Pipeline metal coating corrosion evaluation method
Through high-temperature and high-pressure reactor simulation experiments and original coating analysis, the corrosion resistance of pipeline metal coatings is evaluated, which solves the gap in coating corrosion evaluation under harsh conditions and achieves accurate prediction of the service life of steel pipelines and resource saving.
Patent Information
- Application Number
- CN202410752916.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-08
AI Technical Summary
Existing technology is difficult to effectively evaluate the corrosion resistance of pipeline metal coatings under harsh conditions, resulting in severe corrosion of steel pipelines in high-temperature and highly corrosive media, affecting service safety and service life, and increasing production costs and resource consumption.
A high-temperature and high-pressure reactor was used to conduct corrosion simulation experiments and analyze the original coating before the experiment. By measuring the uniform corrosion rate, pitting corrosion rate and thinning amount of the coating, the corrosion resistance of the pipeline metal coating was comprehensively evaluated and its service life was evaluated.
It achieves an accurate assessment of the corrosion resistance of pipeline metal coatings, predicts local corrosion risks during long-term service, provides a reference for material selection, is fast and accurate, and has industrial application prospects.
Smart Images

Figure FDA0004888601550000011 
Figure HDA0004888601580000011 
Figure HDA0004888601580000012
Abstract
Description
Technical Field
[0001] The invention relates to a pipeline metal coating corrosion evaluation method. Background Art
[0002] Steel pipelines are one of the most important steel structures in the industrial and civil fields. They are used in large quantities in chemical production, oil and gas field exploitation, long-distance oil and gas transportation, urban pipeline networks and other fields, and play an indispensable role. However, they will inevitably corrode during use and service. Corrosion not only affects the service safety and life of steel pipelines, increases production and development costs, but also consumes precious energy and resources. A large number of steel pipelines are scrapped due to corrosion. The production of new steel pipelines will undoubtedly consume a lot of energy and increase carbon emissions. Improving the level of corrosion protection is conducive to increasing the service life of steel pipelines and reducing resource consumption and carbon emissions.
[0003] With the rapid development of metal surface treatment technology, material surface plating technology has been widely used. This technology has been widely used in many fields such as aerospace, machinery, chemical industry, petroleum, etc. with its unique advantages. Metal plating is currently the most widely used coating. Commonly used are Zn, Al, Cr, Ni, Cu, Fe and W. After the corrosion-resistant metal is plated on the surface of the pipeline, its corrosion resistance is significantly improved, but in some relatively harsh environments, such as high temperature and strong corrosive media, the corrosion of the metal plating is still very serious.
[0004] In order to evaluate the corrosion resistance of pipeline metal coatings under harsh conditions, a method suitable for metal coatings is needed to accurately evaluate their corrosion resistance. However, there is still a gap in this condition in China. In order to fill this gap, the present invention uses a high-temperature and high-pressure reactor to conduct corrosion simulation experiments and original coating analysis before the experiment, and defines a method for evaluating the corrosion resistance of pipeline metal coatings, which achieves the characteristics of saving time, economy, and high efficiency, and provides a reference index for material selection. Summary of the invention
[0005] The purpose of the present invention is to provide a method for evaluating the corrosion of pipeline metal coatings, which defines a method for evaluating the corrosion resistance of pipeline metal coatings and evaluates the applicability of materials for long-term service by performing corrosion simulation experiments using a high-temperature and high-pressure reactor and analyzing the original coating before the experiment.
[0006] The present invention provides a method for evaluating the corrosion of a metal coating on a pipeline, comprising the following steps: taking a metal-coated pipeline as a test material, and conducting a corrosion simulation experiment in a high-temperature and high-pressure reactor to determine the uniform corrosion rate of the coating of the metal-coated pipeline to judge the uniform corrosion resistance of the metal coating, to determine the pitting corrosion rate of the coating to judge the pitting corrosion resistance of the metal coating, to determine the thinning amount of the coating to judge the corrosion resistance of the metal coating, and to comprehensively evaluate the corrosion of the pipeline metal coating based on the uniform corrosion rate, the pitting corrosion rate, and the thinning amount of the coating data to evaluate the service life of the metal coating.
