Preparation method of photoelectric device

By using an oxygen-free water vapor environment for energization and illumination during the preparation process of the optoelectronic device, the defect density of the electron transport layer is reduced, the problem of poor performance and life of the optoelectronic device in the existing technology is solved, and efficient optoelectronic device preparation is achieved .

CN118748232APending Publication Date: 2024-10-08ZHEJIANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410718340.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing optoelectronic devices have defective states during the preparation process, resulting in poor performance of the electron transport layer, affecting device efficiency and lifespan, and traditional processing methods cannot achieve a defect-free oxide semiconductor electron injection layer.

Method used

When preparing an optoelectronic device, place it in an oxygen-free water vapor environment for electrical treatment and/or light treatment, and use water vapor and photochemical reactions to reduce the defect density of the electron transport layer and build an ideal ohmic contact.

Benefits of technology

It significantly improves the performance and life of optoelectronic devices, achieves low or no electron defect states, improves the internal quantum efficiency and open circuit voltage of the device, and solves the problem that traditional methods cannot meet the needs of industrialization.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748232A_ABST
    Figure CN118748232A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of a photoelectric device, and the method comprises the steps: preparing an electron transmission layer on a substrate with a first electrode, and the material of the electron transmission layer is n-type oxide semiconductor nanocrystalline; preparing a second electrode on the electron transport layer to obtain a photoelectric device to be processed; after the to-be-processed photoelectric device is placed in the oxygen-free water vapor environment for a certain time, the to-be-processed photoelectric device is subjected to power-on processing and / or illumination processing, and the photoelectric device is obtained; wherein the relative humidity of the environment is 5-85%, oxygen-free means that the oxygen content is smaller than or equal to 100 ppm, and the second electrode is made of metal. The preparation method passivates the defects of the electron transport material, improves the performance of the photoelectric device and prolongs the service life of the photoelectric device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to optoelectronic device technology, and in particular, to a method for preparing an optoelectronic device. Background Art

[0002] N-type oxide semiconductor nanoparticles have solution processability and are particularly suitable for making large-area optoelectronic devices. They are widely used as electron injection or electron transport layers in optoelectronic devices such as light-emitting diodes and solar cells. However, defect states will inevitably be generated during the preparation of nanoparticle materials and subsequent device preparation processes. For n-type semiconductor materials, the presence of these defect states will capture conduction band free electrons, thereby significantly reducing the electron concentration and mobility of the material, and will also cause invalid recombination currents through defect recombination channels, reducing device efficiency. On the other hand, if the defect concentration of the transport layer is too high, it will affect the construction of ohmic contact between the electrode and the electrode, affecting electron injection.

[0003] In the past, people have found that the improvement in the performance of the electron transport layer is related to the acidic substances in the encapsulation glue used for encapsulation, but the process is relatively complicated, uncontrollable, and cannot be mass-produced. People have proposed various ways to improve the effective charge transfer capacity of the electron transport layer, including using an acidic atmosphere to treat the electron transport layer, placing the electron transport layer in a humid environment, and adding acid generators to the electron transport layer. However, the effects of these solutions are either to increase the device current and luminescence brightness, and slightly increase efficiency; or to increase efficiency and slightly increase current and luminescence brightness. This shows that the electron transport layer treatment solutions that have been disclosed in the past cannot achieve the ideal goal of a 'defect-free oxide semiconductor electron injection layer'.

[0004] The high-performance quantum dot light-emitting diodes (QLEDs) reported so far still have the problem that their luminescence performance and lifespan do not meet the needs of industrialization. Summary of the invention

[0005] The purpose of the present disclosure is to provide a method for preparing a photoelectric device to solve the problem of poor performance and life of the photoelectric device.

[0006] In a first aspect, a method for preparing a photoelectric device is provided, the method comprising: preparing an electron transport layer on a substrate having a first electrode, wherein the material of the electron transport layer is n-type oxide semiconductor nanocrystals; preparing a second electrode on the electron transport layer to obtain a photoelectric device to be processed; placing the photoelectric device to be processed in an oxygen-free water vapor environment for a certain period of time, and then performing an electrical treatment and / or light treatment on the photoelectric device to be processed to obtain the photoelectric device; wherein the relative humidity of the environment is 5-85%, oxygen-free means that the oxygen content is less than or equal to 100 ppm, and the material of the second electrode is metal.

[0007] Optionally, the material of the second electrode includes one or more of Ag, Au, Al, Mg, Zn, Ti, Ca, Cr, Cu, and Zr.

[0008] Optionally, the n-type oxide semiconductor nanocrystals are metal oxide nanocrystals, and the metal oxide nanocrystals are selected from zinc oxide, zinc oxide doped with metal elements, titanium oxide or tin oxide. Preferably, the average diameter of the metal oxide nanocrystals is 1-20 nm.

[0009] Optionally, the substrate having the first electrode includes a substrate, a first electrode, a hole injection layer, a hole transport layer and a quantum dot light-emitting layer.

[0010] Optionally, the certain period of time is greater than or equal to 1 minute and less than or equal to 3 days; preferably, the certain period of time is less than or equal to 60 minutes.

[0011] Optionally, the electron transport layer has a film thickness of 30-100 nm.

[0012] Optionally, the second electrode has a thickness of 30-200 nm.

[0013] Optionally, the ambient temperatures of the water vapor post-processing, the power-on post-processing and the light post-processing are all room temperature.

[0014] Optionally, the power-on treatment lasts for 1-600s.

[0015] Optionally, the voltage of the power-on process is greater than 0 and less than or equal to 20V.

[0016] Optionally, the power-on treatment is performed multiple times, and the interval between the multiple power-on treatments is greater than 0 and less than or equal to 10 minutes.

[0017] Optionally, a peak wavelength of a light source for the light treatment is shorter than a band gap wavelength of the n-type oxide semiconductor nanocrystal.

