24% to 4.93%, so that the polyester-covered cotton fabric has excellent moisture conduction and cool and quick-drying properties.
[0106] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A method for preparing a functional polyester-covered cotton fabric, characterized in that: The preparation method comprises the following steps: S1, treating a polyester-covered cotton fabric substrate in a cool finishing agent; S2, mixing the nano zinc oxide and the dispersant and subjecting them to ultrasonic treatment to obtain a nano zinc oxide dispersion; S3, mixing the nano zinc oxide dispersion and the thickener, and coating the mixture on the first surface of the fabric substrate treated in step S1; S4, mixing the mixed solution obtained in step S3 with the fluorine-free waterproofing agent, and coating the mixture on the other surface of the fabric substrate treated in step S3.
2. According to the preparation method according to claim 1, in step S1, the weight of the fabric substrate is 180-220 g / m 2 The warp density is 280-320 strands / 10cm, and the weft density is 240-280 strands / 10cm.
3. According to the preparation method according to claim 1, in step S1, the cool finishing agent is COOL-MAX contact cool finishing agent; preferably, in step S1, the concentration of the cool finishing agent is 5-11 wt%.
4. According to the preparation method according to claim 1, in step S1, the soaking time is 20 to 35 minutes; preferably, in step S1, the soaking temperature is 50 to 80°C.
5. According to the preparation method according to claim 1, in step S2, the dispersant is sodium polynaphthalenesulfonate; the concentration of the dispersant is 0.6-1.0 g / L; preferably, in step S2, the mass ratio of the nano zinc oxide to the dispersant is 1:0.4-0.
7.
6. According to the preparation method according to claim 1, in step S2, the time of the ultrasonic treatment is 5 to 15 minutes; preferably, in step S2, the frequency of the ultrasonic treatment is 10 to 30 KHZ; preferably, the power of the ultrasonic treatment is 400 to 600 W.
7. According to the preparation method according to claim 1, in step S3, the thickener is PTF; preferably, in step S3, the concentration of the thickener is 2-4wt%; preferably, in step S3, the mass ratio of the nano zinc oxide dispersion and the thickener is 23-27:2; preferably, in step S3, the coating thickness is 450-550μm; preferably, the number of coatings in step S3 is 1-3 times.
8. According to the preparation method according to claim 1, in step S4, the fluorine-free waterproofing agent is PSY CONC; preferably, in step S4, the concentration of the fluorine-free waterproofing agent is 13-17wt%; preferably, in step S4, the mass ratio of the mixed liquid to the fluorine-free waterproofing agent is 23-27:2; preferably, the coating thickness is 450-550μm; preferably, in step S4, the number of coatings is 1 to 3 times.
9. A functional polyester-covered cotton fabric, characterized in that: Prepared by the preparation method according to any one of claims 1 to 8, the functional polyester-covered cotton fabric comprises: Fabric substrate; A cooling layer impregnated on the fabric substrate; A UV protection layer coated on one side of the first surface of the fabric substrate; A unidirectional moisture conducting layer is coated on the second surface of the fabric substrate.
10. Use of the functional polyester-covered cotton fabric prepared by the preparation method according to any one of claims 1 to 8 in the preparation of textile products.
Citation Information
Patent Citations
Fiber and fiber structure
CN102597344A
Biological intelligent healthcare garment
CN108606373A
Preparing method for unidirectional wet-conduction pure cotton fabric based on nano-zinc oxide
CN109778529A
Preparation method of multifunctional one-way moisture-conducting cotton fabric
CN110983760A
Breathable cool fabric and preparation method thereof
CN117403369A
Cited By
Processing method of fabric with ice-cold feeling
CN121653893A