[0007] In the above method, the method further comprises analyzing the original coating of the metal-coated pipe before the corrosion simulation experiment;
[0008] The analysis of the original coating includes the thickness fluctuation of the original coating and the macroscopic and microscopic coating integrity inspection.
[0009] In the above method, the original coating is analyzed before the experiment, including the following steps:
[0010] 1) Samples were prepared from different positions of the original coated pipe. Two samples were cut from the top and bottom ring surfaces of the pipe at 3 o'clock, 6 o'clock, 9 o'clock, and 12 o'clock, for a total of 16 samples, which were divided into a coating surface group and a coating cross-section group, with 8 samples in each group;
[0011] 2) Observe the macroscopic morphology of all samples to ensure that the original coating has no macroscopic local damage, and check the microscopic coating in the secondary electron mode of the scanning electron microscope to ensure that the original coating has no microscopic local damage;
[0012] 3) The coating cross-section group samples were sealed with epoxy resin, and the coating cross-section was observed under the backscattering mode of the scanning electron microscope. The coating thickness fluctuation rate was calculated according to the following formula I:
[0013] Formula I
[0014] In Formula I, the coating thickness max refers to the maximum coating thickness in the pipeline, and the coating thickness min refers to the minimum coating thickness in the pipeline.
[0015] In the above method, the thickness fluctuation rate of the original coating is 0-5%, and there is no local damage to the macroscopic and microscopic coatings.
[0016] In the above method, when a corrosion simulation experiment is carried out using a high temperature and high pressure reactor, the following steps are included:
[0017] S1. Counting the basic parameters of the actual field application of the metal-coated pipeline, wherein the basic parameters include temperature, pressure, corrosive medium, flow velocity in the pipeline and anti-corrosion measures, and determining the corrosion environmental conditions and experimental parameters of the inner wall of the metal-coated pipeline according to the statistical results;
[0018] S2. Before conducting the experiment, the non-coated surface of the metal-coated pipe sample should be sealed to ensure that only the coated surface is in contact with the corrosive environment;
[0019] S3. Using a high-temperature and high-pressure reactor to simulate the on-site corrosion environment conditions of the metal-coated pipeline, a corrosion immersion test is performed at different constant temperatures. The experimental cycle is set to 72 to 336 hours, and the corrosive medium is a simulated on-site aqueous solution produced from the metal-coated pipeline.
[0020] In the above method, in step S3, the immersion solution used in the corrosion immersion test is a corrosive medium, and the corrosive medium is the same as the aqueous solution produced on-site from the metal-coated pipeline.
[0021] In the above method, the temperature and gas environment of the corrosion immersion test in step S3 are set to the temperature and gas environment of the metal-coated pipeline in actual service at the site in step S1.
[0022] In the present invention, a corrosion simulation test is conducted on the above-mentioned materials that have passed the original coating analysis. When conducting a high-temperature and high-pressure reactor test, at least three parallel samples should be ensured in each group to ensure the reliability of the data; the following steps are included:
[0023] (1) The non-coated surface of the metal-coated steel sample is sealed to ensure that only the coated surface is in contact with the corrosive environment;
[0024] (2) After the sealed sample is cleaned with deionized water, degreased with acetone, cleaned with anhydrous ethanol, and dried with cold air, the size of the coupon is measured and weighed. Each coupon needs to be measured three times and the data is recorded and the average value is taken. The data is retained to four decimal places to avoid affecting the evaluation results;
[0025] (3) Place the sample prepared in step (2) into a high-temperature and high-pressure reactor, add the aforementioned simulated pipeline on-site extraction aqueous solution, and completely immerse the sample. The prepared corrosion simulation solution needs to be deoxygenated by passing high-purity nitrogen gas, and the deoxygenation time shall not be less than 8 hours;
[0026] (4) The experimental parameters are determined according to the statistical results of the on-site pipeline service environment. The experimental period can be set between 72 and 336 hours. After the period, the corroded samples are taken out, rinsed with deionized water, dehydrated with anhydrous ethanol and blown dry.
