Flexible microfiber bamboo-based composite material and preparation method thereof
By removing and modifying the bamboo matrix and combining with polyester film composite, the problem of insufficient flexibility of bamboo is solved, and flexible ultra-fiber bamboo-based composite materials are prepared, achieving high longitudinal and transverse tensile strength, suitable for flexibility In the packaging field, production costs have been reduced and application scope has been expanded.
Patent Information
- Application Number
- CN202411276950.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-05
AI Technical Summary
Bamboo is less flexible when cut in a thin manner, prone to cracking and breaking, and it is difficult to make plastic products of complex shapes, which limits its application in plastic substitutes.
By removing, modifying and combining the thin bamboo with cutting, the flexible ultra-fiber bamboo matrix composite material is prepared, and the matrix is removed by using alkaline hydrogen peroxide aqueous solution containing polymer aluminum chloride, and the modification treatment solution is used to remove the matrix. Water-based polyurethane and elastic UV photocuring resin are added, combined with nanocellulose, and ultrasonic treatment is carried out to improve the flexibility and mechanical properties of the material.
It overcomes the problem of easy cracking and damage of bamboo materials, improves the flexibility and mechanical properties of bamboo-based composite materials, and can make some plastic products with complex shapes, reduces production costs, and expands the application scope of "using bamboo instead of plastic".
Smart Images

Figure CN118893681A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bamboo-based composite materials and packaging materials, and particularly relates to a flexible ultra-fiber bamboo-based composite material and a preparation method thereof. Background Art
[0002] It takes hundreds of years or even longer for plastic to decompose, and harmful substances are released during the decomposition process, polluting the soil, water and air, causing serious damage to terrestrial and marine ecosystems. In order to deal with plastic pollution, the international community has successively introduced a series of plastic ban and restriction policies, encouraging the reduction of plastic consumption and promoting biodegradable plastic alternatives. Bamboo, as a green, renewable and degradable biomass material, has become one of the important choices for plastic substitutes.
[0003] "Replacing plastic with bamboo" is a sustainable alternative to plastic. Unlike the petroleum-based raw materials of traditional plastic products and the pollution they produce, bamboo grows quickly, matures quickly, and has excellent material properties. The natural cellulose of bamboo can be processed and treated to make materials that replace plastic. Not only is the resource renewable, but the bamboo cellulose material is also naturally degradable. Therefore, using bamboo as a green, low-carbon, renewable, and degradable biomass material to reduce the use of plastic from the source is an effective way to reduce plastic pollution. "Replacing plastic with bamboo" takes into account both ecological and economic benefits and presents broad development prospects.
[0004] At the same time, although bamboo has good mechanical properties and hardness, it has poor plasticity and is difficult to make plastic products with complex shapes. In order to promote the use of bamboo to replace plastic products, for special-shaped and curved plastic products on the market, if we want to "replace plastic with bamboo", we must solve the problem that thinly sliced bamboo has poor flexibility and is easy to crack and break. Further research and improvement is still needed in terms of cost, processing and molding technology. Summary of the invention
[0005] In view of the content of the background technology, the purpose of the present invention is to provide a flexible ultra-fine bamboo-based composite material and a preparation method thereof. The present invention sequentially removes the matrix, performs modification treatment, and composites a polyester film on sliced thin bamboo to prepare a bamboo-based composite material with excellent mechanical properties and flexibility, which overcomes the shortcomings of existing bamboo materials, expands the application scope of "replacing plastic with bamboo", and has a good market prospect.
[0006] In order to achieve the above object, the present invention specifically adopts the following technical solutions: The present invention provides a method for preparing a flexible ultra-fine bamboo-based composite material, comprising the following steps: Step 1: Take fresh bamboo, segment it, remove the green and yellow parts, steam it, and then process it into thin sliced bamboo for later use; Step 2: removing the matrix from the sliced thin bamboo using a treatment agent; Step 3: Immerse the thin bamboo after removing the matrix into the modified treatment solution; Step 4: Use polyester film to composite the modified thin bamboo to obtain a flexible ultra-thin bamboo-based composite material.
