Recovery method of waste fuel cell membrane electrode key material
By separating and recovering the gas diffusion layer, proton exchange membrane and catalytic layer of the fuel cell membrane electrode, the problems of low recycling efficiency and environmental pollution in the prior art are solved, and an efficient and simplified membrane electrode recycling process is achieved, which is suitable for large-scale application.
Patent Information
- Application Number
- CN202411049220.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The existing fuel cell membrane electrode recycling technology has high costs, environmental pollution and complex processes, especially the low recovery efficiency of precious metal catalysts and proton exchange membranes, and ignores the treatment of the gas diffusion layer, which affects the regeneration performance of the membrane electrode.
By separating the gas diffusion layer, proton exchange membrane and catalytic layer of the waste fuel cell, the precious metal catalyst and perfluorosulfonic acid resin solution are recovered separately by using solvent peeling, acid impregnation, hydrothermal treatment and burning steps, the recovery efficiency is improved and the recovery efficiency is reduced. Impurity content.
It realizes efficient recycling of key materials for membrane electrodes, reduces production costs, simplifies process flow, reduces environmental pollution, and improves recycling rate. It is suitable for the recycling of large-scale waste membrane electrodes.
Smart Images

Figure CN118983457A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of membrane electrode recycling, and in particular to a method for recycling key materials of waste fuel cell membrane electrodes. Background Art
[0002] Proton exchange membrane fuel cells (PEMFC) have the advantages of cleanliness, high efficiency, safety and reliability, and have broad development potential and application prospects in many fields. They have received widespread attention in recent years. The key part and core component of proton exchange membrane fuel cells is the membrane electrode (MEA), which is assembled by a hot pressing process from a proton exchange membrane, anode and cathode catalyst layers, and cathode and cathode gas diffusion layers. The main material of the gas diffusion layer is carbon paper or carbon cloth, the main material of the catalyst layer is a precious metal catalyst, and the proton exchange membrane is mainly a perfluorosulfonic acid proton exchange membrane.
[0003] Currently, the high cost of proton exchange membrane fuel cells poses a huge challenge to their large-scale application. The cost of precious metal catalysts and proton exchange membranes accounts for about 70% of the total cost of MEA. Therefore, if the precious metal catalysts and proton exchange membranes can be recycled at the same time, it can not only effectively reduce the cost of fuel cells, but also make full use of resources and protect the environment, which is of great significance to further promote the commercial application of fuel cells.
[0004] In recent years, the recovery methods of key materials of membrane electrode have become common. For example, after the solvent treatment, simple separation and incineration, a large amount of residual organic solvent and resin will produce toxic fluoride, which will pollute the environment. Chinese patent CN110747341A discloses a method for recovering key materials from fuel cell membrane electrode, including the following steps: first, the membrane electrode is immersed in an organic reagent, and after the membrane electrode is swollen and deformed, it is crushed by an ultrasonic crusher; secondly, the mixed liquid obtained by ultrasound is taken out to remove the solid matter floating on the upper layer, and then the remaining liquid is filtered and the filtered residue is collected; the obtained filter residue is added to deionized water, and reacted in a high-pressure reactor to obtain a transparent solution with a precipitate; finally, the above-obtained transparent solution with a precipitate is placed in a muffle furnace for incineration treatment, and then the treated precipitate is completely dissolved in aqua regia, and formic acid is added dropwise to react to obtain platinum. This method adopts the high-pressure dissolution method in a reactor, and its reaction conditions need to be strictly controlled, which is not conducive to large-scale application. The normal pressure dissolution method easily destroys the sulfonic acid group, resulting in a decrease in membrane performance. In addition, the use of aqua regia solvent for dissolution requires a special non-operating environment, has a high implementation cost, and has complicated steps. There are problems such as low recovery rate and long nitrate removal time.