[0027] In the above method, the uniform corrosion rate is measured by weight loss method with reference to standard ASTM G31. The greater the uniform corrosion rate, the worse the uniform corrosion resistance of the metal coating.
[0028] In the above method, the coating thinning amount is calculated by observing the cross section of the sample under the backscattering mode of the scanning electron microscope;
[0029] The corrosion resistance of the metal coating is determined by the amount of coating thinning combined with the duration of the experimental cycle and the surface area of the sample coating.
[0030] In the above method, the service life of the metal coating is evaluated according to the following steps:
[0031] a. For uniform corrosion, after the corrosion simulation experiment, the sample is pickled and the weight loss method is used to obtain the overall corrosion rate of the sample; the uniform corrosion rate of the sample is calculated by testing the weight change of the sample before and after the test, and the long-term corrosion rate of the metal coating is calculated based on the uniform corrosion rate value, and the service life of the metal coating is predicted and recorded as Y1;
[0032] b. For pitting, according to the specific situation of pitting, the pitting depth and distribution are tested by metallographic method, laser confocal mapping method or profile measurement method, the pitting rate is calculated, and the service life of the metal coating is predicted to be Y2;
[0033] c. For the cross-section analysis of the coating, determine the bonding between the metal coating and the substrate, check whether there are cracks in the metal coating, observe and measure the coating thickness of the sample before and after the experiment in the backscattering mode of the scanning electron microscope, calculate the coating thinning amount, calculate the corrosion rate based on the experimental cycle length and the surface area of the sample coating, and predict the service life of the coating, which is recorded as Y3;
[0034] The corrosion situation and service life of the coating are comprehensively determined by combining the above three evaluation indicators. The actual service life Y is the shortest of the three groups of prediction results Y1, Y2, and Y3, that is: Y = min{Y1, Y2, Y3}.
[0035] In the present invention, metallographic method and scanning electron microscope are used to analyze whether there is pitting corrosion in the on-site pipe section. If there is pitting corrosion, laser confocal microscopy is used to perform three-dimensional mapping of the pits to clarify the diameter, depth and distribution of the pits, and the pitting rate is calculated by the following formula II:
[0036] Formula II
[0037] The present invention has the following beneficial effects:
[0038] The uniform corrosion rate, pitting rate, and coating thinning data are used to comprehensively evaluate the corrosion resistance of metal coatings, analyze the strength of corrosion resistance, predict the local corrosion risk during long-term service, and determine the applicability and service life of long-term service materials under field conditions. This method is simple and easy to use, with fast and accurate evaluation, and has certain industrial application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 Schematic diagram of cutting and preparing nickel-tungsten coated steel samples.
[0040] Figure 2 This is the analysis diagram of the original coating of nickel-tungsten coated steel.
[0041] Figure 3 This is the corrosion rate diagram of nickel-tungsten coated steel under 68℃ / 130℃ simulated formation water solution + different CO2 partial pressures.
[0042] Figure 4 This is a diagram showing the pitting corrosion of nickel-tungsten coated steel under 68℃ / 130℃ simulated formation water solution + different CO2 partial pressures.
[0043] Figure 5 This is a measurement diagram of the coating thickness of nickel-tungsten coated steel under 130℃ simulated formation water solution + 1.21MPaCO2 partial pressure. DETAILED DESCRIPTION
[0044] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0045] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0046] In order to make the present invention more clearly understood, preferred embodiments are described in detail below with reference to the accompanying drawings.