[0018] Optionally, the peak wavelength of the light source of the light treatment is shorter than the band gap wavelength of the quantum dot light-emitting layer.

[0019] Optionally, before the power-on treatment or the light-irradiation treatment, the photoelectric device after the water vapor treatment is packaged.

[0020] Optionally, the optoelectronic device is a quantum dot light emitting diode, a solar cell, a photodetector or a laser.

[0021] By applying the technical solution disclosed in the present invention, the optoelectronic device has better performance and lifespan, and the preparation method of the optoelectronic device has industrial feasibility, which greatly promotes the industrial application of optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting part of the present application are used to provide a further understanding of the present disclosure. The exemplary embodiments of the present disclosure and their descriptions are used to explain the present disclosure and do not constitute an improper limitation on the present disclosure. In the drawings:

[0023] Figure 1 The present invention is a schematic diagram of a process for preparing a photoelectric device according to an embodiment of the present invention.

[0024] Figure 2 The voltage-current density-brightness curve of the QLED device according to an embodiment of the present disclosure (before power-on treatment) is shown.

[0025] Figure 3 The current density-external quantum efficiency curve of the QLED device according to one embodiment of the present disclosure (before power-on treatment) is shown.

[0026] Figure 4 The voltage-current density-brightness curve of the QLED device according to an embodiment of the present disclosure (after power-on treatment) is shown.

[0027] Figure 5 The current density-external quantum efficiency curve of the QLED device according to an embodiment of the present disclosure (after power-on treatment) is shown.

[0028] Figure 6 The voltage-current density curve of the QLED device according to an embodiment of the present disclosure (after 1 to 7 power-on treatments) is shown.

[0029] Figure 7 The voltage-brightness curve of the QLED device according to an embodiment of the present disclosure (after 1 to 7 power-on treatments) is shown.

[0030] Figure 8 The voltage-external quantum efficiency curve of the QLED device according to an embodiment of the present disclosure (after 1 to 7 power-on treatments) is shown.

[0031] Fig. 9 Graphs showing time-voltage and time-relative brightness of a QLED device according to an embodiment of the present disclosure (before and after treatment) at a specific current density.

[0032] Fig.10 The voltage-current density-brightness curve of a QLED device of a comparative example (before power-on treatment) of the present disclosure is shown.

[0033] Fig.11 The current density-external quantum efficiency curve of a QLED device of a comparative example (before power-on treatment) of the present disclosure is shown.

[0034] Fig.12The voltage-current density-brightness curve of a QLED device of a comparative example (after power-on treatment) of the present disclosure is shown.

[0035] Fig.13 The current density-external quantum efficiency curve of a QLED device of a comparative example (after power-on treatment) of the present disclosure is shown.

[0036] Fig.14 The voltage-current density curve of the QLED device according to an embodiment of the present disclosure (after light irradiation treatment and 1 to 4 power-on treatments) is shown.

[0037] Fig.15 The voltage-brightness curve of the QLED device according to an embodiment of the present disclosure (after light treatment and 1 to 4 power-on treatments) is shown.

[0038] Fig.16 The voltage-external quantum efficiency curve of the QLED device according to an embodiment of the present disclosure (after light treatment and 1 to 4 power-on treatments) is shown.

[0039] Fig.17 The voltage-current density-brightness curve of the QLED device according to another embodiment of the present disclosure (before power-on treatment) is shown.

[0040] Fig.18 The current density-external quantum efficiency curve of the QLED device according to another embodiment of the present disclosure (before power-on treatment) is shown.

[0041] Fig.19 The voltage-current density-brightness curve of the QLED device according to another embodiment of the present disclosure (after power-on treatment) is shown.

[0042] Fig. 20 The current density-external quantum efficiency curve of the QLED device according to another embodiment of the present disclosure (after power-on treatment) is shown.

[0043] Fig.21 Graphs showing time-voltage and time-relative brightness of a QLED device according to an embodiment of the present disclosure (before and after treatment) at a specific current density.

[0044] Fig. 22 The voltage-current density-brightness curve of the QLED device of another comparative example (before power-on treatment) of the present disclosure is shown.

[0045] Fig.23 The current density-external quantum efficiency curve of the QLED device of another comparative example (before power-on treatment) of the present disclosure is shown. Fig.24 The voltage-current density-brightness curve of a QLED device of a comparative example (after power-on treatment) of the present disclosure is shown. Fig.25 The current density-external quantum efficiency curve of a QLED device of a comparative example (after power-on treatment) of the present disclosure is shown.

[0046] Fig.26 The graph shows the change curves of external quantum efficiency and brightness at different water flow times for a QLED device of a comparative example (water vapor treatment only) of the present invention.

[0047] Fig. 27 The graph shows the change curves of external quantum efficiency and brightness at different water humidity levels for a QLED device of a comparative example (water vapor treatment only) of the present invention. DETAILED DESCRIPTION

[0048] Various exemplary embodiments of the present disclosure will be described in detail below with reference to the accompanying drawings. It should be noted that unless otherwise specifically stated, the relative arrangement of components and steps, numerical expressions and numerical values ​​set forth in these embodiments do not limit the scope of the present disclosure.

[0049] The following description of at least one exemplary embodiment is in fact merely illustrative and is in no way intended to limit the present disclosure and its application or use. That is, the structures and methods herein are shown in an exemplary manner to illustrate different embodiments of the structures and methods in the present disclosure. However, those skilled in the art will appreciate that they merely illustrate exemplary ways of the present disclosure that can be implemented, rather than exhaustive ways. In addition, the drawings need not be drawn to scale, and some features may be enlarged to illustrate the details of specific components.

[0050] In addition, technologies, methods, and apparatus known to ordinary technicians in the relevant field may not be discussed in detail, but where appropriate, such technologies, methods, and apparatus should be considered part of the authorization specification.

[0051] In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.

