Processing technology of antibacterial warm-keeping socks

Through the weaving process of modified cotton thread and Coolmax spandex covered yarn, the problem of bacterial growth on the surface of cotton socks is solved, the wear resistance, breathability and deodorization performance of the socks are improved, and the antibacterial and warm effect is achieved.

CN118745663APending Publication Date: 2024-10-08ZHEJIANG GUANGTAI DELTA SOCKS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410753624.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Because cotton socks are worn for a long time, sweat, sebum and dirt are absorbed on the surface, leading to the growth of bacteria, and they lack effective antibacterial and warmth-keeping properties.

Method used

It adopts the weaving process of modified cotton thread and Coolmax spandex covered yarn, and modifies the cotton yarn through pretreatment liquid, quaternary ammonium salt modifier and finishing liquid to form a modified cotton yarn with antibacterial properties, and combines it with elastic for weaving to make Antibacterial thermal socks.

Benefits of technology

It improves the wear resistance, breathability and deodorizing performance of the socks, extends the service life of the product, and provides good antibacterial and thermal insulation effects.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the related technical field of sock production, and discloses a processing technology of an antibacterial warm-keeping sock, the antibacterial warm-keeping sock is formed by weaving rubber bands, modified cotton threads and Coolmax spandex wrap yarns; the modified cotton threads are prepared by sequentially modifying pure cotton yarns through a pretreatment solution, a quaternary ammonium salt modifier and a finishing solution. The surface of the cotton fiber is rich in hydroxyl, so that after the cotton thread is sequentially modified by the pretreatment liquid, the quaternary ammonium salt modifier and the finishing liquid, thiol bonds on the surface of the cotton thread are combined with sulfydryl obtained after the finishing liquid is broken to form new disulfide bonds, and the cotton thread is endowed with certain elasticity and antibacterial performance; furthermore, the texture structures and raw materials of different parts of the pretreated socks are limited, so that the aim of comprehensively improving the wear resistance, the air permeability and the deodorization performance of the whole socks is fulfilled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field related to socks production, in particular to a processing technology for antibacterial and warm-keeping socks. Background Art

[0002] Socks are a textile product that protects and decorates the feet. There are many raw materials for socks on the market, such as cotton, linen and wool.

[0003] Cotton is the main raw material of socks, which has excellent moisture absorption and comfort. Cotton socks made of cotton have excellent moisture absorption and perspiration effect in summer and can keep the feet warm in winter. However, since people generally wear socks for a long time a day, the friction between the feet and socks and the influence of human metabolism make the surface of cotton socks easily absorb sweat, sebum and dirt, which in turn causes the growth of bacteria. In order to solve this problem, a processing technology for antibacterial and warm socks is proposed. Summary of the invention

[0004] The invention provides a processing technology for antibacterial thermal socks, which solves the problems in the above-mentioned background technology.

[0005] The present invention solves the technical problem by adopting the following technical solutions:

[0006] A processing technology for antibacterial and warm socks, comprising weaving elastic, modified cotton thread and Coolmax spandex coated yarn; the modified cotton thread is prepared by modifying pure cotton yarn in sequence through a pretreatment liquid, a quaternary ammonium salt modifier and a finishing liquid; the pretreatment liquid is prepared by mixing 3-mercaptopropyltriethoxysilane and ethyl acetate; the quaternary ammonium salt modifier is prepared by processing raw materials including the following parts by weight: 790-795 parts of α, α'-dibromo-p-xylene and 940-945 parts of dimethylaminoethyl methacrylate; the finishing liquid is prepared by processing raw materials including the following parts by weight: terminal epoxy silicone oil, 4,4-diaminophenylene disulfide and a composite emulsifier; the preparation of the finishing liquid is prepared by the following steps;

[0007] S1: After the measured amount of 4,4'-diaminodiphenyl disulfide is dissolved in a solvent, the measured amount of epoxy-terminated silicone oil is added dropwise at a rate of 0.5-2 ml / min, stirred evenly, and reacted at 75-85°C for 40-50 min to obtain a premixed solution A;

[0008] S2: Add composite emulsifier and deionized water to the premixed liquid A, mix and stir, adjust the pH value to 5.5-6.5, mix and stir at a speed of 200-300 rpm for 30-40 minutes, and homogenize for 20-30 minutes to obtain a finishing liquid.