[0007] Preferably, in step 1, fresh bamboo is used as the substrate, and the thickness of the sliced thin bamboo obtained is 0.1-0.4 mm.
[0008] Preferably, the treatment agent used for the matrix removal in step 2 is an alkaline hydrogen peroxide aqueous solution containing polyaluminium chloride; the treatment temperature for matrix removal is 75-90°C, and the treatment time is 8-11 h.
[0009] Preferably, the alkaline aqueous hydrogen peroxide solution contains 1.5%-2.5% NaOH, 1%-1.3% H2O2 and 0.1%-0.12% polyaluminium chloride.
[0010] The present invention takes micro-thin bamboo as the research object, analyzes the influence of treatment agent type, temperature and time on the microstructure and physical properties of micro-thin bamboo after matrix removal, and adopts alkaline hydrogen peroxide aqueous solution containing polyaluminium chloride to effectively remove lignin and hemicellulose without damaging the bamboo fiber structure.
[0011] Preferably, the modified treatment liquid in step three is composed of waterborne polyurethane and elastic UV light-curing resin, into which nanocellulose is also added.
[0012] Preferably, the modified treatment liquid comprises, by weight, 100 parts of waterborne polyurethane, 9-12 parts of elastic UV light-curable resin, and 0.3-0.6 parts of nanocellulose.
[0013] Preferably, in step 3, the treatment temperature of the micro-thin bamboo being immersed in the modified treatment solution is 60-72° C. for 4-8 h, and ultrasonic treatment is also applied during the process.
[0014] In view of the problem that bamboo-based composite materials have poor transverse strength and are easy to crack and break, the current field mostly adopts the method of criss-cross assembly. However, this processing method is complicated, takes a long time to process, and the production cost is significantly increased. The high price is also a key factor affecting the application scope of "replacing plastic with bamboo". Based on this, the present invention provides a modified treatment liquid to further process the thin bamboo after the matrix is removed: the water-based polyurethane can penetrate into the gaps between the thin bamboo fibers after the matrix is removed, thereby increasing the flexibility of the thin bamboo; the elastic UV light-curing resin contains active functional groups, which can improve the stress cracking resistance of the thin bamboo on the one hand, and on the other hand, it can build a stable network structure with the water-based polyurethane and bamboo fibers, thereby facilitating the penetration and embedding of nanocellulose into it to form a dense system, so that the nanocellulose can be densely distributed in the bamboo fibers, as an unoriented "reinforcement rib" to evenly disperse the stress load on the material, thereby greatly improving the mechanical properties of the material; ultrasonic treatment promotes the uniform dispersion of nanocellulose. The present invention does not require complex processing technology for crisscrossing blank assembly. The dense network system constructed by the modified treatment liquid can greatly improve the lateral strength of the material, effectively overcoming the problem that the bamboo-based composite material is easy to crack and break.
[0015] Preferably, the polyester film in step 4 is a polyethylene terephthalate film, and the composite molding adopts a hot pressing molding process, and the hot pressing conditions are 120° C. and 0.6 MPa. The present invention also uses polyethylene terephthalate film to further hot press composite molding of micro-thin bamboo, which has good stability and can further improve the mechanical properties of the composite material, and finally obtains a bamboo-based composite material suitable for the field of flexible packaging.
[0016] The present invention also provides application of the flexible ultra-fiber bamboo-based composite material obtained by the preparation method in replacing plastic packaging.
[0017] Compared with the prior art, the present invention has the following beneficial effects: 1. The flexible ultra-fiber bamboo-based composite material of the present invention has good flexibility and can be used to produce some plastic products with complex shapes.
[0018] 2. The flexible ultra-fine bamboo-based composite material of the present invention has good longitudinal and transverse tensile strength, overcoming the shortcomings of existing bamboo materials.
