Fullerene-based anti-free radical membrane electrode and preparation method and application thereof

By adding a fullerene anti-radical quencher to the catalytic layer of the fuel cell membrane electrode, combined with a Pt/C catalyst and Nafion resin, and optimizing the addition amount, the performance degradation problem caused by free radical attack in the fuel cell was solved and significantly improved. improve battery stability and performance.

CN118748262APending Publication Date: 2024-10-08TONGJI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410766377.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The proton conductivity of the catalytic layer decreases due to free radical attacks during operation of existing fuel cell membrane electrodes, affecting battery performance and durability. In addition, the introduction of metal oxide quenchers will cause the loss of mass transfer channels, resulting in a decline in battery performance.

Method used

Add 0.1%-10% fullerene to the catalytic layer as an anti-free radical quenching agent, combine Pt/C catalyst and Nafion perfluorosulfonic acid resin, prepare membrane electrodes by transfer printing or spraying, and optimize the performance of anode and cathode. Add amount.

Benefits of technology

It effectively improves the chemical stability and current density peak decay rate of the battery, reduces the membrane electrode decay rate, and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748262A_ABST
    Figure CN118748262A_ABST
Patent Text Reader

Abstract

The invention relates to a fullerene-based anti-free radical membrane electrode and a preparation method and application thereof. The membrane electrode comprises catalyst layers and a proton exchange membrane, and the catalyst layers cover the two sides of the proton exchange membrane; the catalyst layer comprises a catalyst, an ionomer and a fullerene-based anti-radical quencher; the addition mass percentage of the anti-free radical quenching agent based on fullerene is 0.1%-10%; the adding mass percentage of the ionomer is 10-40%. The preparation method comprises the following steps: adding the catalyst and the ionomer into an alcohol / water mixed solvent, then adding the fullerene-based anti-free radical quenching agent, uniformly stirring, and coating the proton exchange membrane with the mixture. Compared with the prior art, the fullerene with the free radical quenching function is added into the catalyst layer, so that the purpose of improving the stability of the battery is achieved, an optimization strategy of different additive amounts of the cathode catalyst layer and the anode catalyst layer is implemented, and good battery performance is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of membrane electrodes, and in particular to a fullerene-based anti-free radical membrane electrode and a preparation method and application thereof. Background Art

[0002] Proton exchange membrane fuel cell (PEMFC) is a power generation device that converts chemical energy into electrical energy using hydrogen as a carrier. It has the advantages of low reaction temperature, fast dynamic response speed, high reaction efficiency, and high power density. It has broad application prospects in the field of transportation. However, the large-scale commercial application of fuel cells is restricted by durability and reliability. The membrane electrode is the core component of the fuel cell, which consists of a proton exchange membrane, a catalyst layer, and a gas diffusion layer. The catalyst layer is the place where the electrochemical reaction occurs, and the ionomer, as a binder, plays an important role in transporting protons. A large number of hydroxyl radicals will be generated during battery operation, attacking the ionomer and causing structural degradation, resulting in a decrease in the proton conductivity of the catalyst layer. Therefore, it is of great research value to modify the catalyst layer to resist free radicals and thus improve the durability of the membrane electrode, which is the key to accelerating the commercialization of PEMFC.

[0003] Chinese patent CN106876754B proposes a catalyst layer structure that can improve the stability of fuel cells, including Ag2O, inorganic metal oxides treated with organic matter, and one or more of heteropoly acids, wherein the heteropoly acid is 12-HSW, 21-HPW, and one or more of cesium phosphotungstate as free radical quenching additives, thereby achieving the purpose of improving the stability of the fuel cell.

[0004] Chinese patent CN 112670520 A proposes a method for implementing different amounts of free radical scavengers in the cathode catalyst layer and the anode catalyst layer. The first free radical scavenger is added to the anode catalyst layer, and the second free radical scavenger is added to the cathode catalyst layer. The added types include one or a combination of metal particles and inorganic metal oxides. The weight ratio of the first free radical scavenger to the entire catalyst layer is 0.2%-5%; the weight ratio of the second free radical scavenger to the entire catalyst layer is 0%-1%.

[0005] However, after the metal oxide free radical quencher is introduced into the catalyst layer, the generated metal ions will be adsorbed on the sulfonate groups at the proton transfer sites in the ionomer, causing the loss of mass transfer channels and resulting in a decrease in battery performance. Therefore, it is urgent to study a method for preparing a battery membrane structure that can improve the stability of battery performance. Summary of the invention

[0006] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a fullerene-based anti-free radical membrane electrode and its preparation method and application. By adding fullerene with free radical quenching function in the catalytic layer, the purpose of improving the stability of the battery is achieved.

