Compressor shell and rotor type compressor
By using iron-nickel austenitic alloy and C-shaped snap ring support design, the problem of weak magnetic permeability of the rotary compressor shell material is solved, induced current and uneven thermal sleeve deformation are avoided, and the compressor's performance is significantly improved. Motor efficiency.
Patent Information
- Application Number
- CN202410951839.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The casing material of the rotary compressor has weak magnetic permeability, which causes the magnetic properties of the stator to deteriorate, increases the iron loss of the motor, and thereby reduces the efficiency of the compressor.
Iron-nickel austenitic alloy is used as the compressor shell material, combined with the C-shaped snap ring support design to ensure interference fit between the shell and the stator, avoid induced current and uneven thermal sleeve deformation, and improve motor efficiency.
It effectively avoids the increase in induced current and iron loss, ensures uniform heating of the compressor casing, reduces the deformation of the stator, and significantly improves the motor efficiency of the compressor.
Smart Images

Figure CN118745998A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of compressors, and in particular to a compressor housing and a rotor type compressor. Background Art
[0002] A rotary compressor (i.e. a rotor compressor) is a new type of compressor. Its motor does not need to convert the rotational motion of the rotor into the reciprocating motion of the piston, but directly drives the rotary piston to rotate to complete the compression of the refrigerant vapor.
[0003] At present, the housing of the rotary compressor is connected to the motor stator by interference fit, and then the stator is assembled by shrinkage, or the stator and the housing are fixed by welding. However, this assembly and fixing method will produce compressive stress on the stator due to the thermal shrinkage of the housing. When the silicon steel material used in the stator is subjected to external compressive stress, its magnetic properties will deteriorate, which will lead to increased iron loss of the motor. Therefore, after the stator and the housing are shrinkage-fitted, the motor efficiency will decrease to a certain extent compared with the motor without shrinkage-fitting, and the specific decrease range is 0.3% to 0.5%.
[0004] In addition, the compressor casing is mainly made of cold-rolled steel. Although this material is a weakly magnetic material, it also has magnetic conductivity. Therefore, when the stator silicon steel sheet is in close axial contact with the casing cold-rolled steel plate over a large area, when the motor is running, due to the existence of the alternating magnetic field in the stator core, the casing steel plate will generate induced current, thereby generating a large amount of eddy current loss, which will also affect the motor efficiency of the compressor.
[0005] Therefore, how to improve the motor efficiency of the compressor is a problem that those skilled in the art need to solve. Summary of the invention
[0006] The embodiments of the present invention provide a compressor housing and a rotor-type compressor, which are intended to solve the problem that the compressor housing material has weak magnetic conductivity and improve the motor efficiency in the compressor.
[0007] An embodiment of the present invention provides a compressor housing, wherein the compressor housing is made of an iron-nickel austenite alloy, wherein the components of the iron-nickel austenite alloy include: nickel, iron, chromium, manganese and titanium;
[0008] The microstructure of the iron-nickel austenite alloy is equiaxed austenite grains.
[0009] Furthermore, the mass ratios of the nickel element, the iron element, the chromium element, the manganese element and the titanium element are 8% to 80%, 5% to 80%, 14% to 20%, 1% to 2% and 0% to 3%, respectively.
[0010] Furthermore, the size of the equiaxed austenite grains is 15 to 25 μm.
[0011] Furthermore, the hardness of the iron-nickel austenitic alloy is 185-195 HV.
[0012] An embodiment of the present invention further provides a rotor-type compressor, comprising a compressor housing as described in any one of the above items and a stator connected to the compressor housing.
[0013] Furthermore, the compressor housing and the stator are interference fit, and the interference amount is 0.09-0.11 mm.
[0014] Furthermore, a supporting portion for supporting the stator is provided at the lower end of the stator.
[0015] Furthermore, the supporting portion is a C-shaped snap ring, both ends of which are fixedly disposed on the stator, and the ring portion of the C-shaped snap ring is interference fit with the compressor housing.
[0016] Furthermore, the C-shaped clamping ring includes a plurality of stacked single sheets, and the thickness of each single sheet is less than 0.3 mm.
[0017] Furthermore, the tensile strength of the C-shaped clamping ring is greater than or equal to 850 MPa, and the elongation is 20% to 25%.