[0052] The words "left", "right", "front", "back", "top", "bottom", "up", "down", "high", "low", etc., in the specification and claims, if present, are used for descriptive purposes and are not necessarily used to describe an unchanging relative position. It should be understood that the words so used are interchangeable under appropriate circumstances, so that the embodiments of the present disclosure described herein, for example, can operate in other orientations than those shown or otherwise described herein. For example, when the device in the drawings is turned over, features previously described as being "above" other features may now be described as being "below" the other features. The device may also be oriented in other ways (rotated 90 degrees or in other orientations), and the relative spatial relationships will be interpreted accordingly.

[0053] In the specification and claims, when an element is referred to as being "on", "attached", "connected", "coupled" or "coupled" to another element, the element may be directly on, directly attached, directly connected, directly coupled or directly coupled to another element, or one or more intermediate elements may be present. In contrast, when an element is referred to as being "directly" "on", "directly attached", "directly connected", "directly coupled" or "directly coupled" to another element, there will be no intermediate elements. In the specification and claims, a feature being arranged "adjacent" to another feature may refer to a feature having a portion that overlaps with an adjacent feature or a portion that is located above or below the adjacent feature.

[0054] As used herein, the word "exemplary" means "serving as an example, instance, or illustration" rather than as a "model" to be exactly copied. Any implementation described as exemplary herein is not necessarily to be construed as preferred or advantageous over other implementations. Furthermore, the present disclosure is not to be limited by any expressed or implied theory given in the technical field, background, summary, or detailed description.

[0055] As used herein, the term "substantially" is intended to include any minor variations due to design or manufacturing imperfections, device or component tolerances, environmental influences, and / or other factors. The term "substantially" also allows for deviations from a perfect or ideal condition due to parasitic effects, noise, and other practical considerations that may exist in actual implementations.

[0056] In addition, the terms "first", "second" and the like may also be used herein for reference purposes only, and thus are not intended to be limiting. For example, the terms "first", "second" and other such numerical terms referring to structures or elements do not imply a sequence or order unless the context clearly indicates otherwise.

[0057] It should also be understood that when the term “include / comprises” is used in this document, it indicates the presence of the specified features, integers, steps, operations, units and / or components, but does not exclude the presence or addition of one or more other features, integers, steps, operations, units and / or components and / or their combinations.

[0058] In the present disclosure, the term "providing" is used in a broad sense to cover all ways of obtaining an object, so "providing an object" includes but is not limited to "purchasing", "preparing / manufacturing", "arranging / setting", "installing / assembling", and / or "ordering" an object, etc. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. The terms used herein are for the purpose of describing specific embodiments only and are not intended to limit the present disclosure. As used herein, the singular forms "a", "an", and "the" are also intended to include the plural forms unless the context clearly indicates otherwise.

[0059] In the present disclosure, the electron injection layer and the electron transport layer are not distinguished and can be interchanged. The hole injection layer and the hole transport layer are not distinguished and can be interchanged.

[0060] The applicant has found that the preparation of n-type oxide semiconductor nanocrystalline materials and the subsequent device preparation process are not completed in a strict environment that does not produce defect states. The common solution preparation environment and atmospheric purification and manufacturing environment make the generation of defect states inevitable. There are many sources of defects, including surface dangling bonds that come with the material during synthesis, water and oxygen adsorption in the atmospheric environment (electronic defects), and subsequent process steps such as spin coating, thermal evaporation, etc. The damage to the underlying film. It should be pointed out that the electronic defects referred to in this disclosure do not include electronic doping of n-type semiconductors. The latter is the majority carrier of n-type semiconductors, while electronic defects are capture traps for free electrons in the conduction band. For n-type semiconductor materials, the presence of these defect states will capture free electrons in the conduction band, thereby significantly reducing the electron concentration and mobility of the electron transport material, and will also cause invalid recombination currents through defect recombination channels, reducing device efficiency. On the other hand, if the defect concentration of the electron transport layer is too high, it will affect the construction of the ohmic contact between the electrode and the electrode, and affect electron injection. Because of different working conditions, the performance deterioration of optoelectronic devices caused by defects in the electron transport layer is different in electro-optical and photoelectric conversion devices. Taking light-emitting diodes as a typical electro-optical conversion device as an example, defects in the electron transport layer will significantly reduce the effective current density, luminous brightness and luminous efficiency of the device under low-voltage drive; taking solar cells as a typical photo-electrical conversion device as an example, defects in the electron transport layer will significantly reduce the open circuit voltage and energy conversion efficiency of the device.

[0061] The applicant speculates that the acceptor defects (such as adsorbed O2, etc.) and donor defects (such as M n+ , M represents the metal element constituting the oxide semiconductor) is the main factor causing the poor conductivity and reduced device efficiency. At the same time, the subsequent processes of the electron transport layer (such as solution spin coating, thermal evaporation, etc.) are likely to be involved in the generation of these defect states.

[0062] Based on the above research findings, according to the first aspect of the present disclosure, a method for preparing a photoelectric device is provided, the preparation method comprising: preparing an electron transport layer on a substrate having a first electrode, wherein the material of the electron transport layer is n-type oxide semiconductor nanocrystals; preparing a second electrode on the electron transport layer to obtain a photoelectric device to be processed; placing the photoelectric device to be processed in an oxygen-free water vapor environment for a certain period of time, and then performing an electrical treatment and / or light treatment on the photoelectric device to be processed to obtain a photoelectric device; wherein the relative humidity of the environment is 5-85%, oxygen-free means that the oxygen content is less than or equal to 100 ppm, and the material of the second electrode is metal.