[0047] Example
[0048] (1) The corrosion resistance of nickel-tungsten coated pipes (containing 14%wt W tungsten-plated pipes) under simulated working conditions (as shown in the data in Table 1-2) was evaluated. Figure 1 As shown in the figure, 16 original coating samples of 10mm×10mm×original thickness were cut from different parts of the nickel-tungsten coated steel (two samples were cut from each of the 3 o'clock, 6 o'clock, 9 o'clock and 12 o'clock directions of the top and bottom annular surfaces of the pipe, divided into a coating surface group and a coating cross-section group, with 8 samples in each group). The original coating surface and cross-section, macroscopic and microscopic tests were carried out. The results are shown in the figure. Figure 2Observe the macroscopic morphology of all samples to ensure that the original coating has no macroscopic local damage, check the microscopic coating in the secondary electron mode of the scanning electron microscope to ensure that the original coating has no microscopic local damage, observe the coating cross section in the backscattering mode of the scanning electron microscope, and require that the coating thickness fluctuation rate must be less than 5%;
[0049] The coating thickness fluctuation rate is calculated according to the following formula I:
[0050] Formula I
[0051] In Formula I, the coating thickness max refers to the maximum coating thickness in the pipeline, and the coating thickness min refers to the minimum coating thickness in the pipeline.
[0052] Table 1 Ion composition of formation water in the well area
[0053]
[0054] Table 2 Reservoir temperature and gas partial pressure in the well area
[0055]
[0056] (2) Cut the nickel-tungsten coated steel into 50 mm × 13 mm × original thickness. The corrosion coupons and the analysis samples of 10mm×10mm×original thickness are sealed with white insulating epoxy resin on the non-plated surface. After cleaning with deionized water, degreasing with acetone, cleaning with anhydrous ethanol, and drying with cold air, the coupons are measured and weighed. Each coupon needs to be measured three times and the data is recorded to take the average value, and the data is retained to four decimal places;
[0057] (3) Prepare a simulated formation water solution (as shown in Table 3). The prepared corrosion simulation solution needs to be deoxygenated by passing high-purity nitrogen. The deoxygenation time shall not be less than 8 hours. According to the experimental conditions, the samples are insulated from each other and installed on the corresponding experimental fixtures and placed in the autoclave.
[0058] Table 3 Composition of simulated formation water solution
[0059] Ion concentration, mg / L <![CDATA[Cl - ]]> <![CDATA[SO4 2- ]]> <![CDATA[HCO3 - ]]> <![CDATA[CO3 2- ]]> <![CDATA[Mg 2+ ]]> <![CDATA[Ca 2+ ]]> <![CDATA[Na + ]]> <![CDATA[K + <!-- 4 -->]]> Simulated formation water 3307 293 2948 10 5 35 3220 450
[0060] (4) The autoclave was sealed, and high-purity CO2 was introduced for 4 hours to remove the oxygen mixed in during the installation process. Then the temperature and pressure were adjusted to the experimental requirements, and the experiment was carried out according to the simulated working condition corrosion simulation experimental conditions in Table 4; the corrosion cycle was 336 hours, and the corroded sample was taken out after 336 hours, and then acid-washed and rinsed with deionized water, dehydrated with anhydrous ethanol and blown dry, and weighed again to record the data;
[0061] Table 4 Simulated working conditions corrosion simulation test conditions
[0062]
[0063] (5) The specific evaluation process is as follows:
[0064] a. According to the standard ASTM G31, the uniform corrosion rate is calculated by the weight loss method. The calculation formula of uniform corrosion rate by weight loss method is:
[0065]
[0066] Where: C i is the uniform corrosion rate, mm / y; W 0i is the original weight of the sample before corrosion, g; W 1i is the weight of the sample after pickling, g; t is the corrosion simulation test period, h; ρ is the density of the metal material, g / cm 3 ; S is the sample exposure area, cm 2 ;