[0018] Furthermore, the hardness of the compressor housing is smaller than the hardness of the stator, and the hardness ratio of the compressor housing to the stator is 1:1.1 to 1:1.5.
[0019] The embodiment of the present invention provides a compressor housing and a rotor compressor, wherein the compressor housing is made of an iron-nickel austenitic alloy, and the components of the iron-nickel austenitic alloy include: nickel, iron, chromium, manganese and titanium; the microstructure of the iron-nickel austenitic alloy is equiaxed austenite grains. The embodiment of the present invention proposes a new housing material, that is, the compressor housing is prepared by an iron-nickel austenitic alloy, and the components of the iron-nickel austenitic alloy include nickel, iron, chromium, manganese and titanium. Compared with the commonly used housing cold-rolled steel, the iron-nickel austenitic alloy is non-magnetic, so it will not generate induced current with the stator core, so that it can avoid causing an increase in iron loss, thereby solving the problem of the compressor housing material having weak magnetic conductivity and improving the motor efficiency in the compressor. In addition, the microstructure of the iron-nickel austenitic alloy in the embodiment of the present invention is equiaxed austenite grains, and the material under the microstructure of the equiaxed austenite grains is dense and uniform. In this way, the compressor casing can be heated more uniformly during hot-fitting while ensuring that the compressor casing and the stator are non-magnetic, thereby reducing the adverse effect of uneven deformation of the compressor casing due to heating on the coaxiality of the stator, and further improving the motor efficiency of the compressor. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying any creative work.
[0021] Figure 1 A schematic structural diagram of a rotor compressor provided by an embodiment of the present invention;
[0022] Figure 2 A microstructure metallographic diagram of an iron-nickel austenitic alloy of a compressor housing provided by an embodiment of the present invention;
[0023] Figure 3 for Figure 1 A magnified schematic diagram of part A;
[0024] Figure 4 A schematic diagram of the structure of a C-type clamp ring in a rotor compressor provided by an embodiment of the present invention;
[0025] Figure 5 A schematic diagram of the connection between a C-shaped retaining ring and a compressor housing and a stator in a rotor-type compressor provided in an embodiment of the present invention.
[0026] Markings in the figure:
[0027] 1. Compressor housing;
[0028] 2. Stator;
[0029] 3. Support part. DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0032] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.
[0033] It should be further understood that the term "and / or" used in the present description and the appended claims refers to and includes any and all possible combinations of one or more of the associated listed items.
[0034] See below Figure 1 , an embodiment of the present invention provides a compressor housing 1, the compressor housing 1 is made of an iron-nickel austenitic alloy, and the components of the iron-nickel austenitic alloy include: nickel element, iron element, chromium element, manganese element and titanium element;
[0035] The microstructure of the iron-nickel austenite alloy is equiaxed austenite grains.
[0036] This embodiment proposes a new shell material, that is, the compressor shell 1 is prepared using an iron-nickel austenitic alloy. The components of the iron-nickel austenitic alloy include nickel, iron, chromium, manganese and titanium. Compared with the commonly used shell cold-rolled steel, the iron-nickel austenitic alloy is non-magnetic, so it will not generate induced current with the iron core of the stator 2, so as to avoid causing increased iron loss, thereby solving the problem that the compressor shell 1 material has weak magnetic conductivity and improving the motor efficiency in the compressor. In addition, combined with Figure 2 The microstructure of the iron-nickel austenitic alloy in this embodiment is equiaxed austenite grains, and the material under the microstructure of the equiaxed austenite grains is dense and uniform. In this way, the compressor housing 1 can be heated more uniformly during shrink-fitting while ensuring that the compressor housing 1 and the stator 2 are non-magnetic, thereby reducing the adverse effect of the compressor housing 1 on the coaxiality of the stator 2 due to uneven deformation due to heating.