[0063] The idea of ​​passivating the defects of the electron transport material in the above preparation method is: after the subsequent process of the electron transport layer is completed (after the second electrode is prepared), the device is treated with a humid atmosphere as a whole to allow water molecules to be adsorbed inside the second electrode with a nanostructure. After the water vapor treatment is completed, the device is energized or illuminated to allow the water molecules to undergo an electrochemical reduction reaction or a photochemical reduction reaction in the metal of the second electrode with a nanostructure to generate active hydrogen radicals. Treatment after the subsequent process is completed can prevent the electron transport layer from being damaged again; the active hydrogen radicals after the electrochemical reduction reaction or the photochemical reduction reaction of water in the metal electrode can produce the following effects with the electron capture sites in the electron transport layer: (1) competitive adsorption without introducing new electron adsorption sites; (2) combining with oxidizing species (for example, reacting O2- to OH-); (3) releasing carriers to the conduction band to improve the conductivity of the film; (4) reducing the defect density and constructing an ideal ohmic contact. By reducing the defects of the electron transport material, the performance and life of the optoelectronic device can be improved.

[0064] In some embodiments, the electron transport layer of the above-mentioned optoelectronic device has no electron defect state or low electron defect state. When the device structure of the above-mentioned optoelectronic device has good matching (such as work function matching of materials), the electron transport layer has no electron defect state or low electron defect state has the following definition:

[0065] For optoelectronic devices based on the principle of light-to-electricity devices, defects in the electron transport layer lead to reduced internal quantum yield and open circuit voltage. The present disclosure defines a state without electron defects as follows: the internal quantum efficiency of the device exceeds 95%, and the difference between the device open circuit voltage and the photon equivalent voltage of the light-absorbing material is less than or equal to 0.3V.

[0066] For optoelectronic devices based on the working principle of light-to-electricity devices, the present disclosure defines a low electron defect state: the quantum efficiency in the device exceeds 80%, and the difference between the device open-circuit voltage and the photon equivalent voltage of the light-absorbing material is less than or equal to 0.6V.

[0067] For optoelectronic devices based on the principle of electro-optical devices, defects in the electron transport layer lead to reduced internal quantum efficiency, low-voltage efficiency, and low-voltage current density. The present disclosure defines a state without electron defects as follows: the internal quantum efficiency of the device exceeds 95%, the device reaches the peak internal quantum efficiency when the photon equivalent voltage is less than the photon equivalent voltage of the luminescent material, and the current density of the device exceeds 5mA / cm when driven by the photon equivalent voltage 2 When driven by 1.5 times the photon equivalent voltage, the current density exceeds 370mA / cm 2 .

[0068] For optoelectronic devices based on the working principle of electro-optical devices, the present disclosure defines low electron defect states as follows: the internal quantum efficiency of the device exceeds 80%, the device reaches the peak internal quantum efficiency when the photon equivalent voltage of the device is no more than 1.1 times that of the light-emitting material, and the current density of the device exceeds 1 mA / cm when driven by the photon equivalent voltage. 2 When driven by 1.5 times the photon equivalent voltage, the current density exceeds 250mA / cm 2 .

[0069] The present disclosure proposes a method of suppressing and eliminating the electron defect state of the electron transport layer, and obtains an n-type oxide nanocrystalline film with low or no electron defect state. The electron transport layer has near-perfect electron transport and electron injection / extraction characteristics, which solves the problem of low brightness and poor efficiency of electro-optical devices under low-voltage driving (within 2 times the photon equivalent voltage). When the internal structure and overall material of the device are relatively matched, its peak efficiency reaches the theoretical prediction limit, and the brightness is improved by 1-2 orders of magnitude compared with the existing technical solutions.

[0070] In some embodiments, the water vapor treatment environment may include one or more of other inert gases and N2 in addition to water vapor. In some embodiments, the formation of the water vapor treatment environment includes deoxygenating air and then adjusting the water vapor concentration, or mixing the inert gas (N2) and water vapor.

[0071] In some embodiments, the environment of the above-mentioned power treatment or light treatment is an indoor environment, without special water vapor or temperature or other atmosphere requirements, which reduces the requirements for industrial preparation.

[0072] In some embodiments, the power-on treatment and the light-irradiation treatment are performed simultaneously, but the treatment times can be the same or different, that is, the treatment times can overlap, thereby accelerating the speed of passivating defects in the electron transport material and improving the preparation efficiency.

[0073] In some embodiments, different water vapor concentrations will affect the speed at which water vapor enters the electron transport layer, thereby affecting the preparation time required, but excessive water vapor will also affect the conductivity of the device. Preferably, the relative humidity is 40-55% or 40-60% or 40-65% or 40-70% or 45-65% or 45-65% or 45-70%.

[0074] In some embodiments, the material of the second electrode includes one or more of Ag, Au, Al, Mg, Zn, Ti, Ca, Cr, Cu, and Zr. These metals can react with water to generate hydrogen radicals, and in particular, the electrical treatment can promote the reaction of inert metals such as Ag and Au with water to generate hydrogen radicals.

[0075] In some embodiments, the n-type oxide semiconductor nanocrystals are metal oxide nanocrystals, and the metal oxide nanocrystals are selected from zinc oxide, zinc oxide doped with metal elements, titanium oxide or tin oxide. In some embodiments, the zinc oxide doped with metal elements is ZnMgO or ZnMgAlO, and the doping ratio is not limited. In some embodiments, the average diameter of the metal oxide nanocrystals is 1-20nm, and the average diameter is obtained by transmission electron microscopy.

[0076] In some embodiments, the substrate having a first electrode includes a substrate, a first electrode, a hole injection layer, a hole transport layer, and a quantum dot light emitting layer.

[0077] In some embodiments, the second electrode may be directly adjacent to the electron transport layer or not. In some embodiments, the second electrode may be prepared by stacking one or more layers. The preparation method of the second electrode includes but is not limited to evaporation and sputtering.

[0078] In some embodiments, the optoelectronic device comprises at least one quantum dot light emitting diode, and the quantum dot light emitting diode is a bottom-emitting type, a top-emitting type, or a double-sided light emitting type. In some embodiments, the quantum dot light emitting diode is a positive type or a negative type. The optoelectronic device is used in a display device.

