Method and device for testing anti-icing property of anti-icing coating
By employing freeze-thaw cycle testing and a rotating impact force sensor, the shortcomings of existing anti-icing coating testing methods have been overcome. This approach enables accurate evaluation of the anti-icing performance of hydrophobic coatings, improves testing precision and stability, and reduces energy consumption and structural damage.
Patent Information
- Application Number
- CN202410670852.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-28
- Publication Date
- 2024-10-08
AI Technical Summary
Existing anti-icing coating testing methods cannot effectively evaluate the anti-icing performance of hydrophobic coatings under long-term immersion in water, and traditional testing methods are inefficient, destructive to the structure, and energy-intensive.
A freeze-thaw cycle test simulating winter icing and melting in channels is conducted. By rotating the sample to make the ice layer impact the sensor, shear force and ice residue rate are measured. Combined with infrared thermal imaging analysis of freezing time and morphology, an ice-resistant testing method and device are provided.
Accurate assessment of changes in the anti-icing performance of hydrophobic coatings under long-term immersion in water improves the accuracy and stability of testing, and reduces structural damage and energy consumption.
Smart Images

Figure CN118746547A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of anti-icing coatings, and more specifically, to a method and device for testing the anti-icing properties of anti-icing coatings. Background Art
[0002] Winter freezing is common in cold regions of my country, and freezing damage has brought many adverse effects on the construction, operation, maintenance and ecological environment of water conservancy and hydropower projects. For (ultra) long-distance water diversion projects, such as the typical South-to-North Water Diversion Project, which stretches thousands of kilometers and crosses different climate zones in my country, concrete materials, as one of the most important building materials for water diversion channels, are easily affected by winter freezing and frost heave damage; on the other hand, the freezing problem affects the flow capacity of the channel, causing damage to hydraulic structures, and even threatening people's lives, health and property. The current solutions mainly include gradually raising the water level to facilitate the formation of an ice cover so that water can be transferred stably under the ice cover; setting up ice cables, ice-breaking piers and ice-proof fences to prevent ice blockage; installing passive anti-icing technologies such as heating equipment, which have problems such as low work efficiency, damage to the concrete structure itself, and high energy consumption.
[0003] Applying a hydrophobic coating on the channel surface can inhibit channel icing to a certain extent and facilitate the removal of floating ice. Current research mainly focuses on the anti-icing performance of road surfaces, and obtains the ice bonding strength or ice volume of the coating by simulating natural conditions such as frost, rain and snow. The long-term water-soaked environment of the channel requires higher durability of the coating. The existing research methods cannot effectively support the coating to maintain good anti-icing performance in a long-term water-soaked environment. Therefore, it is necessary to design a new test method for evaluation. Summary of the invention
[0004] The present application provides an anti-icing property testing method and device for an anti-icing coating. By continuously freezing and thawing samples to simulate ice formation and melting in channels in winter, a unique ice layer impact method is used to accurately obtain shear force and ice residual rate, which can more accurately reflect changes in the anti-icing performance of the hydrophobic coating in a long-term water immersion environment.
[0005] In a first aspect, the present application provides a method for testing the anti-icing property of an anti-icing coating, using the following technical solution:
[0006] A method for testing the anti-icing property of an anti-icing coating comprises the following steps:
[0007] Freezing treatment: Freezing the sample to form an ice layer on the sample;
[0008] Ice layer impact: The sample is rotated and dropped, so that the ice layer hits the force sensor. The motion trajectory of the sample is an arc, and the ice layer contacts the force sensor along the circumferential direction of the sample motion trajectory.
[0009] Parameter acquisition: When the ice layer is peeled off, the force of the force sensor is recorded as the shear force during ice peeling, and the ice residual rate of the sample is calculated;
[0010] Freeze-thaw cycle test: After completing the calculation of shear force and ice residue, melt the ice layer of the sample, then repeat all steps and calculate the change rate of the final ice residue;
[0011] When the shear force change rate is no more than 15% and the ice residue change rate is no more than 15%, it indicates that the anti-icing property of the anti-icing coating is qualified.