[0007] The purpose of the present invention can be achieved by the following technical solutions:

[0008] The present invention provides a free radical resistant membrane electrode based on fullerene, wherein the membrane electrode comprises a catalyst layer and a proton exchange membrane, wherein the catalyst layer covers both sides of the proton exchange membrane;

[0009] The catalyst layer comprises a catalyst, an ionomer, and a fullerene-based anti-radical quencher;

[0010] The added mass percentage of the fullerene-based anti-free radical quencher is 0.1%-10%; preferably, the added mass percentage of the fullerene-based anti-free radical quencher is 2%-5%;

[0011] The added mass percentage of the ionomer is 10-40%; preferably, the added mass percentage of the ionomer is 11-14%.

[0012] Furthermore, the fullerene-based anti-radical quencher is one or more of fullerene and fullerene derivatives.

[0013] Furthermore, the fullerene derivatives include fullerene polyvinyl pyrrolidone and polyhydroxyfullerene.

[0014] Furthermore, the particle size of the fullerene-based anti-radical quencher is 1-30 nm.

[0015] Furthermore, the ionomer includes one or more of Nafion perfluorosulfonic acid resin dispersion and Aquivion perfluorosulfonic acid resin dispersion.

[0016] Furthermore, the catalyst is a Pt / C catalyst, and the mass ratio of Pt in the Pt / C catalyst is 40%-60%; preferably, the mass ratio of Pt in the Pt / C catalyst is 40%.

[0017] The present invention also provides a method for preparing a fullerene-based anti-free radical membrane electrode, comprising the following steps:

[0018] S1: adding the catalyst and the ionomer into an alcohol / water mixed solvent, and then adding a fullerene-based anti-radical quencher, and stirring evenly to obtain a catalyst layer slurry;

[0019] S2: The anode and cathode catalyst layer slurries are coated on the proton exchange membrane by transfer, scraping or spraying, and dried into layers to obtain CCM, and then covered with a gas diffusion layer to obtain a membrane electrode.

[0020] Furthermore, in S2, the gas diffusion layer is carbon paper.

[0021] Further, in S1, the mass ratio of the catalyst, the ionomer and the alcohol / water mixed solvent in the catalyst layer slurry is 1:4:180;

[0022] The mass ratio of ethanol to water in the alcohol / water mixed solvent is 1:1.

[0023] The present invention also provides an application of a fullerene-based anti-free radical membrane electrode, wherein the anti-free radical membrane electrode is used in a battery preparation process.

[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0025] The present invention achieves the purpose of improving battery stability by adding fullerene with free radical quenching function in the catalyst layer, and implements the optimization strategy of different addition amounts of cathode and anode catalyst layers to ensure good battery performance. -2 When the peak current density is reduced by 34.4%, the membrane electrode attenuation rate is effectively alleviated, and the chemical stability is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 The polarization curves of the membrane electrode before attenuation of Example 1, Example 2 and Comparative Example 1 are shown;

[0027] Figure 2 The battery performance diagram before membrane electrode attenuation of Example 1, Example 2 and Comparative Example 1;

[0028] Figure 3 The polarization curves of the membrane electrodes of Example 1, Example 2 and Comparative Example 1 after attenuation;

[0029] Figure 4 The battery performance diagram after membrane electrode attenuation of Example 1, Example 2 and Comparative Example 1;

[0030] Figure 5 The ECSA value diagram of the membrane electrode with different decay times of Example 1, Example 2 and Comparative Example 1;

[0031] Figure 6 This is a comparison diagram of the ohmic resistance values ​​of membrane electrodes at different decay times of Example 1, Example 2 and Comparative Example 1;

[0032] Figure 7 It is a comparison chart of the F ion loss rate of the membrane electrode at different decay times of Example 1, Example 2 and Comparative Example 1. DETAILED DESCRIPTION

[0033] The specific implementation methods of the present invention are described in detail below through examples. These examples are implemented on the premise of the scheme described in the present invention, and provide detailed implementation methods and specific operating processes, but the protection scope of the present invention is not limited to the following examples.

[0034] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. Any features such as component models, material names, connection structures, preparation methods, materials, structures or composition ratios not clearly described in this technical solution are deemed to be common technical features disclosed in the prior art.

[0035] Example 1

[0036] This embodiment provides a fullerene-based anti-radical membrane electrode, which includes a catalyst layer and a proton exchange membrane, wherein the catalyst layer covers both sides of the proton exchange membrane; the catalyst layer contains a catalyst, an ionomer and a fullerene-based anti-radical additive.