[0079] In some embodiments, the quantum dot light-emitting layer is one or more layers. In some embodiments, the quantum dot light-emitting diode further comprises other functional layers, such as a hole blocking layer, an electron blocking layer, a buffer layer, an interface modification layer and / or any layer that realizes other desired functions, etc. The preparation method of the light-emitting layer or the functional layer can refer to the prior art, such as inkjet printing, spin coating, spray coating, full-surface coating, etc.

[0080] In some embodiments, the optoelectronic device is a quantum dot light emitting diode, which includes a substrate, a first electrode, a hole transport layer, a quantum dot light emitting layer, an electron transport layer and a second electrode arranged in sequence.

[0081] In some embodiments, the quantum dot light-emitting diode further includes functional layers with the same function made of multiple different materials, such as two electron transport layers.

[0082] In some embodiments, the preparation method further includes providing a light extraction structure on at least one quantum dot light emitting diode to improve light extraction efficiency.

[0083] In some embodiments, the optoelectronic device comprises a hole transport layer, and the number of hole defect states of the hole transport layer material is low or zero.

[0084] In some embodiments, when the material of the second electrode is Ag, the external quantum efficiency of the quantum dot light emitting diode is greater than or equal to 20%. In some embodiments, when the material of the second electrode is Ag, the external quantum efficiency of the quantum dot light emitting diode is less than or equal to 25%. In some embodiments, when the material of the second electrode is Ag, the external quantum efficiency of the quantum dot light emitting diode is less than or equal to 30%.

[0085] It should be noted that the above external quantum efficiency (EQE) is obtained based on the test without light extraction structure, and there is no light extraction structure inside or outside the optoelectronic device. If there is a light extraction structure, the external quantum efficiency can be higher for the electro-optical device.

[0086] In some embodiments, the above-mentioned certain time is greater than or equal to 1 minute and less than or equal to 3 days. In some embodiments, the above-mentioned certain time is less than or equal to 60 minutes or less than or equal to 50 minutes or less than or equal to 40 minutes, and greater than or equal to 5 minutes. The shorter the time, the higher the production efficiency of the preparation method. The above-mentioned time can be judged according to the effect of removing defect states and the production efficiency. It is worth mentioning that when the thickness of the metal electrode increases, the processing intensity needs to be increased (increase time or humidity), and when the thickness of the metal electrode decreases, the processing intensity needs to be reduced (reduce time or humidity). The optimal device performance that can be achieved by various parameter combinations is relatively close. When the humidity of the environment is low, the time for water vapor treatment needs to be extended.

[0087] In some embodiments, the optoelectronic device includes a light-emitting layer or a light-absorbing layer, the light-emitting layer includes a light-emitting material, or the light-absorbing layer includes a light-absorbing material.

[0088] In some embodiments, the electron transport layer has a film thickness of 30-100 nm.

[0089] In some embodiments, the thickness of the second electrode is 30-200 nm or 30-150 nm. The thickness of the electrode may affect the efficiency of the above-mentioned post-treatment method, such as the penetration rate of water vapor. The appropriate thickness can be selected according to the requirements of production efficiency and the performance requirements of the optoelectronic device itself.

[0090] In some embodiments, the oxygen content of the environment is less than or equal to 10 ppm.

[0091] In some preferred embodiments, the oxygen content of the environment is less than or equal to 5 ppm, or less than or equal to 3 ppm.

[0092] In some embodiments, the ambient temperature of the water vapor treatment and the post-power-on treatment is room temperature. Different ambient temperatures also affect the speed of water vapor entry. From the perspective of energy saving, it is sufficient to treat at room temperature. Of course, in order to standardize the preparation process, the temperature can be controlled between 10-35 degrees Celsius.

[0093] In some embodiments, the power-on treatment time is 1-600 seconds. In some embodiments, the power-on treatment time is 60-120 seconds. The shorter the time, the higher the preparation efficiency.

[0094] In some embodiments, the voltage of the power-on treatment is 0-20 V (excluding 0 V). In some embodiments, the voltage of the power-on treatment is 1.9-4 V. Within the aforementioned range, a faster electrochemical reduction speed can be achieved while reducing the risk of device burnout.

[0095] In some embodiments, the number of times of power-on treatment is multiple, and the interval time of multiple power-on treatments is 0-10 minutes (excluding 0s). It should be noted that power-on treatment without interval is also possible, and interval or not basically does not affect the final performance of the device.

[0096] In some embodiments, the light treatment time is 0-3 hours (excluding 0s). The treatment time mainly refers to the speed of the photochemical reduction reaction. If the speed is fast, the time can be shortened, and if the speed is slow, the time must be extended.

[0097] In order to achieve photochemical reduction reaction, the peak wavelength of the light source of the light treatment is shorter than the band gap wavelength of the quantum dot light emitting layer (quantum dot material) (the absorption edge in the absorption spectrum is defined as the band gap wavelength). In other embodiments, the peak wavelength of the light source of the light treatment is shorter than the band gap wavelength of the n-type oxide semiconductor nanocrystal (the absorption edge in the absorption spectrum is defined as the band gap wavelength). In some embodiments, the wavelength of the light treatment is 300-700nm, preferably the wavelength of the light treatment is 300-400nm, or more preferably 300-370nm. In some embodiments, the power density is 1-1000mW / cm 2 , the preferred power density is 35-105mW / cm 2 .

[0098] In some embodiments, before the power-on treatment or the light-irradiation treatment, the photoelectric device after the water vapor treatment is packaged. The packaging method can refer to the existing technology, such as packaging glue packaging or thin film packaging or glass packaging.

[0099] The optoelectronic device is any device containing an electron transport layer. In some embodiments, the optoelectronic device is a quantum dot light emitting diode, a solar cell, a photodetector, or a laser. In some embodiments, the optoelectronic device is a device comprising a quantum dot light emitting diode, a solar cell, a photodetector, or a laser.