[0009] Preferably, in the preparation of the finishing liquid, the molar ratio of the terminal epoxy silicone oil to the 4,4-diaminophenylene disulfide is 30:22-28, and the weight average molecular weight of the terminal epoxy silicone oil is 430-440.

[0010] Preferably, the composite emulsifier comprises cetyltrimethylammonium bromide, isomeric tridecanol polyoxyethylene ether A and isomeric tridecanol polyoxyethylene ether B; the cloud point of the isomeric tridecanol polyoxyethylene ether A is 38.0-42.0 and the HLB value is 8.0-9.0; the cloud point of the isomeric tridecanol polyoxyethylene ether B is 60.0-62.0 and the HLB value is 10.5.

[0011] Preferably, the mass ratio of the cetyltrimethylammonium bromide, isomeric tridecanol polyoxyethylene ether A and isomeric tridecanol polyoxyethylene ether B is 7-9:40:50-54.

[0012] A processing technology for antibacterial thermal socks comprises the following steps:

[0013] S1: Preparation of modified cotton thread;

[0014] S2: After the modified cotton yarn prepared in S1 is wound, the Coolmax spandex coated yarn, the modified cotton yarn after winding and 100# rubber band are used as raw materials to weave pretreated socks, wherein the sock opening of the pretreated socks is 1+1 false ribbing, the sock barrel is a variable plain stitch, the high heel and the sock base are both plain stitch, the sock toe is a terry stitch, the sock sole is a double-needle double-row tuck stitch, and the sock surface is a fancy terry stitch;

[0015] S3: After the seam ends of the pretreated socks prepared in S2 are treated, they are shaped at a pressure of 17.68 N / cm2 and 65°C for 4 minutes to obtain a product.

[0016] Preferably, the preparation of the modified cotton thread in S1 specifically comprises the following steps:

[0017] S11: preparation of pretreatment solution, quaternary ammonium salt modifier and finishing solution;

[0018] S12: putting the pure cotton yarn into the pretreatment solution at 25-35° C. and a bath ratio of 1:45-60 for reaction for 100-120 min, then washing with anhydrous ethanol and distilled water in turn, and finally drying at 40-55° C. for 10-15 min to obtain pretreated cotton yarn A;

[0019] S13: 3-6% by mass of a quaternary ammonium salt modifier and 94-97% of deionized water are mixed and stirred to obtain a modified solution A, and the pH value of the modified solution A is adjusted to 7.5-8.5, and 0.002 mol of tris(2-carboxyethyl)phosphine hydrochloride is added per liter of the mixed solution, and the mixed solution is obtained after mixing and stirring for 220-260 min. The pretreated cotton thread A is put into the mixed solution at 25-35° C. and a bath ratio of 1:45-60 for reaction for 400-450 min. After the reaction is completed, it is rinsed with distilled water 3-4 times, and the pretreated cotton thread is dried at 55-65° C. for 20-30 min;

[0020] S14: Under the conditions of a bath ratio of 1:20-30 and a temperature of 38-42° C., the pretreated cotton thread B is placed in a finishing liquid with a concentration of 28-32 g / L for 7-12 minutes, and after the shaping treatment, a modified cotton thread is obtained.

[0021] Preferably, the shaping treatment in step S14 is specifically as follows: pre-baking at 50-55° C. for 3-7 minutes, heating to 60-70° C. for reaction for 30-40 minutes, cooling and drying to obtain the modified cotton thread.

[0022] The advantages and positive effects of the present invention are: since the surface of cotton fibers is rich in hydroxyl groups, after the cotton thread in the present application is modified by the pretreatment liquid, the quaternary ammonium salt modifier and the finishing liquid in sequence, the thiol bonds on the surface of the cotton thread are combined with the thiol groups obtained after the finishing liquid is broken to form new disulfide bonds, giving the cotton thread certain elasticity and antibacterial properties, thereby comprehensively improving the wear resistance and anti-wrinkle properties of the product, and by limiting the organizational structure and raw materials of different parts of the pretreated socks, the overall wear resistance, air permeability and deodorization performance of the socks are comprehensively improved. DETAILED DESCRIPTION

[0023] The present invention will now be described in further detail.