[0037] This embodiment also provides a method for preparing a fullerene-based anti-free radical membrane electrode, comprising the following steps:

[0038] S1: Preparation of membrane electrode: Weigh 0.1304g of platinum carbon catalyst with a Pt content of 40wt.% and pour it into a beaker, then add 12.51g of deionized water, stir it evenly, add 0.2445g of Nafion D2020 perfluorosulfonic acid dispersion and 11.9347g of ethanol, and mix the slurry evenly by ultrasound and high-speed shearing. Then add 0.0036g of fullerene free radical quencher accounting for 2wt.% of the mass ratio of the catalytic layer, stir evenly to obtain a slurry. The mass ratio of the catalyst, ionomer and alcohol / water mixed solvent in the catalytic layer slurry is 1:4:180. The mass ratio of ethanol and water in the alcohol / water mixed solvent is 1:1. The mass ratio of the ionomer to the catalytic layer is 12.92%.

[0039] S2: The amount of anode slurry used was controlled to be 10 g, and the amount of cathode slurry used was controlled to be 20 g. The slurry in S1 was sprayed on both sides of the proton exchange membrane, and dried into layers to obtain a CCM (catalyst coated membrane) sample containing 2 wt.% of anti-free radical additive in the catalyst layer. The CCM sample was bonded to the test frame and then covered with gas diffusion layer carbon paper to obtain a membrane electrode, named TS-2%-0.

[0040] The CCM membrane electrodes prepared above were immersed in Fenton's reagent for 4 h, 8 h, and 12 h at 80°C for accelerated chemical decay experiments and were named TS-2%-4, TS-2%-8, and TS-2%-12, respectively.

[0041] Example 2

[0042] S1: Preparation of membrane electrode: Weigh 0.1304g of platinum carbon catalyst with a Pt content of 40wt.% and pour it into a beaker, then add 12.51g of deionized water, stir it evenly, add 0.2445g of Nafion D2020 perfluorosulfonic acid dispersion and 11.9347g of ethanol. Mix the slurry evenly by ultrasound and high-speed shearing, then add 0.009g of fullerene free radical quencher accounting for 5wt.% of the mass ratio of the catalyst layer, and stir evenly to obtain a slurry. The mass ratio of the catalyst, ionomer and alcohol / water mixed solvent in the catalyst layer slurry is 1:4:180. The mass ratio of ethanol and water in the alcohol / water mixed solvent is 1:1. The mass ratio of the ionomer to the catalyst layer is 12.74%.

[0043] S2: The amount of anode slurry used was controlled to be 10g, and the amount of cathode slurry used was 20g. The slurry in S1 was sprayed on both sides of the proton exchange membrane and dried into layers to obtain a 5wt.% anti-free radical additive CCM sample in the catalyst layer. The CCM sample was bonded to the test frame and then covered with gas diffusion layer carbon paper to obtain a membrane electrode named TS-5%-0.

[0044] The CCM samples prepared above were immersed in Fenton's reagent for 4 h, 8 h, and 12 h, respectively, at 80° C., and an accelerated chemical decay experiment was performed. The samples were named TS-5%-4, TS-5%-8, and TS-5%-12, respectively.

[0045] Comparative Example 1

[0046] S1. Preparation of membrane electrode: Weigh 0.1304 g of platinum carbon catalyst with a Pt content of 40 wt.% and pour it into a beaker, then add 12.5 g of deionized water, stir it evenly, add 0.2445 g of Nafion D2020 perfluorosulfonic acid dispersion and 11.9347 g of ethanol, and mix the slurry evenly by ultrasonic and high-speed shearing to obtain slurry.

[0047] S2: The amount of anode slurry used was controlled to be 10g, and the amount of cathode slurry used was 20g. The slurry obtained in S1 was sprayed on both sides of the proton exchange membrane, and dried into layers to obtain a CCM sample. The CCM sample was bonded to the test frame and then covered with gas diffusion layer carbon paper to obtain a membrane electrode, named BS-0.

[0048] The BS-0 samples prepared above were immersed in Fenton's reagent for 4 h, 8 h, and 12 h, respectively, at 80°C, and accelerated chemical decay experiments were performed. The samples were named BS-4, BS-8, and BS-12, respectively.

[0049] The samples prepared in the comparative examples and the examples were subjected to electrochemical performance tests, the battery temperature was 80°C, the relative humidity of the cathode and anode inlet was 50%, the back pressure was 100KPa and 80KPa respectively, and the polarization curve, electrochemical active area (ECSA), and ohmic resistance were obtained. The Fenton reagents after the accelerated decay of different samples were collected to test the F ion concentration.

[0050] like Figure 1 and Figure 2 As shown in the figure, compared with the membrane electrode BS-0 without adding fullerene anti-radical quencher, the battery performance of the membrane electrode TS-2%-0 and TS-5%-0 with adding amount of 2wt.% and 5wt.% is reduced, but the overall decline is small. The current density is 1200mA cm -2 When the cell voltage of BS-0 membrane electrode is 0.664 V, the peak current density is 941.4 mA cm -2 The cell voltage of TS-2%-0 membrane electrode is 0.652 V and the peak current density is 912.6 mA cm -2 The fullerene-based anti-radical membrane electrode structure has a current density of 1200 mA cm -2 When the peak current density is reduced by 34.4%, the membrane electrode attenuation rate is effectively alleviated, and the chemical stability is greatly improved.