[0037] In particular, the compressor housing 1 provided in this embodiment is particularly suitable for rotary compressors, including but not limited to single-cylinder single-stage, double-cylinder single-stage, double-cylinder variable displacement and other rotary compressors. It should also be noted that compared with the existing iron-based stainless steel (Ni6%-10%) and nickel-iron-based alloy (≥50%), the iron-nickel austenitic alloy in this embodiment has a wider range of Ni alloy elements (8%-80%), and at the same time removes Si (silicon), N (nitrogen), Cu (copper), Al (aluminum) and other alloy elements in the existing materials. The reason for this design is mainly: the most important reference indicator of the iron-nickel austenitic alloy in this embodiment is to obtain a non-magnetic austenitic structure, and the formation of austenitic structure is mainly related to the Ni alloy element, so the Ni content is designed to be 8% to 80%. Other alloying elements such as Si, N, Cu, and Al are mainly used to improve the toughness and hardness of the material. For the application fields of the iron-nickel austenitic alloy in this embodiment, high strength and high hardness are not required. Therefore, the iron-nickel austenitic alloy in this embodiment is different from the materials in the prior art (such as iron-based stainless steel and nickel-iron-based alloy, etc.).
[0038] In a specific embodiment, the mass ratios of the nickel element, the iron element, the chromium element, the manganese element and the titanium element are 8% to 80%, 5% to 80%, 14% to 20%, 1% to 2% and 0% to 3%, respectively.
[0039] The components of the iron-nickel austenitic alloy of this embodiment are: Ni 8% to 80%, Fe 5% to 80%, Cr 14% to 20%, Mn 1% to 2%, and Ti 0% to 3%. For example, the mass ratio of Ni is 40%, the mass ratio of Fe is 40%, the mass ratio of Cr is 15%, the mass ratio of Mn is 2%, and the mass ratio of Ti is 3%.
[0040] In some optional embodiments, the composition of the iron-nickel austenitic alloy may also be: Ni 8% to 80%, Fe 5% to 70%, Cr 10% to 30%, Mn 1% to 4%, Ti 0% to 5%.
[0041] For example, the mass ratio of Ni is 40%, the mass ratio of Fe is 35%, the mass ratio of Cr is 20%, the mass ratio of Mn is 1%, and the mass ratio of Ti is 4.0%.
[0042] In some other optional embodiments, the composition of the iron-nickel austenitic alloy may also be: Ni 5% to 85%, Fe 5% to 80%, Cr 10% to 20%, Mn 1% to 5%, Ti 0% to 2%.
[0043] For example, the mass ratio of Ni is 50%, the mass ratio of Fe is 35%, the mass ratio of Cr is 10%, the mass ratio of Mn is 4%, and the mass ratio of Ti is 1%.
[0044] In some further optional embodiments, the composition of the iron-nickel austenitic alloy may also be: Ni 5% to 85%, Fe 5% to 80%, Cr 10% to 20%, and Mn 1% to 5%.
[0045] For example, the mass ratio of Ni is 50%, the mass ratio of Fe is 35%, the mass ratio of Cr is 10%, and the mass ratio of Mn is 5%.
[0046] In another specific embodiment, the size of the equiaxed austenite grains is 15-25 μm.
[0047] The iron-nickel austenitic alloy in this embodiment has a microstructure of equiaxed austenitic grains, and the grain size is 15 to 25 μm. Figure 2 The material under this organization is uniform and dense, so that the compressor housing 1 can be heated evenly during shrink fitting, thereby reducing the adverse effect of housing deformation on the coaxiality of the stator 2.
[0048] Specifically, the size of the equiaxed austenite grains is 20 μm.
[0049] In another specific embodiment, the hardness of the iron-nickel austenitic alloy is 185-195 HV.
[0050] Compared with the existing cold-rolled steel, the hardness relationship between the iron-nickel austenitic alloy in this embodiment is:
[0051] HV 铁镍奥氏体合金 <HV 冷轧钢 ;
[0052] That is to say, the hardness of the iron-nickel austenitic alloy in this embodiment is less than the hardness of the existing cold-rolled steel. Specifically, the hardness of the iron-nickel austenitic alloy in this embodiment is preferably 185-195HV, for example 190HV, so that the hardness of the iron-nickel austenitic alloy in this embodiment is lower than that of the conventional cold-rolled steel shell. In this way, after the same shrink-fit process, the compressor shell 1 in this embodiment can apply a smaller deformation force to the contact part stator 2, thereby further reducing the iron loss of the stator 2 after shrink-fit.
[0053] An embodiment of the present invention further provides a rotor-type compressor, comprising a compressor housing 1 as described in any one of the above items and a stator 2 connected to the compressor housing 1 .
[0054] like Figure 1 As shown, in this embodiment, a compressor housing 1 made of an iron-nickel austenitic alloy is connected to a stator 2, specifically an interference connection, and a shrink fit is performed. After the shrink fit, the deterioration of the iron loss of the stator 2 can be avoided, thereby improving the energy efficiency of the compressor.
