Electromagnetic shielding and antibacterial multifunctional polyamide fiber and preparation method thereof

By using new pre-treatment processes and electroless plating methods on textiles, the deficiencies in radiation protection and antibacterial properties of textiles are solved, and multi-functional effects of electromagnetic shielding, antibacterial and water repellency are achieved, and the application scope of nylon fiber is expanded, reducing the cost of Environmental pollution and friction losses.

CN118745658AInactive Publication Date: 2024-10-08ZHEJIANG UNIV OF TECH TONGXIANG RES INST CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410788094.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing textiles have deficiencies in radiation protection and antibacterial properties, and the traditional chemical silver plating process causes heavy environmental pollution and low coating adhesion, which limits its application scope.

Method used

Using a simple and green new pre-treatment process surface modification technology, catecholethylamine is used to replace stannous chloride and palladium chloride to pre-treat nylon fibers, and electroless silver plating is used to improve the silver plating layer. The strong bonding with fibers simplifies the silver plating process and reduces heavy metal pollution.

Benefits of technology

It achieves the electromagnetic shielding, antibacterial, and water-repellent multi-functional effects of the fiber, expands the application scope of nylon fiber, reduces friction loss, and improves the wearing style of the product while being healthy and environmentally friendly.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of textiles, and particularly relates to an electromagnetic shielding and antibacterial multifunctional polyamide fiber and a preparation method thereof. Specifically, polyamide fabric is selected as a base material, and a chemical plating pretreatment process is a simple and green novel pretreatment process surface modification technology, namely, catechol ethylamine is used for pretreatment of polyamide fiber. The chemical plating comprises the following steps of alcohol washing, water washing, acid pickling, water washing, surface modification, water washing, chemical silver plating, water washing and drying. According to the invention, catechol ethylamine with high adhesion and non-toxicity and harmlessness can be deposited on almost all matrix surfaces, the chemical plating process is simplified, the heavy metal pollution is reduced, and an intermediate carrier for connecting a base material and silver is provided, so that the fiber obtains a new surface containing active groups, and the surface of the fiber is improved. And the bonding strength between the silver plating layer and the fiber can be better improved. While being healthy and environment-friendly, the fiber is endowed with a special style, so that the multifunctional effects of electromagnetic shielding, antibiosis and water repellency are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textiles, and specifically relates to an electromagnetic shielding, antibacterial multifunctional nylon fiber and a preparation method thereof. Background Art

[0002] As the electronics industry continues to develop, people's lives and work are becoming more and more convenient, but it cannot be ignored that people are exposed to more and more serious radiation. How to reduce the impact of radiation on people is a very important research topic at present. Textiles, as people's main clothing, can be used as an important carrier to prevent radiation. Based on this, the research on radiation-proof textiles has attracted attention. Moreover, textiles will inevitably be contaminated to a certain extent during wearing and use. These pollution sources (such as sweat and fatty acids, etc.) can provide a good environment for the growth of microorganisms. If microorganisms exist in textiles for a long time, it is likely to affect the properties of the textiles themselves. In addition, long-term exposure to pollutants will also cause textiles to have odors. The antibacterial finishing of textiles is an issue that must be explored in the current industry.

[0003] Chemical silver plating is a traditional silver plating method with a long history of development. Silver-plated textiles are multifunctional materials that integrate multiple functions. Chemical silver plating is widely used in electromagnetic shielding, smart textiles, antibacterial materials, conductive materials and other fields. The chemical silver plating steps are usually divided into three stages: pretreatment, chemical silver plating and post-treatment. At present, there are three pretreatment processes. The first is the most traditional palladium-catalyzed pretreatment process, which has been industrialized. It includes four steps: cleaning, roughening, sensitization and activation; the second process includes two steps: cleaning and surface modification; this method is effective, simple and environmentally friendly, and is the development direction of silver plating pretreatment. The third includes cleaning, roughening and surface modification. The addition of the roughening step is to increase the surface energy and surface activity of the fiber, but it will damage the mechanical properties of the fiber. Chemical silver plating is the fastest-growing surface treatment technology with high all-plating ability. The obtained coating has good wear resistance, excellent corrosion resistance and high hardness. The traditional stannous chloride sensitization and palladium-catalyzed pretreatment chemical silver plating have a general silver plating effect on the silver-plated fiber prepared; and it has a large environmental pollution. Only a coating that meets general requirements can be obtained, and the coating bonding strength is low, which to a certain extent limits the application of its products.