[0051] Figure 3 and Figure 4 The membrane electrode samples with accelerated chemical decay for 12h were analyzed. Compared with the membrane electrode BS-0-12 without free radical scavenger, the membrane electrode TS-2%-12 and TS-5%-12 with 2wt.% and 5wt.% free radical scavenger added had a much lower degree of battery performance decline, and TS-5%-12 had the smallest decline. The current density was 1200mA cm -2 When the cell voltage of BS-12 membrane electrode is 0.378V, the peak current density is 510.4mA cm -2 The decrease rate is 45.78%; the cell voltage of TS-2%-0 membrane electrode is 0.443V, and the peak current density is 635.2mA cm -2 ,, the decline rate is 30.04%. It can be seen that the membrane electrode attenuation rate has been effectively alleviated and the chemical stability has been greatly improved.

[0052] Figure 5The ECSA of membrane electrode samples with different accelerated chemical decay times were analyzed and compared. The ECSA of the membrane electrode without added fullerene anti-radical quencher decreased significantly with the increase of decay time, and decreased by 43.28% after 12 hours. The degree of decrease in the membrane electrode with 2wt.% and 5wt.% fullerene anti-radical quencher added was significantly smaller.

[0053] Figure 6 The ohmic resistance of membrane electrode samples with different accelerated chemical decay times is given. Compared with the membrane electrodes with 2wt.% and 5wt.% fullerene anti-radical quencher added, the ohmic resistance of the membrane electrode without added fullerene anti-radical quencher decreases significantly with the increase of decay time.

[0054] Figure 7 The F ion loss rate after 12 hours of accelerated chemical decay of the membrane electrode is given. Compared with the membrane electrode without fullerene anti-radical quencher, the F ion loss rate of the membrane electrode TS-2% and TS-5% with fullerene anti-radical quencher added is greatly reduced. The reduction of F ion loss rate indicates that the decay degree of perfluorosulfonic acid structure is low and the original structure of the membrane electrode is protected.

[0055] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A fullerene-based anti-free radical membrane electrode, characterized in that: The membrane electrode comprises a catalyst layer and a proton exchange membrane, wherein the catalyst layer covers both sides of the proton exchange membrane; The catalyst layer comprises a catalyst, an ionomer, and a fullerene-based anti-radical quencher; The added mass percentage of the fullerene-based anti-radical quencher is 0.1%-10%; The added mass percentage of the ionomer is 10-40%.

2. The fullerene-based anti-radical membrane electrode according to claim 1, characterized in that: The fullerene-based anti-radical quencher is one or more of fullerene and fullerene derivatives.

3. The fullerene-based anti-radical membrane electrode according to claim 2, characterized in that: The fullerene derivatives include fullerene polyvinyl pyrrolidone and polyhydroxyfullerene.

4. The fullerene-based anti-radical membrane electrode according to claim 1, characterized in that: The particle size of the fullerene-based anti-radical quencher is 1-30 nm.

5. The fullerene-based anti-radical membrane electrode according to claim 1, characterized in that: The ionomer includes one or more of Nafion perfluorosulfonic acid resin dispersion and Aquivion perfluorosulfonic acid resin dispersion.

6. The fullerene-based anti-radical membrane electrode according to claim 1, characterized in that: The catalyst is a Pt / C catalyst, and the mass ratio of Pt in the Pt / C catalyst is 40%-60%.

7. A method for preparing a fullerene-based anti-free radical membrane electrode as claimed in any one of claims 1 to 6, characterized in that: The following steps are involved: S1: adding the catalyst and the ionomer into an alcohol / water mixed solvent, and then adding a fullerene-based anti-radical quencher, and stirring evenly to obtain a catalyst layer slurry; S2: The anode and cathode catalyst layer slurries are coated on the proton exchange membrane by transfer, scraping or spraying, and dried into layers to obtain CCM, and then covered with a gas diffusion layer to obtain a membrane electrode.

8. The method for preparing a fullerene-based anti-free radical membrane electrode according to claim 7, characterized in that: In S2, the gas diffusion layer is carbon paper.

9. The method for preparing a fullerene-based anti-free radical membrane electrode according to claim 7, characterized in that: In S1, the mass ratio of catalyst, ionomer and alcohol / water mixed solvent in the catalyst layer slurry is 1:4:180; The mass ratio of ethanol to water in the alcohol / water mixed solvent is 1:

1.