[0055] In this embodiment, the compressor housing 1 made of an iron-nickel austenitic alloy is heat-fitted with the stator 2. Compared with the commonly used cold-rolled steel housing, the compressor housing 1 made of an iron-nickel austenitic alloy is non-magnetic, so it will not generate induced current with the iron core of the stator 2 when heat-fitting, so that it can avoid causing the iron loss of the iron core to increase, thereby solving the problem of the compressor housing 1 material having weak magnetic conductivity, and improving the motor efficiency in the compressor. In addition, since the microstructure of the iron-nickel austenitic alloy is equiaxed austenite grains, and the material under the organization of the equiaxed austenite grains is dense and uniform, it can ensure that the compressor housing 1 and the stator 2 are non-magnetic, and the compressor housing 1 is better heated uniformly during heat-fitting, thereby reducing the adverse effect of the compressor housing 1 on the coaxiality of the stator 2 due to uneven deformation due to heat, and further improving the motor efficiency of the compressor.
[0056] In a specific embodiment, the compressor housing 1 and the stator 2 are interference fit, and the interference amount is 0.09-0.11 mm.
[0057] The housing of the rotary compressor is connected to the motor stator 2 by an interference fit, and the stator 2 is assembled by shrinkage, or the stator 2 and the housing are fixed by welding. The interference fit between the stator 2 and the housing needs to be within a certain range. If the interference is too small, the retention force between the stator 2 and the housing will be insufficient, and the housing will not be completely cooled and shrunk after shrinkage, which will cause the stator 2 to move down or even fall out of the housing when the workpiece is pulled out; if the interference is too large, the housing will be deformed due to the long heating time, making it impossible to insert the stator 2 or excessively squeeze the stator 2 to deform the inner diameter of the stator 2. Therefore, while ensuring that the stator 2 does not fall off, the smaller the interference is designed, the smaller the stress applied by the housing to the stator 2, the weaker the deformation tendency of the stator 2, and the higher the motor efficiency. The design value of the interference between the existing cold-rolled steel housing and the silicon steel stator 2 is generally between 0.12mm and 0.2mm. The interference fit between the iron-nickel austenitic alloy shell and the stator 2 of this embodiment is designed to be 0.09mm~0.11mm. Compared with the interference fit between the existing shell and the stator 2 of 0.12mm~0.2mm, the interference fit of this embodiment is smaller, which can reduce the stress exerted by the compressor shell 1 on the stator 2, thereby weakening the deformation tendency of the stator 2, thereby further improving the motor efficiency of the compressor.
[0058] In one embodiment, a support portion 3 for supporting the stator 2 is disposed at the lower end of the stator 2 .
[0059] This embodiment designs parameters with small interference for the compressor housing 1 and the stator 2, and combines the reinforcement method of the support portion 3 at the bottom of the stator 2 to ensure that the stator 2 does not fall off after the compressor housing 1 and the stator 2 are shrink-fitted, while reducing the stress of the compressor housing 1 on the stator 2 during shrink-fitting. This can reduce the deformation of the stator 2, thereby significantly reducing the industry bottleneck problem of increased iron loss of the stator 2 after shrink-fitting, and further improve the motor efficiency of the compressor.
[0060] Specific, combined Figure 3 and Figure 5 The support portion 3 is a C-shaped snap ring, both ends of which are fixedly arranged on the stator 2, the ring portion of the C-shaped snap ring is tightly fitted with the compressor housing 1, and the outer diameter of the C-shaped snap ring is the same as the inner diameter of the compressor housing 1.
[0061] Furthermore, the tensile strength of the C-shaped clamping ring is greater than or equal to 850 MPa, and the elongation is 20% to 25%.
[0062] In this embodiment, a C-shaped snap ring is provided at the lower end of the stator 2, and the C-shaped snap ring is tightly fitted with the compressor housing 1, and the outer diameter of the C-shaped snap ring is consistent with the inner diameter of the upper housing of the compressor housing 1, so that the stator 2 will not fall off while ensuring that the compressor housing 1 and the stator 2 have a small interference parameter design. The C-shaped snap ring can be made of high-strength stainless steel, so that the C-shaped snap ring has excellent toughness and strength. In this way, on the one hand, it can be elastically deformed and easy to install, and on the other hand, it can support the stator 2 based on high strength to ensure that the stator 2 will not fall off.