[0004] Nylon fiber is the first to be industrialized among the three major synthetic fibers. Its output is second only to polyester and its cost is low. There are a large number of hydrogen bonds between macromolecules, which results in strong intermolecular forces and high strength. Its end groups contain amino and carboxyl groups and have certain activity. It has good resilience and the best wear resistance among synthetic fibers. Based on these advantages, nylon is a commonly used chemical silver-plated fiber substrate for textiles.

[0005] Therefore, how to prepare an electromagnetic shielding, antibacterial multifunctional nylon fiber is a technical problem to be solved at present. Summary of the invention

[0006] The present invention has developed an electromagnetic shielding, antibacterial multifunctional nylon fiber and a preparation method thereof. The present invention uses nylon fiber as the research object, uses chemical plating to silver-plate the surface of nylon fiber, and uses catechol ethylamine instead of stannous chloride and palladium chloride to pre-treat the fiber. The new pre-treatment process uses a simple and green new pre-treatment process surface modification technology, which can be deposited on almost all substrate surfaces by utilizing its high adhesion and non-toxicity. This method is used to expand the application scope of silver-plated fibers, simplify the chemical plating process, and reduce heavy metal pollution, and provide an intermediate carrier connecting the substrate and silver, so that the fiber obtains a new surface containing active groups, which can better improve the bonding strength between the silver-plated layer and the fiber, thereby reducing the friction loss of the functional medium during the use of the fiber. While being healthy and environmentally friendly, the fiber is given a special wearing style, so that it can achieve the multifunctional effects of electromagnetic shielding, antibacterial, and water repellent.

[0007] The present invention provides the following technical solution: a preparation method of electromagnetic shielding and antibacterial multifunctional nylon fiber proposed by the present invention, specifically, nylon fabric is selected as the substrate, and the chemical plating pretreatment process uses a simple and green new pretreatment process surface modification technology, that is, catechol ethylamine is used to pretreat the nylon fiber, and the chemical plating of the present invention includes the following steps: alcohol washing → water washing → acid washing → water washing → surface modification → water washing → chemical silver plating → water washing → drying.

[0008] Preferably, the alcohol washing process is 25-40 g / L anhydrous ethanol, the temperature is 20-30°C, and the time is 20-30 min; the acid washing process is 2-6% hydrochloric acid (HCl), the temperature is 20-30°C, and the time is 30-90 min.

[0009] Preferably, the surface modification process is catechol ethylamine concentration 1-4 g / L, hydrogen peroxide (H2O2) 0.6 ml / L, anhydrous copper sulfate (CuSO4·5H2O) 0.6-2.4 g / L, temperature 20-30 °C, time 30-120 min, and pH value adjusted to 8-10.

[0010] Preferably, the chemical silver plating solution comprises the following components: 5-8 g / L of silver salt, 5-10 g / L of complexing agent, 8-14 g / L of reducing agent, alkaline pH adjusting agent, 0.1-0.3 g / L of stabilizer, and 50-200 ml / L of surfactant.

[0011] Preferably, the silver salt is silver nitrate (AgNO3) to provide silver ions; the complexing agent is selected from one or a mixture of ethylenediaminetetraacetic acid and tartrate; the reducing agent can be selected from formaldehyde (HCHO), glucose (C6H 12 O6).

[0012] Preferably, the alkaline pH regulator is selected from one of sodium hydroxide and potassium hydroxide, and the pH value is adjusted to 11-13. By increasing the pH value of the plating solution, the stability of the plating solution is improved, which is beneficial to the deposition of silver ions.

[0013] Preferably, the main purpose of the stabilizer is to slow down the decomposition of the chemical silver plating solution due to its own instability. The stabilizer suitable for the present invention can be selected from gelatin, thiourea (CH4N2S), sodium iodide (NaI), potassium iodide (KI), and Cu 2+ 、Co 2+ 、Ni 2+ Salt, etc., slows down the self-decomposition of the silver plating solution, not only has a good stabilizing effect but also plays a role in refining the crystals and increasing the ductility of the coating.