[0100] In some embodiments, the above-mentioned optoelectronic device is not treated with acidic gas. In some embodiments, the electron transport layer of the above-mentioned optoelectronic device is not treated with acidic gas or acidic substance. In some embodiments, the above-mentioned optoelectronic device is not packaged with acidic encapsulation glue. When using acidic encapsulation glue for packaging treatment, it is necessary to react the acidic substance with the electron transport layer material. This type of treatment method is usually accompanied by uncontrollable aging time (ranging from a few hours to a few days, and it cannot be a mass production process), and a substantial change in the brightness uniformity of the device's light-emitting area. After the positive aging process, it is accompanied by a negative effect. Although the device efficiency is acceptable, the device brightness and life are far lower than the results of the technical solution disclosed in the present invention, and the aging process is often accompanied by a rapid increase in the driving voltage.

[0101] In some embodiments, the external quantum efficiency of the prepared optoelectronic device is greater than or equal to 20%. In some embodiments, the external quantum efficiency of the prepared optoelectronic device is less than or equal to 30%.

[0102] Hereinafter, the embodiments are described in more detail with reference to specific examples. However, they are illustrative examples of the present disclosure, and the present disclosure is not limited thereto.

[0103] Example 1

[0104] ZnMgO synthesis:

[0105] The molar ratio of the metal salt precursor of ZnMgO is Zn:Mg=0.85:0.15. Weigh 0.5598g (2.55mmol) zinc acetate dihydrate and 0.0965g (0.45mmol) magnesium acetate tetrahydrate in a three-necked flask, add 30mL dimethyl sulfoxide, and place the three-necked flask in a 50°C water bath and stir until the solid powder is completely dissolved. Weigh 0.8155g (4.5mmol) tetramethylammonium hydroxide pentahydrate, dilute to 10mL with ethanol, and add dropwise to the three-necked flask after the powder is completely dissolved for about 10min. After the addition is complete, stir in a 50°C water bath for 1h. Transfer the reaction stock solution to a centrifuge tube, add 10mL of stock solution to each tube, and then add 20-25mL of ethyl acetate until obvious turbidity occurs. Set the centrifuge speed to 3000r.pm, the time to 3min, and centrifuge to precipitate. Pour off the supernatant, retain the white precipitate, and add 1 mL of anhydrous ethanol to each centrifuge tube to dissolve the precipitate. Add about 5 mL of ethyl acetate to each tube until it becomes obviously turbid. Set the centrifuge speed to 5000 rpm and the time to 3 minutes to centrifuge the precipitate. Pour off the supernatant, add 500 μL of anhydrous ethanol to each centrifuge tube to dissolve the white precipitate, and filter the solution using a 0.22 μm oil phase nylon filter. Use a UV-visible spectrometer to determine the OD value of the solution at 280 nm and dilute to OD = 200.

[0106] QLED device preparation process:

[0107] 1. Cleaning ITO glass substrate: Wipe the ITO surface with a dust-free cloth and ethanol until there is no obvious dust on the surface, then ultrasonically clean it with acetone, deionized water and anhydrous ethanol for 15 minutes each. Blow dry with a nitrogen gun. Treat the ITO surface with plasma for 15 minutes.

[0108] 2. Spin coating of PEDOT:PSS: The PEDOT:PSS solution was filtered through a PVDF microfilter and spin coated at 3000 rpm for 45 s, followed by annealing at 150 °C for 30 min in an air environment.

[0109] 3. Spin coating of hole transport layer: Transfer the device to a glove box and spin coat 8 mg / mL PF8Cz solution at 2000 rpm for 40 seconds. Anneal at 150°C for 30 minutes in the glove box.

[0110] 4. Spin coating quantum dot layer: Spin coating green CdSe / CdZnSe / CdZnS quantum dots (peak wavelength 532nm, corresponding photon equivalent driving voltage of about 2.33V) at a rotation speed of 2500 rpm for 40s.

[0111] 5. Spin coating of electron transport layer: Spin coating of ZnMgO solution at a speed of 2000 rpm for 40 s.

[0112] 6. Place the spin-coated device in the evaporation chamber, evacuate the vacuum, and start evaporating the electrode Ag. Control the evaporation rate and Before, the evaporation rate was achieve After that, the evaporation rate is The final thickness of the Ag electrode is about 70nm.

[0113] 7. Take out the QLED device from the evaporation chamber.

[0114] 8. QLED device water vapor post-treatment: Take a certain amount of deionized water and put it in a container. Pass dry inert gas (argon) into the water. The discharged water-inert gas mixture is fully mixed with another dry inert gas in proportion and passed into the container containing the QLED device. The ambient temperature is 22-25 degrees Celsius, the water vapor concentration in the environment is 45% RH, and the oxygen concentration is less than 3ppm. After 40 minutes of treatment, take it out and use non-acidic UV curing glue to encapsulate it.

[0115] 9. Power on the packaged device to obtain the final QLED device.

[0116] After testing, the brightness of the QLED device at 3V driving voltage was <20000nit during the initial test (before power-on treatment), and the peak external quantum yield was about 17.7%. Figure 2 and Figure 3 After power-on treatment (one scan represents a gradual increase in voltage from 0V to 4V, with a step of 0.1V, and a total duration of about 30 seconds; the same below), the brightness at a driving voltage of 3V is about 131000nit, and the peak external quantum yield is about 20.9%, as shown in FIG. Figure 4 and Figure 5 shown.

[0117] In order to study the effect of power-on time on device performance, the device was powered on (scanned) multiple times. The performance of the QLED device changes with power-on. Figure 6-8 shown.