[0063] The material of the stator 2 is usually silicon steel, and the yield strength of the C-type clamp ring needs to be much greater than the tensile strength (360MPa) of the silicon steel stator 2. The tensile strength of the C-type clamp ring is preferably greater than or equal to 650MPa, and the elongation is 25% to 35%. Here, the yield strength refers to the yield limit of the metal material when the yield phenomenon occurs, that is, the stress that resists the slight plastic deformation. For metal materials without obvious yield phenomenon, the stress value that produces 0.2% residual deformation is specified as its yield limit, which is called conditional yield limit or yield strength. External forces greater than the yield strength will cause the parts to fail permanently and cannot be restored. Tensile strength refers to the critical value of the transition of metal from uniform plastic deformation to local concentrated plastic deformation, and is also the maximum bearing capacity of metal under static tensile conditions. Tensile strength is the resistance to the maximum uniform plastic deformation of the material. Before the tensile specimen is subjected to the maximum tensile stress, the deformation is uniform and consistent, but after exceeding it, the metal begins to shrink, that is, concentrated deformation occurs; for brittle materials with no (or very small) uniform plastic deformation, it reflects the fracture resistance of the material. The symbol is Rm (GB / T 228-1987 old national standard stipulates that the symbol of tensile strength is σb), and the unit is MPa. Elongation refers to the percentage of the total deformation ΔL of the gauge section after the specimen is tensile fractured to the original gauge length L: δ = ΔL / L × 100%. Elongation δ and cross-sectional shrinkage are indicators that describe the plastic properties of the material. Cold-rolled strip steel that has undergone recrystallization annealing needs to be leveled to obtain the various properties required for delivery, and elongation, as the only deformation indicator of leveling rolling, plays a vital role in ensuring the internal organizational structure and performance of the strip steel.
[0064] In actual application scenarios, the C-shaped clamp includes a plurality of stacked single sheets, and the thickness of each of the single sheets is less than 0.3 mm.
[0065] This embodiment uses multiple single pieces stacked together to form a C-shaped snap ring with a certain thickness, wherein the thickness of each single piece is less than 0.3 mm, and the number of single pieces is 5 to 6 pieces, so the thickness of the stacked C-shaped snap ring is 1.5 mm to 1.8 mm.
[0066] It should also be noted that the reason why this embodiment does not directly use a C-shaped clamp ring with a certain thickness, but uses multiple single pieces stacked, is because the material of the C-shaped clamp ring is high-strength stainless steel. If the thickness of the single piece is too thick, the steel will not be easy to elastically deform, which is not easy to install, and the elasticity of the C-shaped clamp ring will be poor. In this way, when the motor is running, the elastic buffering of the C-shaped clamp ring to the stator 2 will be weakened, causing the vibration to become larger, thereby affecting the operation of the motor. Therefore, the design of a structure of multiple thin rings stacked can ensure sufficient strength while ensuring sufficient elasticity, thereby facilitating installation and buffering the running vibration of the motor.
[0067] In one embodiment, the hardness of the compressor housing 1 is smaller than the hardness of the stator 2 , and the hardness ratio of the compressor housing 1 to the stator 2 is 1:1.1 to 1:1.5.