[0014] Preferably, the surfactant is selected from one of ethanol (C2H5OH), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), and polyethylene glycol (PEG) to improve the uniformity and density of silver plating.

[0015] The present invention also provides an electromagnetic shielding and antibacterial multifunctional nylon fiber, which is prepared by the above-mentioned preparation method.

[0016] The invention greatly expands the application field of nylon fiber and develops an electromagnetic shielding and antibacterial multifunctional nylon fiber, which is of great significance to the wide application and development of nylon fiber.

[0017] Compared with the prior art, the present invention has the following outstanding and beneficial technical effects: (1) The present invention uses catechol ethylamine instead of stannous chloride and palladium chloride to pre-treat the fiber, taking advantage of its high adhesion and non-toxicity, and using a simple and green new pre-treatment process surface modification technology to simplify the chemical plating process and reduce heavy metal pollution. It also provides an intermediate carrier connecting the substrate and silver, so that the fiber obtains a new surface containing active groups, which can better improve the bonding strength between the silver-plated layer and the fiber, thereby reducing the friction loss of the conductive functional medium during the use of the fiber.

[0018] (2) While being healthy and environmentally friendly, nylon fiber is endowed with a special wearing style, achieving the multifunctional effects of electromagnetic shielding, antibacterial and water repellent, thus expanding the application range of the fiber; DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0020] It should be noted that the words "front", "rear", "left", "right", "up" and "down" used in the following description refer to directions in the scheme, and the words "inside" and "outside" refer to directions toward or away from the geometric center of a specific component, respectively.

[0021] The present invention provides a method for preparing electromagnetic shielding and antibacterial multifunctional nylon fiber, comprising the following steps: 1) Alcohol washing: Place a certain amount of nylon fiber in a 25-40 g / L anhydrous ethanol solution for degreasing, stir electrically at 20-30 °C for 20-30 min, and the speed during electric stirring is 750 r / min. After degreasing, rinse the nylon fiber with deionized water to remove the residual solution; 2) Pickling: Immerse the fiber after alcohol washing in step 1 in 1~6% HCl solution at room temperature and perform ultrasonic cleaning for 30~90 min. The purpose of acid washing is to remove impurities on the fiber surface. Then use distilled water for 30 min ultrasonic cleaning to clean the chloride ions on the fiber surface to prevent the subsequent formation of white precipitates with AgNO3 and contamination of the plating solution. Put the cleaned fiber into an electric hot air drying oven and dry it at 60 ℃ for 4 h; 3) Weigh 0.6 ml / L H2O2, 0.6~2.4 g / L CuSO4·5H2O and 1~4 g / L catechol ethylamine to prepare a solution, slowly add an appropriate amount of tris(hydroxymethyl)aminomethane powder and 10 g / L sodium hydroxide solution to adjust the pH of the modified solution to 8~10, and the preparation of the catechol ethylamine modified solution is complete. Put the weighed nylon fiber treated in step 2 into the prepared catechol ethylamine solution, and react for 30~120 minutes at 20~30 ℃, 150 r / min, and a bath ratio of 1:25; use distilled water to thoroughly wash the modified nylon fiber to pH=7, remove the residual solution, and then dry it in an electric hot air drying oven at 60 ℃ for use; 4) Preparation of silver ammonia solution: Weigh 5-8 g AgNO3, dissolve it in 1 L of distilled water, and slowly add 50 ml / L ammonia water with a rubber-tipped dropper. Brown silver oxide (Ag2O) precipitates appear in the clear silver nitrate solution. Continue to add until the precipitated Ag2O precipitate is completely dissolved and the solution becomes clear. Next, adjust the pH to 9-12 with 10 g / L sodium hydroxide solution. A small amount of precipitate will appear in the solution at this time. Continue to add ammonia water until the solution is clear. At this time, a silver ammonia solution is obtained. 5) Preparation of reducing solution: weigh 8-14 g C6H 12 O6 and 5-10 g tartaric acid were dissolved in 1 L distilled water, and then boiled in an electric ceramic stove for 15 min. The addition of tartaric acid was to make the glucose conversion complete. After cooling, 50-200 ml / L of anhydrous ethanol solution was added to replenish the excess water evaporated to reach the original solution volume of 1 L, thus obtaining a reduced solution. 6) Chemical silver plating operation: The bath ratio of modified nylon fiber to silver plating solution is 1:25. The modified nylon fiber after step 3 is immersed in the silver ammonia solution prepared in step 4 for 10 minutes. Then, the reducing solution prepared in step 5 is slowly and evenly added at a volume ratio of 1:1. The slow addition is to control the reduction rate of silver. Stir with a magnetic stirrer at 1000 r / min and 25-40 ℃ to allow it to react fully until the fiber is completely silver-plated, which takes about 30 minutes; 7) Then, the silver-plated fiber after finishing in step 6 is taken out, washed with distilled water for several times, and dried in a vacuum drying oven at 40° C. to obtain an electromagnetic shielding and antibacterial multifunctional nylon fiber.