[0012] By adopting the above technical solution, compared with the traditional method of directly applying shear force on the ice layer of the sample to achieve the peeling of the ice layer, the present application makes the sample actively fall and hit the force sensor, so that the size of the shear force on the sample can be directly obtained, and the confirmation of the shear force is more convenient and more accurate. In addition, since the sample of the present application falls in a rotation, when the sample contacts the force sensor along the circumferential direction of the motion trajectory, there are centripetal force and gravity generated by the swing on the sample. Such force acts on the ice layer, and the ice residual rate can be obtained more accurately and stably, which can more accurately reflect the changes in the anti-icing performance of the hydrophobic coating in a water-immersed environment. In addition, the present application simulates the ice formation and melting of the channel in winter through a freeze-thaw cycle test, and combines the shear force and ice residual rate changes obtained by the test method of the present application, and compares the test results after the freeze-thaw cycle test, which can more accurately reflect the changes in the anti-icing performance of the hydrophobic coating in a long-term water-immersed environment.
[0013] Furthermore, the contact surface between the ice layer and the force sensor is rectangular, 30 to 50 mm long and 5 to 30 mm wide.
[0014] Furthermore, the ice layer has a thickness of 5-15 mm.
[0015] Further, the mass of the sample is 200-3000 g, further 325-2750 g, and the distance S between the center of the sample and the center of the sample motion trajectory is 50-70 cm. It should also be noted that the mass of the sample here refers to the mass excluding the ice layer.
[0016] Furthermore, the angle α between the starting point of the sample running track and the vertical line is 5 to 45°. The arc center angle β of the sample running track is (180°-angle α) to (170°-angle α).
[0017] Furthermore, in the freeze-thaw cycle test step, the test is repeated 8-24 times.
[0018] Furthermore, in the freezing process, the freezing process on the sample surface is photographed to determine the freezing time.
[0019] In a second aspect, the present application provides an anti-icing property test of an anti-icing coating, using the following technical solution:
[0020] A device for testing the anti-icing property of an anti-icing coating comprises a bracket, a force sensor, a fixed rod, and a swing rod, wherein the force sensor is mounted on the bracket, the fixed rod is fixedly connected to the bracket, one end of the swing rod is rotatably connected to the top end of the fixed rod, and a clamp for mounting a sample is provided at one end of the swing rod away from the fixed rod.
[0021] In summary, this application has the following beneficial effects:
[0022] This application simulates the ice formation and melting of channels in winter by immersing samples in water for a long time and performing freeze-thaw operations continuously, which can more accurately reflect the changes in the anti-icing performance of the hydrophobic coating in a long-term water immersion environment; this application uses an infrared thermal imager to objectively analyze and compare the ice condensation time and ice condensation morphology on the sample surface under different freeze-thaw cycles; this application also invents a simple method to measure ice shear force, and according to the inertia of the falling specimen, more accurately obtains the shear force and ice residual rate during ice peeling. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a schematic diagram of the sample structure in the embodiment of this application.
[0024] Figure 2 It is a schematic diagram of the test device structure in the embodiment of the present application.
[0025] Figure 3 It is a schematic diagram of the clamp structure in an embodiment of the present application.
[0026] Figure 4 Schematic diagram of the force sensor structure in the embodiment of the present application.
[0027] Explanation of the reference numerals: 1. sample; 11. coating; 12. ice layer; 2. bracket; 21. fixing rod; 22. swing rod; 3. clamp; 31. substrate; 32. screw; 33. clamp; 4. force sensor; 41. impact block; 5. mounting plate; 51. positioning rod; 52. fixing groove. DETAILED DESCRIPTION
[0028] The present application is further described in detail below with reference to the accompanying drawings and embodiments.
[0029] Example
[0030] The present application provides a method for testing the anti-icing property of an anti-icing coating, comprising the following steps:
[0031] Freezing treatment: Sample 1 is subjected to freezing treatment to form an ice layer 12 on the coating 11 of sample 1. After freezing, sample 1 Figure 1The specific operations are as follows:
[0032] The surface of the sample 1 is fully coated with paint and placed in a water tank, with 3 / 4 of the sample immersed in water, ensuring that only the peeled surface of the sample is frozen to form an ice layer 12. The thickness of the ice layer is 5-15 mm.
[0033] Furthermore, during the freezing process, an infrared thermal imager is used to photograph the freezing process on the surface of sample 1 every 30 seconds to determine the freezing time.
[0034] Ice layer impact: Rotate the sample 1 and drop it so that the ice layer 12 hits the force sensor. The motion trajectory of the sample 1 is an arc, and the ice layer 12 contacts the force sensor along the circumferential direction of the motion trajectory of the sample 1. The specific operation is as follows:
[0035] The sample 1 is fixed on the test device so that the ice layer 12 to be tested is opposite to each other along the circumferential direction of the sample motion trajectory. In addition, the size and shape of the contact surface between the ice layer 12 and the force sensor are adjusted by adjusting the size of the contact surface of the force sensor. Specifically, the contact surface between the ice layer 12 and the force sensor is rectangular. The contact surface between the ice layer 12 and the force sensor is 30 to 50 mm long and 5 to 30 mm wide.