[0019] 3. The present invention provides a new material option for "replacing plastic with bamboo", and the preparation process is simple, the cost is low, and it is suitable for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an appearance diagram of the product sample prepared in Example 1 of the present invention.
[0021] Figure 2 This is an appearance diagram of the product sample prepared in Comparative Example 1 of the present invention.
[0022] Figure 3 This is an appearance diagram of the product sample prepared in Comparative Example 2 of the present invention.
[0023] Figure 4 This is an appearance diagram of the product sample prepared in Comparative Example 3 of the present invention.
[0024] Figure 5 This is an appearance diagram of the product sample prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme of the present invention will be clearly and completely described below in conjunction with the embodiments. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.
[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0027] Example 1 A method for preparing a flexible ultra-fine bamboo-based composite material, comprising: 1. Prepare an alkaline hydrogen peroxide aqueous solution (containing 2% NaOH, 1.2% H2O2 and 0.1% polyaluminium chloride) as a treatment agent. Take 100 parts by weight of waterborne polyurethane (organic silicon modified waterborne polyurethane 6755, solid content 32%) and 9.5 parts by weight of elastic UV light curing resin (Lan Kelu L-8200, active ingredient 95%) and mix them evenly, add 0.5 parts by weight of nanocellulose (CNF-H1, L: 1-20 μm, D: 20-80 nm) into the resulting mixed solution, and evenly disperse to obtain a modified treatment solution.
[0028] 2. Take fresh bamboo segments (1.5 m), remove the green and yellow parts, and then steam them to make sliced thin bamboo with a thickness of 0.25 mm; soak the sliced thin bamboo in an alkaline hydrogen peroxide solution, heat it to 80℃, and keep it for 10 hours, then take out the thin bamboo, wash it, and dry it to a moisture content of 10% to obtain the thin bamboo with the matrix removed.
[0029] 3. Heat the modified treatment liquid to 65°C, take the micro-thin bamboo with the matrix removed and immerse it in the modified treatment liquid, continue to stir appropriately for 6 hours, apply 35 W ultrasound for 1 min every 30 minutes during the process, take out and dry after the treatment; evenly apply a layer of epoxy resin adhesive (EP 3628B) on the surface of the obtained micro-thin bamboo, and then cover the surface with polyethylene terephthalate film (thickness 0.1 mm), and then send it into a hot press after bonding, and hot press it at 120°C and 0.6 MPa to obtain a flexible ultra-thin bamboo-based composite material.
[0030] Example 2 A method for preparing a flexible ultra-fine bamboo-based composite material, comprising: 1. Prepare an alkaline hydrogen peroxide aqueous solution (containing 1.5% NaOH, 1% H2O2 and 0.1% polyaluminium chloride) as a treatment agent. Take 100 parts by weight of waterborne polyurethane (organic silicon modified waterborne polyurethane 6755, solid content 32%) and 11.5 parts by weight of elastic UV light curing resin (Lan Kelu L-8200, active ingredient 95%) and mix them evenly, add 0.5 parts by weight of nanocellulose (CNF-H1, L: 1-20 μm, D: 20-80 nm) into the resulting mixed solution, and evenly disperse to obtain a modified treatment solution.
[0031] 2. Take fresh bamboo segments (1.5 m), remove the green and yellow parts, and then steam them to make sliced thin bamboo with a thickness of 0.25 mm; soak the sliced thin bamboo in an alkaline hydrogen peroxide solution, heat it to 85℃, and keep it for 8 hours, then take out the thin bamboo, wash it, and dry it to a moisture content of 10% to obtain the thin bamboo with the matrix removed.
[0032] 3. Heat the modified treatment liquid to 70°C, take the micro-thin bamboo with the matrix removed and immerse it in the modified treatment liquid, continue to stir appropriately for 5 hours, apply 35 W ultrasound for 1 minute every 30 minutes during the process, take out and dry after the treatment; evenly apply a layer of epoxy resin adhesive (EP 3628B) on the surface of the obtained micro-thin bamboo, and then cover the surface with polyethylene terephthalate film (thickness 0.1 mm), and then send it into a hot press after bonding, and hot press it at 120°C and 0.6 MPa to obtain a flexible ultra-thin bamboo-based composite material.