[0067] The corrosion rate of nickel-tungsten coated steel in 68℃ / 130℃ simulated formation water solution + different CO2 partial pressures, such as Figure 3 As shown,
[0068] b. Use metallographic method and scanning electron microscope to analyze whether there is pitting corrosion in the on-site pipe section. If there is pitting corrosion, use laser confocal microscope to conduct three-dimensional mapping of the pits to clarify the diameter, depth and distribution of the pits, and calculate the pitting rate by the following formula:
[0069]
[0070] Pitting corrosion of nickel-tungsten coated steel at 68℃ / 130℃ simulated formation water solution + different CO2 partial pressures, such as Figure 4 As shown;
[0071] c. After the cross-sections of the taken out analysis samples and the original samples are sealed and cured with epoxy resin, the cross-sections are polished to 2000 mesh and then observed using a scanning electron microscope backscattering mode to measure the original coating thickness and the coating thickness after the corrosion simulation experiment, and the coating thinning amount is obtained to calculate the corrosion rate;
[0072] The coating thickness of nickel-tungsten coated steel was measured at 130℃ simulated formation water solution + 1.21MPaCO2 partial pressure. The results are as follows Figure 5 As shown;
[0073] d. Based on the obtained data, the service life of the coating is predicted to be Y1, Y2, and Y3. The actual life Y is the shortest predicted period among the three groups of prediction results, that is, Y = min{Y1, Y2, Y3}.
[0074] Taking the coating thickness of 129μm as an example, the determination results of specific years are shown in Table 5.
[0075] Table 5 Service life of coating Y
[0076] Serial number condition Y1 Y2 Y3 Y 1 <![CDATA[68℃、CO2=0.24MPa]]> 12.90 3.52 0.13 0.13 2 <![CDATA[68℃、CO2=0.30MPa]]> 6.14 2.72 4.95 2.72 3 <![CDATA[68℃、CO2=1.21MPa]]> 5.86 1.97 0.33 0.33 4 <![CDATA[130℃、CO2=0.24MPa]]> 3.00 2.68 1.65 1.65 5 <![CDATA[130℃、CO2=0.30MPa]]> 2.48 2.11 0.99 0.99 6 <![CDATA[130℃、CO2=1.21MPa]]> 2.19 2.25 2.47 2.19
[0077] The above embodiments specifically illustrate the present invention, but the present invention is not limited thereto. Any modifications or amendments made according to the method of the present invention belong to the protection scope of the present invention.
Claims
1. A pipeline metal coating corrosion evaluation method, characterized in that: The method comprises the following steps: taking a metal-coated pipeline as a test material, and conducting a corrosion simulation experiment by adopting a high-temperature and high-pressure reactor to determine the uniform corrosion rate of the coating of the metal-coated pipeline to judge the uniform corrosion resistance of the metal coating, determining the pitting corrosion rate of the coating to judge the pitting corrosion resistance of the metal coating, and determining the thinning amount of the coating to judge the corrosion resistance of the metal coating; and comprehensively evaluating the corrosion of the pipeline metal coating according to the uniform corrosion rate, the pitting corrosion rate, and the thinning amount of the coating to evaluate the service life of the metal coating. The uniform corrosion rate of the coating is used to judge the uniform corrosion resistance of the metal coating, the pitting corrosion rate of the coating is used to judge the pitting corrosion resistance of the metal coating, and the corrosion resistance of the metal coating is judged by the thinning amount of the coating. The service life of the metal coating is evaluated by comprehensively combining the uniform corrosion rate, pitting rate and coating thinning amount data.
2. The method according to claim 1, characterized in that: The method further comprises analyzing the original coating of the metal-coated pipe before the corrosion simulation experiment; The analysis of the original coating includes the thickness fluctuation of the original coating and the macroscopic and microscopic coating integrity inspection.