[0036] The mass of sample 1 is 200 to 3000 g, and it should be noted that this refers to the total mass of sample 1 with ice layer 12. The distance S between the center of sample 1 and the center of the trajectory of sample 1 is 50 to 70 cm. The angle α between the starting point of the trajectory of sample 1 and the vertical line is 5 to 45°. The degree of the arc center angle β of the trajectory of sample 1 is (180°-angle α) to (170°-angle α).
[0037] Parameter acquisition: When the ice layer 12 is peeled off, the force of the force sensor is recorded as the shear force when the ice layer 12 is peeled off. The peeling surface is photographed with an infrared thermal imager to determine the ice residual rate.
[0038] Freeze-thaw cycle test: After completing the calculation of shear force and ice residue, melt the ice layer 12 of the sample and then repeat all the steps. The specific operation is as follows:
[0039] Increase the temperature of the incubator (no more than 10°C) to completely melt the ice. Then repeat the ice treatment, ice surface impact, parameter acquisition and freeze-thaw cycle test steps. In the freeze-thaw cycle test step, repeat the test 8-24 times. Calculate the change rate of the final ice residue.
[0040] When the shear force change rate is no more than 15% and the ice residue change rate is no more than 15%, it indicates that the anti-icing property of the anti-icing coating is qualified.
[0041] In addition, the coating applied on the surface of the sample in the embodiment of the present application is commercial fluorosilane, specifically a waterproof coating, similar to Neverwet Ultra-Ever Dry, which is super dry, wear-resistant and super hydrophobic, and has good long-term anti-icing performance.
[0042] Furthermore, an embodiment of the present application also provides a device for testing the anti-icing properties of the above-mentioned detection method.
[0043] like Figure 2 and Figure 3 As shown, a device for testing the anti-icing property of an anti-icing coating 11 includes a bracket 2, a force sensor 4, a fixed rod 21, and a swing rod 22. The fixed rod 21 is fixedly connected to the vertical side wall of the bracket 2, one end of the swing rod 22 is rotatably connected to the top of the fixed rod 21 and the rotation axis is horizontal, and the end of the swing rod 22 away from the fixed rod 21 is connected to a clamp 3. The clamp 3 in this embodiment includes two base plates 31 relatively connected to the side walls of the swing rod 22, a screw rod 32 threadedly connected to each base plate 31, the screw rod 32 passes through the corresponding base plate 31, and the two screw rods 32 are located on the end walls on the opposite sides of the two base plates 31 and are fixedly connected to clamp plates 33.
[0044] like Figure 2 and Figure 4 As shown, the fixing rod 21 is rotatably connected to the vertical side wall on the side away from the bracket 2, and the rotation axis of the fixing plate 5 is horizontal and in the same direction as the swing rod 22. A plurality of fixing grooves 52 are arranged on the side wall of the fixing plate 5 facing the swing rod 22, and the fixing grooves 52 are arranged along the rotation circumference of the fixing plate 5. The fixing rod 21 is threadedly connected to the positioning rod 51, and the positioning rod 51 passes through the fixing rod 21 and is inserted into a corresponding fixing groove 52 and fits with the groove wall of the fixing groove 52. The force sensor 4 is installed on the side of the mounting plate 5 away from the bracket 2. At the same time, the force-bearing end of the force sensor 4 is detachably connected to the impact block 41, which can be connected by magnetic attraction, adhesion, etc., and can be replaced with different sizes as needed to change the contact surface between the force sensor 4 and the ice layer 12; the impact block 41 and the force sensor 4 are located on the movement track of the ice layer 12 of the sample 1.
[0045] According to the test requirements, the mounting plate 5 is rotated so that the force sensor 4 is at a suitable angle, and then the positioning rod 51 is inserted into the corresponding fixing groove 52, and the mounting plate 5 is fixed. According to the shape and size of the contact surface between the force sensor 4 and the sample 1 in the test, a suitable impact block 41 is selected and installed on the mounting plate 5; then the sample 1 is placed between the two clamping plates 33, and the screw rod 32 is rotated so that the clamping plates 33 clamp the sample 1. Then the sample 1 is pulled to a suitable height so that the sample 1 swings downward with the swing rod 22, and the ice surface of the sample 1 hits the impact block 41.