[0118] In order to study the effect of post-treatment on device life, the 2 A graph showing the relative brightness and voltage of a device without water vapor treatment but with power on, and a device with water vapor treatment and power on, with the same power on time. Fig. 9 It can be seen that as time goes by, the relative brightness of the two compared devices has decreased to a similar degree, but the voltage of the device that has undergone water vapor treatment and power-on treatment is relatively stable. In addition, the other lifespan conditions of the two are shown in Table 1 below:

[0119] Device status Initial brightness (nit) T95(hours) T80(hours) Devices without water vapor treatment but with power treatment 16855 0.4 11.7 Devices for water vapor treatment and electrical treatment 26862 1.7 19.6

[0120] Comparative Example 1

[0121] The preparation of the QLED device is the same as in Example 1, except that there is no QLED water vapor post-treatment, and the QLED device is obtained after packaging and powering on.

[0122] After testing, the brightness of the QLED device at 3V driving voltage was <300nit during the initial test (before power-on treatment), and the peak external quantum yield was about 13.9%. Fig.10 and Fig.11 After the power-on treatment, the brightness of the QLED device at 3V driving voltage is about 800nit, and the peak external quantum efficiency is about 12.3%. Fig.12 and Fig.13 As shown in Figure 2, the performance of the device without water vapor treatment before and after power treatment is as follows: Figure 10-13 As shown in the figure, the brightness of the QLED device does not exceed 800nit at a driving voltage of 3V, the peak external quantum yield does not exceed 13.9%, and there is almost no change before and after power-on, proving the applicant's theoretical speculation. Regardless of whether the power-on treatment is performed, the performance is far inferior to the device treated with water vapor.

[0123] Example 2

[0124] The QLED device was prepared in the same manner as in Example 1, except that light treatment was used instead of power treatment. The light treatment conditions were: the peak wavelength of the light source was 365 nm, and the power density was 85 mW / cm 2 , the illumination time is 5 minutes.

[0125] After testing, the brightness of the QLED device at 3V driving voltage was 115400nit in the initial test (after light treatment), and the peak external quantum yield was about 19.7%, which was equivalent to the performance of the QLED device after multiple power-on treatments in Example 1. The device after light treatment was powered on multiple times, and the performance of the QLED device changed with power-on as shown in the following figure. Figure 14-16 As shown in the figure, it can be seen that the performance of the device after light treatment has been improved before power is turned on, and there is almost no change before and after power is turned on. This proves that light treatment can have the same effect as power treatment.

[0126] Example 3

[0127] The preparation method of the device is basically the same as that of Example 1, except that the material of the vapor-deposited electrode is Au, and the QLED device is obtained by water vapor treatment-packaging-power-on treatment.

[0128] like Fig.17 and Fig.18 As shown in the figure, during the initial test (before power-on treatment), the brightness of the QLED device at a driving voltage of 3V was <100nit, and the peak external quantum yield was about 12.7%. After power-on treatment (4 scans), as shown in the figure, Fig.19 and Fig. 20 As shown in the figure, the brightness at 3V driving voltage is about 11000nit, and the peak external quantum yield is about 22.7%. It can be seen that the brightness and peak external quantum efficiency of the QLED device at 3V driving voltage are significantly improved before and after power is turned on.

[0129] In order to study the effect of post-treatment on device life, the 2 A graph showing the relative brightness and voltage changes over time for a device without moisture treatment but with power on, and a device with moisture treatment and power on, at a current density with the same power on time. Fig.21 It can be seen that as time goes by, the relative brightness of the two compared devices has decreased to a similar degree, but the voltage of the device that has undergone water vapor treatment and power-on treatment is relatively stable and has a higher relative brightness. In addition, the other lifespan conditions of the two are shown in Table 2 below:

[0130] Device status Initial brightness (nit) T95(hours) T80(hours) Devices without water vapor treatment but with power treatment 11707 6.3 21.6 Devices for water vapor treatment and electrical treatment 15302 11.3 39.4

[0131] Comparative Example 2

[0132] The preparation of the QLED device is the same as in Example 3, except that there is no QLED water vapor post-treatment to obtain the QLED device.

[0133] After testing, the brightness of the QLED device at 3V driving voltage was <100nit during the initial test (before power-on treatment), and the peak external quantum yield was about 11.3%. Fig. 22 and Fig.23 After the power-on treatment, the brightness of the QLED device at 3V driving voltage is about 400nit, and the peak external quantum efficiency is about 10.9%. Fig.24 and Fig.25 It can be seen that the performance of the device without water vapor treatment is almost unchanged before and after the power treatment, and regardless of whether the power treatment is performed, the performance is far inferior to the device with water vapor treatment.

[0134] Other comparative examples (water vapor treatment only)

[0135] The preparation method of the device is basically the same as that of Example 1. The preparation process of the QLED device is as follows:

[0136] 1. Clean the ITO glass substrate: Wipe the ITO surface with a dust-free cloth and ethanol until there is no obvious dust on the surface, then ultrasonically clean it with acetone, deionized water and anhydrous ethanol for 15 minutes each. Blow dry with a nitrogen gun. Treat the ITO surface with plasma for 15 minutes.

[0137] 2. Spin coating of PEDOT:PSS: The PEDOT:PSS solution was filtered through a PVDF microfilter and spin coated at 3000 rpm for 45 s, followed by annealing at 150 °C for 30 min in an air environment.

[0138] 3. Spin coating the hole transport layer: Transfer the device to the glove box and spin coat 8 mg / mL PF8Cz solution at 2000 rpm for 40 seconds. Anneal at 150°C for 30 minutes in the glove box.

[0139] 4. Spin coating quantum dot layer: Spin coating green CdSe / CdZnSe / CdZnS quantum dots (peak wavelength 530nm, corresponding photon equivalent driving voltage of about 2.33V) at a rotation speed of 2500 rpm for 40s.