[0024] Socks are a kind of textile product for protecting and decorating the feet. There are many raw materials for socks on the market, such as cotton, linen and wool. Cotton, as the main raw material of socks, has excellent moisture absorption and comfort. Cotton socks made of cotton have excellent moisture absorption and perspiration effect in summer and can keep feet warm in winter. However, since people generally wear socks for a long time in a day, the friction between the feet and socks and the influence of human metabolism make the surface of cotton socks easily absorb sweat, sebum and dirt, which in turn causes the growth of bacteria. In order to solve this problem, a processing technology of antibacterial and warm socks is proposed, including elastic band, modified cotton thread, and Coolmax spandex coated yarn; the modified cotton thread is prepared by modifying pure cotton yarn in sequence through a pretreatment solution, a quaternary ammonium salt modifier and a finishing solution; the pretreatment solution is a mixture of 3-mercaptopropyltriethoxysilane and ethyl acetate; the quaternary ammonium salt modifier is processed from the following raw materials in parts by weight: 790-795 parts of α, α'-dibromo-p-xylene and 940-945 parts of dimethylaminoethyl methacrylate; the finishing solution is processed from the following raw materials: terminal epoxy silicone oil, 4,4-diaminophenylene disulfide and a composite emulsifier; the preparation of the finishing solution is processed by the following steps;

[0025] S1: After the measured amount of 4,4'-diaminodiphenyl disulfide is dissolved in a solvent, the measured amount of epoxy-terminated silicone oil is added dropwise at a rate of 0.5-2 ml / min, stirred evenly, and reacted at 75-85°C for 40-50 min to obtain a premixed solution A;

[0026] S2: Add composite emulsifier and deionized water to premixed liquid A, mix and stir, adjust the pH value to 5.5-6.5, mix and stir at a speed of 200-300rpm for 30-40min, and homogenize for 20-30min to prepare a finishing liquid; since the surface of cotton fiber is rich in hydroxyl groups, the cotton thread in the present application is modified by the pretreatment liquid, quaternary ammonium salt modifier and finishing liquid in sequence, and the thiol bonds on the surface of the cotton thread are combined with the thiol groups obtained after the rupture of the finishing liquid to form new disulfide bonds, giving the cotton thread certain elasticity and antibacterial properties, thereby comprehensively improving the wear resistance and anti-wrinkle properties of the product, and by limiting the organizational structure and raw materials of different parts of the pretreated socks, the overall wear resistance, air permeability and deodorization performance of the socks are comprehensively improved.

[0027] It should be noted that, Preparation Example 1, the preparation of terminal epoxy silicone oil, is specifically prepared as follows: 4500g of methylcyclotetrasiloxane, 247.5g of concentrated sulfuric acid and 1.8g of tetramethylammonium hydroxide are reacted in a nitrogen atmosphere for 490min, the temperature is raised to 183°C, low boiling points are removed by distillation under reduced pressure, 427.5g of allyl glycidyl ether, 8437.5g of toluene and 1.8g of chloroplatinic acid are added, the temperature is raised to 85°C, the reaction is carried out in a nitrogen atmosphere for 570min, and the solvent is removed by distillation under reduced pressure to obtain a terminal epoxy silicone oil with a weight average molecular weight of 433.

[0028] Further, Preparation Example 2, preparation of epoxy-terminated silicone oil, the preparation is specifically as follows: 4500g of methylcyclotetrasiloxane, 224.9g of concentrated sulfuric acid and 2.30g of tetramethylammonium hydroxide are reacted in a nitrogen atmosphere for 540min, the temperature is raised to 180°C, low-boiling substances are removed by vacuum distillation, 450g of allyl glycidyl ether, 8100g of toluene and 1.8g of chloroplatinic acid are added, the temperature is raised to 89°C, the reaction is carried out in a nitrogen atmosphere for 590min, and the solvent is removed by vacuum distillation to obtain an epoxy-terminated silicone oil with a weight average molecular weight of 310;