[0022] According to the above preparation method, further description is given in combination with specific examples as follows: Example 1

[0023] The preparation process of this example is as follows: 1) Alcohol washing (30 g / L anhydrous ethanol, temperature 25 °C, time 25 min) → water washing → acid washing (4% HCl, temperature 25 °C, time 45 min) → water washing → surface modification → water washing → chemical silver plating → water washing → drying; 2) Weigh 0.6 ml / L H2O2, 1.8 g / L CuSO4·5H2O and 3 g / L catechol ethylamine to prepare a solution, slowly add an appropriate amount of trimethylolaminomethane powder and 10 g / L sodium hydroxide solution to adjust the pH of the modified solution to 8.5, and the preparation of the catechol ethylamine modified solution is completed. The acid-washed nylon fiber is placed in the solution for surface modification, and reacted for 120 min at 25 ℃, 150 r / min, and a bath ratio of 1:25; the modified nylon fiber is thoroughly washed with distilled water to pH = 7, the residual solution is removed, and then dried in an electric hot air drying oven at 60 ℃ for use; 3) Preparation of silver ammonia solution: Weigh 8 g of AgNO3 and dissolve it in 1 L of distilled water. Use a rubber-tipped dropper to slowly add 50 ml / L of ammonia water. Brown Ag2O precipitate will appear in the clear AgNO3 solution. Continue to add until the precipitated Ag2O precipitate is completely dissolved and the solution becomes clear. Next, adjust the pH to 11 with 10 g / L sodium hydroxide solution. A small amount of precipitate will appear in the solution. Continue to add ammonia water until the solution is clear. At this time, a silver ammonia solution is obtained. 4) Preparation of reducing solution: weigh 12 g C6H 12 O6 and 5 g tartaric acid were dissolved in 1 L distilled water, and then boiled in an electric ceramic stove for 15 min. After cooling, 50 ml / L anhydrous ethanol solution was added to make the original solution volume reach 1 L, thus obtaining a chemical plating reduction solution; 5) Chemical silver plating operation: The bath ratio of modified nylon fiber to silver plating solution is 1:25. The modified fiber is immersed in the prepared silver ammonia solution for activation for 10 minutes. Then the prepared reducing solution is slowly added at a volume ratio of 1:1 at a uniform rate. At 1000r / min and 40°C, a magnetic stirrer is used to stir the fiber to fully react until the fiber is completely silver-plated, which takes about 30 minutes. Then it is fully washed with distilled water several times and dried in a vacuum drying oven at 40°C to obtain an electromagnetic shielding, antibacterial multifunctional nylon fiber. Example 2