[0068] This embodiment optimizes the material relationship parameters between the shell and the stator 2 to select the best hardness difference and strength difference, which can further reduce iron loss and thus improve motor efficiency. Specifically, when the iron-nickel austenitic alloy shell of this embodiment is used, the corresponding stator 2 iron core needs to use silicon steel 35W360 grade with a thickness of 0.35mm. Under the same stator 2 structure, the thinner the thickness of the silicon steel single sheet, the better the performance, but after the shell is hot-fitted, the thinner the thickness, the more susceptible it is to the impact of shell stress. When the thickness of 0.35mm is matched with the inventive shell, the iron loss is the lowest. The hardness of the iron-nickel austenitic alloy shell and the silicon steel of the stator 2 in this embodiment needs to meet the following requirements:
[0069] HV 铁镍奥氏体合金 <HV 定子 ;
[0070] HV 铁镍奥氏体合金 :HV 定子 =1:1.1~1:1.5;
[0071] Under the above-mentioned hardness relationship, the deformation of the stator 2 after the shrink sleeve is minimal. Correspondingly, the reduction in motor efficiency is significantly reduced, and the vibration and noise of the motor are also significantly reduced. Silicon steel sheet 35w360 is a soft magnetic material with high magnetic induction, high strength and high conductivity, which is widely used in power, electronics and communications and other fields. Its manufacturing process adopts cold rolling and insulation coating technology, which makes the silicon steel sheet have excellent magnetic and mechanical properties. Silicon steel sheet 35w360 has high magnetic induction intensity and can provide a strong magnetic field, which is suitable for high-power and high-frequency electronic equipment. In addition, its good thermal conductivity and mechanical strength also make it an ideal material for equipment such as motors and transformers. The technical parameters of silicon steel sheet 35w360 specifically include:
[0072] 1. Material: Silicon steel sheet 35w360;
[0073] 2. Size: thickness 0.35mm, width 150mm, length 1200mm;
[0074] 3. Magnetic properties: magnetic induction intensity B50 ≥ 1.72T, saturation magnetic induction intensity Bs ≥ 1.82T;
[0075] 4. Resistivity: ρ ≥ 80 μΩ·cm;
[0076] 5. Hardness: HV ≥ 200;
[0077] 6. Coating: Insulation coating, thickness is about 2-3μm;
[0078] 7. Insulation resistance: ≥1000MQ;
[0079] 8. Heat resistance: Maximum working temperature 155°C;
[0080] 9. Corrosion resistance: It has good corrosion resistance and can withstand corrosive media in common environments.
[0081] Silicon steel sheet 35w360 is particularly suitable for motor manufacturing. The high magnetic induction, high strength and good thermal conductivity of silicon steel sheet 35w360 make it an ideal material for motor manufacturing, such as generators, motors, etc.
[0082] In the current compressor industry, the commonly used specifications of the silicon steel sheet thickness of the stator 2 are 0.3mm, 0.35mm, and 0.5mm. Under the same structure, the thinner the thickness, the better the silicon steel performance. However, after the compressor housing 1 is heat-fitted, the thinner the thickness, the more susceptible it is to the housing stress. In summary, when the iron-nickel austenitic alloy housing in this embodiment is used, the silicon steel corresponding to the stator 2 needs to be 0.35mm thick and the grade needs to be S360. Furthermore, the hardness value needs to meet HV 铁镍奥氏体合金 :HV 定子 =1:1.2, the motor efficiency after shrink-fitting under the material combination of the compressor housing 1 and the stator 2 is the highest.
[0083] Several embodiments are provided below to compare the performance of the compressor housing 1 and the rotor compressor provided in this embodiment.
[0084] Embodiment 1:
[0085] The material of the compressor housing 1 is the existing cold-rolled steel, the core of the stator 2 is A35mm stacked, the core silicon steel sheet is 35W300 grade, the housing and the stator 2 are designed and assembled with 0.2mm interference, and after the stator 2 is hot-fitted, the iron loss corresponding to the core scheme is tested by an iron loss meter. The specific data is shown in Table 1. Here, the iron loss meter used is a special instrument for measuring core loss. It is mainly used to measure the energy loss generated by the core during operation, that is, iron loss. Iron loss includes hysteresis loss and eddy current loss. These losses occur when energy storage devices such as transistors and cables can no longer store energy, resulting in energy waste on the core. The iron loss meter uses advanced technology in modern science and technology to use electronic instruments to measure information such as core loss and magnetic flux density, so as to clarify the power and loss of the core.
[0086] Embodiment 2:
[0087] The structural dimensions of the compressor housing 1 and the stator 2 are consistent with those of Example 1, but the material of the compressor housing 1 is iron-nickel austenitic alloy, the iron core silicon steel sheet of the stator 2 is 35W300 grade, the housing and the stator 2 are designed and assembled with an interference fit of 0.2 mm, and after the stator 2 is heat-fitted, the iron loss corresponding to the iron core solution is tested using an iron loss tester. The specific data are shown in Table 1.
[0088] Embodiment 3:
[0089] The structural dimensions of the compressor housing 1 and the stator 2 are consistent with those of Example 1. The material of the compressor housing 1 is iron-nickel austenitic alloy, the iron core silicon steel sheet of the stator 2 is 35W360 grade, and the housing and the stator 2 are designed and assembled with an interference fit of 0.2 mm. After the stator 2 is heat-fitted, the iron loss corresponding to the iron core solution is tested using an iron loss tester. The specific data are shown in Table 1.