3. The method according to claim 2, characterized in that The original coating is analyzed before the experiment, including the following steps: 1) Samples were prepared from different positions of the original coated pipe. Two samples were cut from the top and bottom ring surfaces of the pipe at 3 o'clock, 6 o'clock, 9 o'clock, and 12 o'clock, for a total of 16 samples, which were divided into a coating surface group and a coating cross-section group, with 8 samples in each group; 2) Observe the macroscopic morphology of all samples to ensure that the original coating has no macroscopic local damage, and check the microscopic coating in the secondary electron mode of the scanning electron microscope to ensure that the original coating has no microscopic local damage; 3) The coating cross-section group samples were sealed with epoxy resin, and the coating cross-section was observed under the backscattering mode of the scanning electron microscope. The coating thickness fluctuation rate was calculated according to the following formula I: Formula I In Formula I, the coating thickness max refers to the maximum coating thickness in the pipeline, and the coating thickness min refers to the minimum coating thickness in the pipeline.
4. The method according to claim 2 or 3, characterized in that: The thickness fluctuation rate of the original coating is 0-5%, and there is no local damage to the coating in the macroscopic and microscopic aspects.
5. The method according to claim 1 or 2, characterized in that: When using a high temperature and high pressure reactor for corrosion simulation experiments, the following steps are included: S1. Counting the basic parameters of the actual field application of the metal-coated pipeline, wherein the basic parameters include temperature, pressure, corrosive medium, flow velocity in the pipeline and anti-corrosion measures, and determining the corrosion environmental conditions and experimental parameters of the inner wall of the metal-coated pipeline according to the statistical results; S2. Before conducting the experiment, the non-coated surface of the metal-coated pipe sample should be sealed to ensure that only the coated surface is in contact with the corrosive environment; S3. Using a high-temperature and high-pressure reactor to simulate the on-site corrosion environment conditions of the metal-coated pipeline, a corrosion immersion test is performed at different constant temperatures. The experimental cycle is set to 72 to 336 hours, and the corrosive medium is a simulated on-site aqueous solution produced from the metal-coated pipeline.
6. The method according to claim 5, characterized in that In step S3, the immersion solution used in the corrosion immersion test is a corrosive medium, and the corrosive medium is the same as the aqueous solution produced on-site in the metal-coated pipeline.
7. The method according to claim 5 or 6, characterized in that: The temperature and gas environment of the corrosion immersion test in step S3 are set to the temperature and gas environment of the metal-coated pipeline in actual service at the site in step S1.
8. The method according to any one of claims 1 to 7, characterized in that The uniform corrosion rate is measured by the weight loss method according to the standard ASTM G31. The greater the uniform corrosion rate, the worse the uniform corrosion resistance of the metal coating.
9. The method according to any one of claims 1 to 8, characterized in that The coating thinning amount is calculated by observing the cross section of the sample under the backscattering mode of the scanning electron microscope; The corrosion resistance of the metal coating is determined by the coating thinning amount combined with the experimental cycle length and the surface area of the sample coating.
10. The method according to any one of claims 1 to 9, characterized in that The following steps are used to evaluate the service life of the metal coating: a. For uniform corrosion, after the corrosion simulation experiment, the sample is pickled and the weight loss method is used to obtain the overall corrosion rate of the sample; the uniform corrosion rate of the sample is calculated by testing the weight change of the sample before and after the test, and the long-term corrosion rate of the metal coating is calculated based on the uniform corrosion rate value, and the service life of the metal coating is predicted and recorded as Y1; b. For pitting, according to the specific situation of pitting, the pitting depth and distribution are tested by metallographic method, laser confocal mapping method or profile measurement method, the pitting rate is calculated, and the service life of the metal coating is predicted to be Y2; c. For the cross-section analysis of the coating, determine the bonding between the metal coating and the substrate, check whether there are cracks in the metal coating, observe and measure the coating thickness of the sample before and after the experiment in the backscattering mode of the scanning electron microscope, calculate the coating thinning amount, calculate the corrosion rate based on the experimental cycle length and the surface area of the sample coating, and predict the service life of the coating, which is recorded as Y3; The corrosion situation and coating service life are comprehensively determined by combining the above three evaluation indicators. The actual service life Y is the shortest of the three groups of prediction results Y1, Y2, and Y3.