[0029] Preparation Example 3, preparation of terminal epoxy silicone oil, the preparation is specifically as follows: 4500g of methylcyclotetrasiloxane, 90g of concentrated sulfuric acid and 0.9g of tetramethylammonium hydroxide are reacted in a nitrogen atmosphere for 420min, the temperature is raised to 181°C, and low-boiling substances are removed by reduced pressure distillation. Then, 180g of allyl glycidyl ether, 4725g of toluene and 0.9g of chloroplatinic acid are added, the temperature is raised to 75°C, and the reaction is carried out in a nitrogen atmosphere for 480min. The solvent is removed by reduced pressure distillation to obtain a terminal epoxy silicone oil with a weight average molecular weight of 530.

[0030] It should be noted that, in S1: the preparation of modified cotton thread, the preparation of pretreatment liquid, quaternary ammonium salt modifier and finishing liquid, wherein the preparation of pretreatment liquid is specifically as follows: 3-mercaptopropyl triethoxysilane is mixed and stirred evenly in ethyl acetate to obtain a modified liquid, wherein the mass fraction of 3-mercaptopropyl triethoxysilane in the modified liquid is 1.5%; wherein the preparation of quaternary ammonium salt modifier is specifically as follows: 791.9 g of α, α'-dibromo-p-xylene is prepared, and quaternary ammonium salt modifier is added dropwise at a rate of 5 ml / min while stirring. acetone until α, α'-dibromo-p-xylene is completely dissolved, then 943.3 g of dimethylaminoethyl methacrylate is added dropwise at a rate of 5 ml / min, and the mixture is stirred at reflux at 50°C for 23 h. After filtration, the mixture is washed twice with acetone, and then filtered again to obtain dimethylaminoethyl methacrylate quaternary ammonium salt; wherein the preparation of the finishing liquid comprises the following steps: 2 kg of 4,4'-diaminodiphenyl disulfide is taken and dissolved in 1.35 kg of ethyl acetate, and 1 ml of The epoxy-terminated silicone oil prepared in Preparation Example 1 was added dropwise at a rate of 200 rpm while being mixed and stirred at a speed of 200 rpm. After being stirred evenly, the mixture was reacted at 80° C. for 45 min to obtain a premixed solution A, wherein the molar ratio of the epoxy-terminated silicone oil added dropwise to 4,4'-diaminodiphenyl disulfide was 30:25; and 2.42 kg of a composite emulsifier was added to the premixed solution A and stirred evenly, and deionized water was added and mixed and stirred at a speed of 200 rpm, and then a 36% concentration of After adjusting the pH value of the premixed solution A to 6.0 with acetic acid solution, the mixture was mixed and stirred at a speed of 300 rpm for 30-40 minutes, and then homogenized by a homogenizer for 25 minutes to obtain a finishing solution with a solid content of 30%, wherein the composite emulsifier was prepared by mixing and stirring cetyltrimethylammonium bromide, isomeric tridecanol polyoxyethylene ether A (cloud point of 40, HLB value of 9.0) and isomeric tridecanol polyoxyethylene ether B (cloud point of 67, HLB value of 10.5) in a mass ratio of 8:40:52;

[0031] Further, at 30° C. and a bath ratio of 1:50, the pure cotton yarn was put into the pretreatment solution for reaction for 110 minutes, and then rinsed with anhydrous ethanol and distilled water in turn, and finally dried at 50° C. for 12 minutes to obtain pretreated cotton thread A; 4% by mass of quaternary ammonium salt modifier and 95% of deionized water were mixed and stirred evenly to obtain modified solution A, and the pH value of modified solution A was adjusted to 8.5 with 0.5 mol / L sodium bicarbonate buffer, and 0.002 mol of tris(2-carboxyethyl)phosphine hydrochloride was added per liter of mixed solution, and mixed and stirred for 245 minutes to obtain a mixed solution, and at 30° C. and a bath ratio of 1:50, the pretreated cotton thread A was put into the mixed solution for reaction for 430 minutes, and after the reaction was completed, it was rinsed with distilled water for 3 times, and then dried at 60° C. for 25 minutes to pretreat cotton thread B;