[0090] Embodiment 4:
[0091] The structural dimensions of the compressor housing 1 and the stator 2 are consistent with those of Example 1. The material of the compressor housing 1 is iron-nickel austenitic alloy, the iron core silicon steel sheet of the stator 2 is 35W360 grade, and the housing and the stator 2 are designed and assembled with an interference fit of 0.1 mm. After the stator 2 is heat-fitted, the iron loss corresponding to the iron core solution is tested using an iron loss tester. The specific data are shown in Table 1.
[0092] Embodiment 5:
[0093] The structural dimensions of the compressor housing 1 and the stator 2 are consistent with those of Example 1. The material of the compressor housing 1 is the invented iron-nickel austenitic alloy, the core silicon steel sheet of the stator 2 is 35W300 grade, and the housing and the stator 2 are designed and assembled with an interference fit of 0.1 mm. After the stator 2 is heat-fitted, the iron loss corresponding to the core solution is tested using an iron loss tester. The specific data are shown in Table 1.
[0094]
[0095] Table 1
[0096] It can be seen from Table 1 that the iron loss corresponding to Example 4 is the smallest, that is, the material of the compressor housing 1 is iron-nickel austenitic alloy, the iron core silicon steel sheet of the stator 2 is 35W360 grade, and when the housing and the stator 2 are designed and assembled with an interference fit of 0.1 mm, the iron loss generated by the iron core of the stator 2 is the smallest, and accordingly, the motor efficiency is the highest.
[0097] The various embodiments in the specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same and similar parts between the various embodiments can be referred to each other. For the system disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of this application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of this application.
[0098] It should also be noted that, in this specification, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "comprises", "comprising" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the statement "comprising a ..." does not exclude the presence of other identical elements in the process, method, article or device including the element.
Claims
1. A compressor housing, characterized in that: The compressor housing is made of an iron-nickel austenite alloy, and the components of the iron-nickel austenite alloy include: nickel, iron, chromium, manganese and titanium; The microstructure of the iron-nickel austenite alloy is equiaxed austenite grains.
2. The compressor housing according to claim 1, characterized in that The mass ratios of the nickel element, the iron element, the chromium element, the manganese element and the titanium element are 8% to 80%, 5% to 80%, 14% to 20%, 1% to 2% and 0% to 3% respectively.
3. The compressor housing according to claim 1, characterized in that The size of the equiaxed austenite grains is 15 to 25 μm.
4. The compressor housing according to claim 1, characterized in that The hardness of the iron-nickel austenitic alloy is 185-195 HV.
5. A rotary compressor, characterized in that: It comprises the compressor housing according to any one of claims 1 to 4 and a stator connected to the compressor housing.
6. The rotary compressor according to claim 5, characterized in that: The compressor housing and the stator are interference fit, and the interference amount is 0.09-0.11 mm.
7. The rotary compressor according to claim 5, characterized in that: A supporting portion for supporting the stator is provided at the lower end of the stator.
8. The rotary compressor according to claim 7, characterized in that: The supporting portion is a C-shaped snap ring, both ends of which are fixedly arranged on the stator, and the ring portion of the C-shaped snap ring is interference-fitted with the compressor housing.
9. The rotary compressor according to claim 8, characterized in that: The C-shaped clamping ring includes a plurality of stacked single sheets, and the thickness of each of the single sheets is less than 0.3 mm.
10. The rotary compressor according to claim 8, characterized in that: The tensile strength of the C-shaped clamping ring is greater than or equal to 850 MPa, and the elongation is 20% to 25%.
11. The rotary compressor according to claim 5, characterized in that: The hardness of the compressor housing is smaller than that of the stator, and a hardness ratio of the compressor housing to the stator is 1:1.1 to 1:1.5.
Citation Information
Patent Citations
Submicron austenite-strengthened high-strength steel sheet and preparation method thereof
CN104328336A
High-strength austenite light steel with high impact toughness and manufacturing method thereof
CN114892084A
Stainless steel alloy, turbocharger assembly formed therefrom, and method of manufacturing same
CN117265431A
Stator core and processing method thereof, motor and compressor
CN117639309A
Method for fabricating austenitic steel and compressor casing produced from said steel
CN1974799A