[0033] Example 3 A method for preparing a flexible ultra-fine bamboo-based composite material, comprising: 1. Prepare an alkaline hydrogen peroxide aqueous solution (containing 2.5% NaOH, 1.2% H2O2 and 0.12% polyaluminium chloride) as a treatment agent. Take 100 parts by weight of waterborne polyurethane (organic silicon modified waterborne polyurethane 6755, solid content 32%) and 10 parts by weight of elastic UV light curing resin (Lan Kelu L-8200, active ingredient 95%) and mix them evenly, add 0.6 parts by weight of nanocellulose (CNF-H1, L: 1-20 μm, D: 20-80 nm) into the resulting mixed solution, and evenly disperse to obtain a modified treatment solution.
[0034] 2. Take fresh bamboo segments (1.5 m), remove the green and yellow parts, and then steam them to make sliced thin bamboo with a thickness of 0.25 mm; soak the sliced thin bamboo in an alkaline hydrogen peroxide solution, heat it to 80℃ for 9 hours, then take out the thin bamboo, wash it, and dry it to a moisture content of 10% to obtain the thin bamboo with the matrix removed.
[0035] 3. Heat the modified treatment liquid to 62°C, take the micro-thin bamboo with the matrix removed and immerse it in the modified treatment liquid, continue to stir appropriately for 8 h, apply 35 W ultrasound for 1 min every 30 min during the process, take out and dry after the treatment; evenly apply a layer of epoxy resin adhesive (EP 3628B) on the surface of the obtained micro-thin bamboo, and then cover the surface with polyethylene terephthalate film (thickness 0.1 mm), and then send it into a hot press after bonding, and hot press it at 120°C and 0.6 MPa to obtain a flexible ultra-thin bamboo-based composite material.
[0036] Comparative Example 1 Referring to the step parameters in Example 1, the difference is that no polyaluminium chloride is added to the treating agent; that is, an alkaline hydrogen peroxide aqueous solution (containing 2% NaOH and 1.2% H2O2) is prepared as the treating agent.
[0037] Comparative Example 2 Refer to the step parameters in Example 1, except that no nanocellulose is added to the modified treatment liquid; that is, 100 parts by weight of water-based polyurethane (silicone-modified water-based polyurethane 6755, solid content 32%) and 9.5 parts by weight of elastic UV light-curing resin (Lancolu L-8200, active ingredient 95%) are mixed and used as the modified treatment liquid.
[0038] Comparative Example 3 Referring to the step parameters in Example 1, the difference is that no elastic UV light-curing resin is added to the modified treatment liquid; that is, 100 parts by weight of water-based polyurethane (silicone-modified water-based polyurethane 6755, solid content 32%) is taken, and 0.5 parts by weight of nanocellulose (CNF-H1, L: 1-20 μm, D: 20-80 nm) is added thereto and uniformly dispersed as the modified treatment liquid.
[0039] Comparative Example 4 Refer to the step parameters in Example 1, except that ultrasound is not applied during the immersion and stirring of the modified treatment liquid.
[0040] The appearance of the samples prepared in Comparative Examples 1-4 is as follows: Figure 1-Figure 5 .
[0041] Test example The performance of the bamboo-based composite material samples prepared in the above embodiments and comparative examples was tested (LY / T 2879-2017), and the results are shown in Table 1.
[0042] After the decorative veneer material is wound around a circular steel tube of a certain diameter for one circle, observe whether there are cracks on the surface of the decorative veneer material. The minimum steel tube diameter reached by the flexible ultra-fiber bamboo-based composite material is used as the flexibility index.