[0046] The following is explained by specific examples.
[0047] The difference between Examples 1-15 is that in the anti-icing property test method, the parameters of the operation process are different, as shown in Tables 1 to 3. Each example is tested twice.
[0048] Table 1 Test method parameter table of Examples 1-5
[0049]
[0050]
[0051] Table 2 Test method parameters of Examples 6-10
[0052]
[0053]
[0054] Table 3 Test method parameters of Examples 11-15
[0055]
[0056]
[0057]
[0058] Test method accuracy analysis
[0059] For commercial fluorosilane coatings, they have good hydrophobicity, so they have good applications in anti-icing coatings. It can be seen from the test results of Examples 1-10 that according to the evaluation criteria of this application (when the shear force change rate is not greater than 15%, the change rate of ice residue is not greater than 15%, indicating that the anti-icing property of the anti-icing coating is qualified), the coating test results of Examples 1-10 are all qualified, indicating that the test results of Examples 1-10 have a certain degree of accuracy. Among them, the first shear force and the last shear force of each example, as well as the first ice residue rate and the last ice residue rate, have certain changes, which is caused by the change of the anti-icing performance of the coating after the freeze-thaw cycle.
[0060] By observing the test results of each embodiment in Examples 1-10, it can be seen that the shear force change rate and ice residual rate change rate of the two test results of the same embodiment are not much different, which shows that the detection process of Example 1-10 has good detection stability. Further analysis of the test results of Examples 11-15 shows that although the test results of Examples 11-15 are still qualified, the two results of each embodiment of Examples 11-15 have a large difference, indicating that the detection stability of Examples 11-15 is poor. This may be because the contact surface conditions of the ice layer and the force sensor and the sample movement conditions under the definition of Example 1-10 are more conducive to obtaining accurate shear force and ice residual rate.
[0061] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for testing the anti-icing property of an anti-icing coating, characterized in that: The following steps are involved: Freezing treatment: Freezing the sample to form an ice layer on the sample; Ice layer impact: The sample is rotated and dropped, so that the ice layer hits the force sensor. The motion trajectory of the sample is an arc, and the ice layer contacts the force sensor along the circumferential direction of the sample motion trajectory. Parameter acquisition: When the ice layer is peeled off, the force of the force sensor is recorded as the shear force during ice peeling, and the ice residual rate of the sample is calculated; Freeze-thaw cycle test: After completing the calculation of shear force and ice residue, melt the ice layer of the sample, then repeat all steps and calculate the change rate of the final ice residue; When the shear force change rate is no more than 15% and the ice residue change rate is no more than 15%, it indicates that the anti-icing property of the anti-icing coating is qualified.
2. The method for testing the anti-icing property of an anti-icing coating according to claim 1, characterized in that: The contact surface between the ice layer and the force sensor is rectangular.
3. The method for testing the anti-icing property of an anti-icing coating according to claim 2, characterized in that: The contact surface between the ice layer and the force sensor is 30 to 50 mm long and 5 to 30 mm wide.
4. The method for testing the anti-icing property of an anti-icing coating according to claim 1, characterized in that: The thickness of the ice layer is 5-15 mm.
5. The method for testing the anti-icing property of an anti-icing coating according to claim 1, characterized in that: The mass of the sample is 200-3000 g, and the distance S between the center of the sample and the center of the sample movement trajectory is 50-70 cm.
6. The method for testing the anti-icing property of an anti-icing coating according to claim 5, characterized in that: The angle α between the starting point of the sample running track and the vertical line is 5 to 45°.
7. The method for testing the anti-icing property of an anti-icing coating according to claim 6, characterized in that: The arc center angle β of the sample running track is (180°-angle α) to (170°-angle α).
8. The method for testing the anti-icing property of an anti-icing coating according to claim 1, characterized in that: In the freeze-thaw cycle test step, the test is repeated 8-24 times.
9. The method for testing the anti-icing property of an anti-icing coating according to claim 1, characterized in that: In the freezing process, the freezing process on the sample surface is photographed to determine the freezing time.
10. A device for testing the anti-icing property of an anti-icing coating, characterized in that: It includes a bracket, a force sensor, a fixed rod, and a swing rod. The force sensor is installed on the bracket. The fixed rod is fixedly connected to the bracket. One end of the swing rod is rotatably connected to the top end of the fixed rod. A clamp for mounting a sample is provided at one end of the swing rod away from the fixed rod.