[0024] The preparation process of this example is as follows: 1) Alcohol washing (30 g / L anhydrous ethanol, temperature 25 °C, time 25 min) → water washing → acid washing (4% HCl, temperature 25 °C, time 45 min) → water washing → surface modification → water washing → chemical silver plating → water washing → drying; 2) Weigh 0.6 ml / L H2O2, 2.4 g / L CuSO4·5H2O and 4 g / L catechol ethylamine to prepare a solution, slowly add an appropriate amount of trimethylolaminomethane powder and 10 g / L sodium hydroxide solution to adjust the pH of the modified solution to 8.5, and the preparation of the catechol ethylamine modified solution is completed. The acid-washed nylon fiber is placed in the solution for surface modification, and reacted for 120 min at 25 ℃, 150 r / min, and a bath ratio of 1:25; the modified nylon fiber is thoroughly washed with distilled water to pH = 7, the residual solution is removed, and then dried in an electric hot air drying oven at 60 ℃ for use; 3) Preparation of silver ammonia solution: Weigh 8 g of AgNO3 and dissolve it in 1 L of distilled water. Use a rubber-tipped dropper to slowly add 50 ml / L of ammonia water. Brown Ag2O precipitate will appear in the clear AgNO3 solution. Continue to add until the precipitated Ag2O precipitate is completely dissolved and the solution becomes clear. Next, adjust the pH to 11 with 10 g / L sodium hydroxide solution. A small amount of precipitate will appear in the solution. Continue to add ammonia water until the solution is clear. At this time, a silver ammonia solution is obtained. 4) Preparation of reducing solution: weigh 12 g C6H 12 O6 and 5 g tartaric acid were dissolved in 1 L distilled water, and then boiled in an electric ceramic stove for 15 min. After cooling, 50 ml / L anhydrous ethanol solution was added to make the original solution volume reach 1 L, thus obtaining a chemical plating reduction solution; 5) Chemical silver plating operation: The bath ratio of modified nylon fiber to silver plating solution is 1:25. The modified fiber is immersed in the prepared silver ammonia solution for activation for 10 minutes. Then the prepared reducing solution is slowly added at a volume ratio of 1:1 at a uniform rate. At 1000r / min and 40°C, a magnetic stirrer is used to stir the fiber to fully react until the fiber is completely silver-plated, which takes about 30 minutes. Then it is fully washed with distilled water several times and dried in a vacuum drying oven at 40°C to obtain an electromagnetic shielding, antibacterial multifunctional nylon fiber. Example 3

[0025] The preparation process of this example is as follows: 1) Alcohol washing (30 g / L anhydrous ethanol, temperature 25 °C, time 25 min) → water washing → acid washing (4% HCl, temperature 25 °C, time 45 min) → water washing → surface modification → water washing → chemical silver plating → water washing → drying; 2) Weigh 0.6 ml / L H2O2, 1.8 g / L CuSO4·5H2O and 3 g / L catechol ethylamine to prepare a solution, slowly add an appropriate amount of trimethylolaminomethane powder and 10 g / L sodium hydroxide solution to adjust the pH of the modified solution to 8.5, and the preparation of the catechol ethylamine modified solution is completed. The acid-washed nylon fiber is placed in the solution for surface modification, and reacted for 120 min at 25 ℃, 150 r / min, and a bath ratio of 1:25; the modified nylon fiber is thoroughly washed with distilled water to pH = 7, the residual solution is removed, and then dried in an electric hot air drying oven at 60 ℃ for use; 3) Preparation of silver ammonia solution: Weigh 8 g of AgNO3 and dissolve it in 1 L of distilled water. Use a rubber-tipped dropper to slowly add 50 ml / L of ammonia water. Brown Ag2O precipitate will appear in the clear AgNO3 solution. Continue to add until the precipitated Ag2O precipitate is completely dissolved and the solution becomes clear. Next, adjust the pH to 11 with 10 g / L sodium hydroxide solution. A small amount of precipitate will appear in the solution. Continue to add ammonia water until the solution is clear. At this time, a silver ammonia solution is obtained. 4) Preparation of reducing solution: weigh 14 g C6H 12 O6 and 10 g tartaric acid were dissolved in 1 L distilled water, and then boiled in an electric ceramic furnace for 15 min. After cooling, 50 ml / L anhydrous ethanol solution was added to make the original solution volume reach 1 L, thus obtaining a chemical plating reduction solution; 5) Chemical silver plating operation: The bath ratio of modified nylon fiber to silver plating solution is 1:25. The modified fiber is immersed in the prepared silver ammonia solution for activation for 10 minutes. Then the prepared reducing solution is slowly added at a volume ratio of 1:1 at a uniform rate. At 1000r / min and 40°C, a magnetic stirrer is used to stir the fiber to fully react until the fiber is completely silver-plated, which takes about 30 minutes. Then it is fully washed with distilled water several times and dried in a vacuum drying oven at 40°C to obtain an electromagnetic shielding, antibacterial multifunctional nylon fiber.