[0140] 5. Spin coating the electron transport layer: Spin coating the ZnMgO solution at a speed of 2000 rpm for 40 seconds. 6. Place the spin-coated device in the evaporation chamber, evacuate the chamber, and start evaporating the electrode A1. Control the evaporation rate and when the electrode thickness reaches Before, the evaporation rate was achieve After that, the evaporation rate is The final thickness of the Al electrode is about 70nm.

[0141] 7. Remove the device from the evaporation chamber.

[0142] 8. QLED water vapor (Al electrode) post-treatment: Take a certain amount of deionized water and put it in a container, pass dry inert gas (argon) into the water, and mix the discharged water-inert gas mixture with another dry inert gas in proportion, and pass it into the container containing the device. The ambient temperature is 22-25 degrees Celsius, the water vapor concentration in the environment is as described below, the oxygen concentration is less than 3ppm, the treatment time is as described below, take it out, and use non-acidic UV curing glue to encapsulate.

[0143] The difference between the different comparison examples lies in the specific conditions of water vapor treatment. The first comparison group: different water flow times (0min, 1min, 3min, 5min, 10min, 20min, 40min), humidity is 45RH%; the second comparison group: different water flow humidity (water vapor concentration 0.8RH%, 10RH%, 45RH%, 60RH%, 75RH%, 90RH%), the lower the water vapor concentration of the device, the longer the treatment time, the treatment time is 16 hours when the water vapor concentration is 0.8RH%. The external quantum efficiency and brightness results of the device are shown in Figure 2. Figure 26-27 As shown. The environment where active metal Al and water vapor coexist allows active metal Al and water to react chemically to generate hydrogen reducing substances. Water vapor reaches the electron transport layer through the electrode pores, and the active hydrogen reducing substances generated by the reaction react with the electron defect substances (such as O2) adsorbed on the surface of the electron transport layer material to generate -OH. Compared with the electrode material used in the embodiment, it is easier to react with water vapor, so the device performance is also excellent when no illumination or power treatment is required. Characterization method of QLED prototype devices for all embodiments and comparative examples: a self-built photoelectric test system is used to obtain the current-voltage-brightness-external quantum efficiency information of the QLED prototype device. The ISP-50 integrating sphere is matched with the QEpro spectrometer through optical fiber to obtain the luminescence information of the QLED device; the Keithley 2450 high-precision digital source meter can be used for the application and measurement of voltage and current. Python code controls the above instruments to work together. The absolute spectral radiation flux is calibrated by using a standard lamp (HL-3plus, Ocean Optics).

[0144] Although some specific embodiments of the present disclosure have been described in detail by way of example, it should be understood by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present disclosure. The various embodiments disclosed herein may be combined in any manner without departing from the spirit and scope of the present disclosure. It should also be understood by those skilled in the art that various modifications may be made to the embodiments without departing from the scope and spirit of the present disclosure. The scope of the present disclosure is defined by the appended claims.

Claims

1. A method for preparing a photoelectric device, characterized in that: The preparation method comprises: preparing an electron transport layer on a substrate having a first electrode, wherein the material of the electron transport layer is n-type oxide semiconductor nanocrystal; preparing a second electrode on the electron transport layer to obtain a photoelectric device to be processed; placing the photoelectric device to be processed in an oxygen-free water vapor environment for a certain period of time, and then performing an electrical treatment and / or light treatment on the photoelectric device to be processed to obtain the photoelectric device; wherein the relative humidity of the environment is 5-85%, oxygen-free means that the oxygen content is less than or equal to 100 ppm, and the material of the second electrode is metal.

2. The preparation method according to claim 1, characterized in that: The material of the second electrode includes one or more of Ag, Au, Al, Mg, Zn, Ti, Ca, Cr, Cu, and Zr.

3. The preparation method according to claim 1 or 2, characterized in that: The n-type oxide semiconductor nanocrystals are metal oxide nanocrystals, and the metal oxide nanocrystals are selected from zinc oxide, zinc oxide doped with metal elements, titanium oxide or tin oxide. Preferably, the average diameter of the metal oxide nanocrystals is 1-20 nm.

4. The preparation method according to claim 1 or 2, characterized in that: The substrate with a first electrode includes a substrate, a first electrode, a hole injection layer, a hole transport layer and a quantum dot light-emitting layer.

5. The preparation method according to claim 1 or 2, characterized in that: The certain period of time is greater than or equal to 1 minute and less than or equal to 3 days; preferably, the certain period of time is less than or equal to 60 minutes.

6. The preparation method according to claim 1 or 2, characterized in that: The film thickness of the electron transport layer is 30-100 nm.

7. The preparation method according to claim 1 or 2, characterized in that: The thickness of the second electrode is 30-200 nm.

8. The preparation method according to claim 1 or 2, characterized in that: The ambient temperature for water vapor post-treatment, power-on post-treatment and light post-treatment is room temperature.

9. The preparation method according to claim 1 or 2, characterized in that: The duration of the power-on treatment is 1-600s.

10. The preparation method according to claim 1 or 2, characterized in that: The voltage of the power-on process is greater than 0 and less than or equal to 20V.

11. The preparation method according to claim 1 or 2, characterized in that: The number of times of the power-on treatment is multiple times, and the interval time of the multiple power-on treatments is greater than 0 and less than or equal to 10 minutes.

12. The preparation method according to claim 1 or 2, characterized in that: The peak wavelength of the light source for the light irradiation treatment is shorter than the band gap wavelength of the n-type oxide semiconductor nanocrystal.

13. The preparation method according to claim 4, characterized in that: The peak wavelength of the light source for the light treatment is shorter than the band gap wavelength of the quantum dot light emitting layer.

14. The preparation method according to claim 1 or 2, characterized in that: Before the power-on treatment or the light-irradiation treatment, the photoelectric device after the water vapor treatment is packaged.

15. The preparation method according to claim 1 or 2, characterized in that: The optoelectronic device is a quantum dot light emitting diode, a solar cell, a photodetector or a laser.