[0032] Under the conditions of bath ratio of 1:20 and temperature of 40°C, the pretreated cotton thread B was placed in a finishing liquid with a concentration of 30 g / L for 10 min, pre-dried at 53°C for 4 min, heated to 65°C for 35 min, taken out and cooled to room temperature, and dried at 40°C for 30 min to obtain a modified cotton thread with a specification of 21S / 2;

[0033] It should also be noted that S2: after the modified cotton yarn prepared in S1 is wound, the 30 / 75D Coolmax spandex coated yarn, the modified cotton yarn after winding and 100# elastic are used as raw materials, and the yarn is passed through a 108-needle YF-200311 fully computerized hosiery machine with a controlled machine speed of 200r /

[0034] min, knitted into pretreated socks with a cuff width of 6.5 cm, a cuff length of 3.5 cm, a sock length of 3.8 cm, a sole length of 10.3 cm and a sole width of 6.5 cm; wherein the modified cotton yarn of 21S / 2 prepared in S1 is the face yarn, and the Coolmax spandex covered yarn with a specification of 30 / 75D is the base yarn; the sock cuff is a 1+1 false rib knitted by knitting 100# elastic and the face yarn, and the number of rows of knitting coils of the sock cuff is 24; the sock cuff is a changed plain stitch knitted by knitting the face yarn and the base yarn, and the number of rows of knitting coils of the sock cuff is 15; the high heel is a plain stitch knitted by knitting the face yarn and the base yarn, and the number of rows of knitting coils of the high heel is 8; the sock heel is a plain stitch knitted by knitting the face yarn and the base yarn, and the number of pick-up stitches at the sock heel is 23 stitches, the number of narrowing stitches is 12 stitches, and the number of releasing stitches is 11 stitches; the sock toe is a knitted by knitting the face yarn and the base yarn The bottom yarn is woven into a terry structure, and the number of needles for the sock head is 23, the number of needles for the narrowing is 12, and the number of needles for the releasing is 11; the sock sole is a double-needle double-row tuck structure woven from the face yarn and the bottom yarn, and the number of horizontal rows of the knitting coils of the sock sole is 58. The setting of the double-needle double-row tuck makes the inner and outer yarns of the tuck large mesh structure functional socks exchange positions at the tuck part, the coolmax spandex coated yarn appears on the front of the socks, and the modified cotton thread appears on the back of the socks in the form of floating thread, forming a large and small mesh on the front and a fish scale-like flower pattern on the back; the sock surface is a fancy terry structure woven from the face yarn and the bottom yarn, and the number of horizontal rows of the knitting coils of the sock surface is 15. The setting of the fancy terry structure makes the back of the sock surface form a moisture-conducting groove of the coolmax spandex coated yarn similar to a capillary channel composed of horizontal and vertical rows of linting coils, while the front is all modified cotton thread;

[0035] S3: After the seams of the pretreated socks prepared in S2 are treated, they are shaped at a pressure of 17.68 N / cm2 and 65°C for 4 minutes to obtain the antibacterial and warm-keeping product.

[0036] It should be emphasized that the embodiments described in the present invention are illustrative rather than restrictive, and therefore the present invention is not limited to the embodiments described in the specific implementation manners. Any other implementation manners derived by those skilled in the art based on the technical solutions of the present invention also fall within the scope of protection of the present invention.

Claims

1. An antibacterial thermal socks, characterized in that: The invention comprises elastic band, modified cotton thread and Coolmax spandex coated yarn; the modified cotton thread is prepared by modifying pure cotton yarn in sequence through a pretreatment liquid, a quaternary ammonium salt modifier and a finishing liquid; the pretreatment liquid is prepared by mixing 3-mercaptopropyltriethoxysilane and ethyl acetate; the quaternary ammonium salt modifier is prepared by processing raw materials including the following parts by weight: 790-795 parts of α, α'-dibromo-p-xylene and 940-945 parts of dimethylaminoethyl methacrylate; the finishing liquid is prepared by processing raw materials including the following parts by weight: terminal epoxy silicone oil, 4,4-diaminophenylene disulfide and a composite emulsifier; the preparation of the finishing liquid is prepared by the following steps; S1: After the measured amount of 4,4'-diaminodiphenyl disulfide is dissolved in a solvent, the measured amount of epoxy-terminated silicone oil is added dropwise at a rate of 0.5-2 ml / min, stirred evenly, and reacted at 75-85°C for 40-50 min to obtain a premixed solution A; S2: Add composite emulsifier and deionized water to the premixed liquid A, mix and stir, adjust the pH value to 5.5-6.5, mix and stir at a speed of 200-300 rpm for 30-40 minutes, and homogenize for 20-30 minutes to obtain a finishing liquid.