[0026] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, material or apparatus including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, material or apparatus.

[0027] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing electromagnetic shielding and antibacterial multifunctional nylon fiber, Features: Specifically, nylon fabric is selected as the base material, and the following steps are performed on the base material in sequence: alcohol washing → water washing → acid washing → water washing → surface modification → water washing → chemical silver plating → water washing → drying.

2. A method for preparing an electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 1, It is characterized in that The alcohol washing process is to place a certain amount of nylon fiber into a 25-40 g / L anhydrous ethanol solution for oil removal, and electrically stir the fiber at 20-30 °C for 20-30 min at a speed of 750 r / min. The water washing process after alcohol washing is to rinse the nylon fiber with deionized water to remove residual solution.

3. The method for preparing the electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 1, It is characterized in that The nylon fiber after alcohol washing in step 1 is immersed in a 1-6% HCl solution at a temperature of 20-30°C and ultrasonically cleaned for 30-90 min; the nylon fiber after acid washing is ultrasonically cleaned with distilled water for 30 min, and then the cleaned fiber is placed in an electric heated blast drying oven and dried at 60°C for 4 h.

4. The method for preparing an electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 1, It is characterized in that The surface modification process includes: weighing 0.6 ml / LH 2 O 2 , 0.6~2.4 g / L CuSO 4 ·5H 2 O and 1~4 g / L catechol ethylamine are used to prepare the solution, and an appropriate amount of trimethylolaminomethane powder and 10 g / L sodium hydroxide solution are slowly added to adjust the pH value of the modified solution to 8~10, and the preparation of the catechol ethylamine solution is completed: the weighed nylon fiber after acid washing and finishing is placed in the prepared catechol ethylamine solution, and reacted for 30~120 min at 20~30 ℃, 150 r / min, and a bath ratio of 1:25; after the surface modification is completed, the modified nylon fiber is thoroughly washed with distilled water to pH=7 to remove the residual solution, and then dried in an electric blast drying oven at 60 ℃ for use.

5. The method for preparing the electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 1, It is characterized in that The chemical silver plating process comprises: weighing 5-8 g / L silver nitrate, 5-10 g / L complexing agent, 8-14 g / L reducing agent, alkaline pH adjusting agent, 0.1-0.3 g / L stabilizer and 50-200 ml / L surfactant to prepare chemical silver plating solution; the bath ratio of modified nylon fiber to silver plating solution is 1:25, immersing the surface-modified nylon fiber in the prepared chemical silver plating solution for 10 minutes, then slowly and uniformly adding the reducing solution at a volume ratio of 1:1; stirring with a magnetic stirrer at 1000 r / min and 25-40°C to fully react until the fiber is completely silver-plated.

6. The method for preparing the electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 5, It is characterized in that The complexing agent is selected from one of ethylenediaminetetraacetic acid and tartrate or a mixture of the two; the reducing agent can be selected from formaldehyde (HCHO), glucose (C 6 H 12 O 6 ) 7. The method for preparing the electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 5, It is characterized in that The alkaline pH regulator is one of sodium hydroxide and potassium hydroxide, and is used to adjust the pH value of the chemical silver plating solution to 11-13.

8. The method for preparing the electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 5, It is characterized in that The stabilizer is selected from gelatin, thiourea (CH 4 N 2 S), sodium iodide (NaI), potassium iodide (KI), and Cu 2+ 、Co 2+ 、Ni 2+ A type of salt.

9. The method for preparing the electromagnetic shielding and antibacterial multifunctional nylon fiber according to claim 5, It is characterized in that The surfactant is selected from ethanol (C 2 H 5 OH), polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), and polyethylene glycol (PEG).

10. An electromagnetic shielding and antibacterial multifunctional nylon fiber, It is characterized in that The method is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Fluorine-containing polymer / conductive fiber dielectric material and preparation method thereof

    CN105802092A

  • Palladium-free chemical copper plating method

    CN105821396A

  • Preparation method of pattered metallic textile on the basis of pretreatment with dopamine

    CN107747214A

  • Silver-plated nylon conductive fiber and preparation method thereof

    CN113445310A

  • Method for manufacturing magnetic fiber using catechol polymer