[0043] Table 1
[0044] To sum up the above, it can be seen that the flexible ultra-fiber bamboo-based composite material prepared by the present invention has good longitudinal and transverse tensile strength, and also has excellent flexibility, which overcomes the defects of existing bamboo-based composite materials and can meet the performance requirements in the field of flexible packaging; at the same time, the preparation process of the present invention is simple and the cost is low, which can expand the application scope of "replacing plastic with bamboo" and has good market prospects.
[0045] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a flexible ultra-fine bamboo-based composite material, characterized in that: The steps include: Step 1: Take fresh bamboo, segment it, remove the green and yellow parts, steam it, and then process it into thin sliced bamboo for later use; Step 2: removing the matrix from the sliced thin bamboo using a treatment agent; Step 3: Immerse the thin bamboo after removing the matrix into the modified treatment solution; Step 4: Use polyester film to composite the modified thin bamboo to obtain a flexible ultra-thin bamboo-based composite material.
2. The method for preparing a flexible ultra-fine bamboo-based composite material according to claim 1, characterized in that: In step 1, fresh bamboo is used as the base material, and the thickness of the obtained sliced thin bamboo is 0.1-0.4 mm.
3. The method for preparing a flexible ultra-fine bamboo-based composite material according to claim 1, characterized in that: The treatment agent used for the matrix removal in step 2 is an alkaline hydrogen peroxide aqueous solution containing polyaluminium chloride; the treatment temperature for matrix removal is 75-90°C and the treatment time is 8-11 h.
4. The method for preparing a flexible ultra-fiber bamboo-based composite material according to claim 3, characterized in that: The alkaline hydrogen peroxide aqueous solution contains 1.5%-2.5% NaOH, 1%-1.3% H2O2 and 0.1%-0.12% polyaluminium chloride.
5. The method for preparing a flexible ultra-fiber bamboo-based composite material according to claim 1, characterized in that: The modified treatment liquid in step 3 is composed of water-based polyurethane and elastic UV light-curing resin, and nanocellulose is also added therein.
6. The method for preparing a flexible ultra-fiber bamboo-based composite material according to claim 5, characterized in that: The modified treatment liquid comprises, by weight, 100 parts of waterborne polyurethane, 9-12 parts of elastic UV light-curing resin, and 0.3-0.6 parts of nanocellulose.
7. The method for preparing a flexible ultra-fiber bamboo-based composite material according to claim 1, characterized in that: In step 3, the treatment temperature of the micro-thin bamboo being immersed in the modified treatment solution is 60-72° C. and the time is 4-8 h, and ultrasonic treatment is also applied during the process.
8. The method for preparing a flexible ultra-fine bamboo-based composite material according to claim 1, characterized in that: The polyester film in step 4 is a polyethylene terephthalate film, and the composite molding adopts a hot pressing molding process, and the hot pressing conditions are 120° C. and 0.6 MPa.
9. The flexible ultra-fiber bamboo-based composite material obtained by the preparation method according to any one of claims 1 to 8.
10. Application of the flexible ultra-fiber bamboo-based composite material obtained by the preparation method according to any one of claims 1 to 8 in replacing plastic packaging.
Citation Information
Patent Citations
Preparation method for nanometer cellulose composite waterborne polyurethane paint film on wood surface
CN103320003A
Enhancement processing method for sliced thin bamboo veneer
CN107214794A
Preparation method of water-resistant, oil-resistant and anti-falling bamboo fiber environment-friendly meal box
CN111702886A
Preparation method of high-strength flexible transparent bamboo wood
CN114851323A
Manufacturing method of bamboo decorative veneer material
CN118081933A
Cited By
Flexible composite material and preparation method thereof
CN119319598A
Flexible composite material and method for producing the same
CN119319598B
Ultrathin foldable flexible composite material and preparation method thereof
CN119820944A
High-performance soft composite material and preparation method thereof
CN119820945A
Production method of environment-friendly flexible flattened bamboo veneer
CN120023894A