2. The antibacterial thermal socks according to claim 1, characterized in that: In the preparation of the finishing liquid, the molar ratio of the terminal epoxy silicone oil to the 4,4-diaminophenylene disulfide is 30:22-28, and the weight average molecular weight of the terminal epoxy silicone oil is 430-440.

3. The antibacterial thermal socks according to claim 1, characterized in that: The composite emulsifier comprises cetyltrimethylammonium bromide, isomeric tridecanol polyoxyethylene ether A and isomeric tridecanol polyoxyethylene ether B; the cloud point of the isomeric tridecanol polyoxyethylene ether A is 38.0-42.0 and the HLB value is 8.0-9.0; the cloud point of the isomeric tridecanol polyoxyethylene ether B is 60.0-62.0 and the HLB value is 10.

5.

4. The antibacterial thermal socks according to claim 3, characterized in that: The mass ratio of the hexadecyltrimethylammonium bromide, isomeric tridecanol polyoxyethylene ether A and isomeric tridecanol polyoxyethylene ether B is 7-9:40:50-54.

5. A processing technology for antibacterial thermal socks, characterized in that: The following steps are involved: S1: Preparation of modified cotton thread; S2: After the modified cotton yarn prepared in S1 is wound, the Coolmax spandex coated yarn, the modified cotton yarn after winding and 100# rubber band are used as raw materials to weave pretreated socks, wherein the sock opening of the pretreated socks is 1+1 false ribbing, the sock barrel is a variable plain stitch, the high heel and the sock base are both plain stitch, the sock toe is a terry stitch, the sock sole is a double-needle double-row tuck stitch, and the sock surface is a fancy terry stitch; S3: After the seam ends of the pretreated socks prepared in S2 are treated, they are shaped at a pressure of 17.68 N / cm2 and 65°C for 4 minutes to obtain a product.

6. The processing technology of antibacterial thermal socks according to claim 5 is characterized in that: The preparation of the modified cotton thread in S1 specifically comprises the following steps: S11: preparation of pretreatment solution, quaternary ammonium salt modifier and finishing solution; S12: putting the pure cotton yarn into the pretreatment solution at 25-35° C. and a bath ratio of 1:45-60 for reaction for 100-120 min, then washing with anhydrous ethanol and distilled water in turn, and finally drying at 40-55° C. for 10-15 min to obtain pretreated cotton yarn A; S13: 3-6% by mass of a quaternary ammonium salt modifier and 94-97% of deionized water are mixed and stirred to obtain a modified solution A, and the pH value of the modified solution A is adjusted to 7.5-8.5, and 0.002 mol of tris(2-carboxyethyl)phosphine hydrochloride is added per liter of the mixed solution, and the mixed solution is obtained after mixing and stirring for 220-260 min. The pretreated cotton thread A is put into the mixed solution at 25-35° C. and a bath ratio of 1:45-60 for reaction for 400-450 min. After the reaction is completed, it is rinsed with distilled water 3-4 times, and the pretreated cotton thread is dried at 55-65° C. for 20-30 min; S14: Under the conditions of a bath ratio of 1:20-30 and a temperature of 38-42° C., the pretreated cotton thread B is placed in a finishing liquid with a concentration of 28-32 g / L for 7-12 minutes, and after the shaping treatment, a modified cotton thread is obtained.

7. The processing technology of antibacterial thermal socks according to claim 5 is characterized in that: The shaping treatment in step S14 is specifically as follows: pre-baking at 50-55° C. for 3-7 minutes, heating to 60-70° C. for reaction for 30-40 minutes, cooling and drying to obtain the modified cotton thread.