[0005] Chinese patent CN114678553A discloses a method for recycling and reusing waste proton exchange membrane water electrolysis membrane electrodes, which includes soaking the waste membrane electrodes in a solvent, peeling off the catalyst layer and the proton exchange membrane by ultrasound, scraping, and flushing, and then cleaning the proton exchange membrane with a solvent and performing a modification and regeneration treatment on it. This method can overcome the defects of the above-mentioned recycling method, but this method ignores the recycling of the gas diffusion layer. At the same time, after the membrane electrode is actually operated for a long time, the proton exchange membrane will inevitably increase the amount of hydrogen permeation, and it is almost difficult to reuse it by a re-modification method. The regeneration of the membrane will also increase the process complexity, and the proton conductivity of the proton exchange membrane cannot be guaranteed. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a method for recycling key materials of waste fuel cell membrane electrodes. The present invention fully recycles the gas diffusion layer, proton exchange membrane and catalytic layer of waste fuel cell membrane electrodes, with a simple process flow and high recycling efficiency.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for recycling key materials of waste fuel cell membrane electrode, comprising the following steps:
[0009] Separating the gas diffusion layer in the waste proton exchange membrane fuel cell membrane electrode to obtain a gas diffusion layer and a proton exchange membrane-catalyst layer composite material layer;
[0010] Immersing the gas diffusion layer in a first solvent for a first stripping treatment to obtain a first liquid suspension; performing solid-liquid separation on the first liquid suspension to obtain a microporous layer filter residue and a filtrate, wherein the microporous layer filter residue includes a noble metal catalyst and carbon powder, and the filtrate includes a perfluorosulfonic acid ionomer;
[0011] Immersing the proton exchange membrane-catalyst layer composite material layer in a second solvent for a second stripping treatment to obtain a proton exchange membrane and a second liquid suspension;
[0012] The proton exchange membrane is sequentially subjected to acid immersion heat treatment, hydrothermal treatment, drying, crushing and dissolving to obtain a perfluorosulfonic acid resin solution;
[0013] The second liquid suspension is mixed with water and subjected to heating treatment, and the obtained mixed liquid is subjected to solid-liquid separation to obtain a catalytic layer filter residue; the catalytic layer filter residue and the microporous layer filter residue are burned and then leached to obtain a leaching solution enriched with precious metals.
[0014] Preferably, the first solvent is one or more of water, ethanol, methanol, isopropanol, n-propanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide.
[0015] Preferably, the second solvent is one or more of water, ethanol, methanol, isopropanol, n-propanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide.
[0016] Preferably, the first stripping treatment and the second stripping treatment both include sequentially performing ultrasound, scraping and rinsing.
[0017] Preferably, the acid leaching solution used in the acid leaching heat treatment is one or more of sulfuric acid, hydrochloric acid and nitric acid, and the concentration of the acid leaching solution is 1.5 to 3 mol / L.
[0018] Preferably, the acid leaching heat treatment is carried out at a temperature of 80 to 150° C. and for a time of 12 to 24 hours.
[0019] Preferably, the temperature of the hydrothermal treatment is 80-150° C., and the time is 12-24 hours.
[0020] Preferably, the mass ratio of the water to the solvent in the second liquid suspension is 1:1 to 1:4; the temperature of the heating treatment is 120 to 200° C., and the time is 18 to 30 hours.
[0021] Preferably, the burning temperature is 450-550° C. and the burning time is 8-12 hours.
[0022] Preferably, the leaching includes a first leaching and a second leaching in sequence, the leaching liquid used in the first leaching is an inorganic acid, the inorganic acid is one or more of hydrochloric acid, sulfuric acid, nitric acid, perchloric acid and chlorous acid, and the concentration of the inorganic acid is 2 to 8 mol / L, and the leaching liquid used in the second leaching is an inorganic acid solution containing an oxidant, the concentration of the oxidant in the inorganic acid solution containing the oxidant is 1.5 to 8 mol / L, and the concentration of the inorganic acid is 2 to 10 mol / L.
[0023] The invention provides a method for recovering key materials of waste fuel cell membrane electrode, comprising the following steps: separating a gas diffusion layer in a waste proton exchange membrane fuel cell membrane electrode to obtain a gas diffusion layer and a proton exchange membrane-catalytic layer composite material layer; immersing the gas diffusion layer in a first solvent for a first stripping treatment to obtain a first liquid suspension; performing solid-liquid separation on the first liquid suspension to obtain a microporous layer filter residue and a filtrate, wherein the microporous layer filter residue comprises a noble metal catalyst and carbon powder, and the filtrate comprises a perfluorosulfonic acid ionomer; immersing the proton exchange membrane-catalytic layer composite material layer in a second solvent for a second stripping treatment to obtain a proton exchange membrane and a second liquid suspension; performing acid immersion heat treatment, hydrothermal treatment, drying, crushing and dissolving on the proton exchange membrane in sequence to obtain a perfluorosulfonic acid resin solution; mixing the second liquid suspension with water for a heating treatment, performing solid-liquid separation on the obtained mixed solution to obtain a catalyst layer filter residue; and leaching the catalyst layer filter residue and the microporous layer filter residue after burning to obtain a leaching solution enriched with noble metals. In the past, researchers often ignored the precious metal part taken away from the gas diffusion layer side in the process of recycling waste membrane electrodes. The present invention fully considers this point and recycles the ionomers and precious metals adhering to the surface of the microporous layer side after the gas diffusion layer is separated. This not only eliminates the interference of the gas diffusion layer on the catalyst recovery, but also improves the recovery efficiency of the precious metal catalyst; and, after the membrane electrode has been in actual operation for a long time, the proton exchange membrane will inevitably increase the amount of hydrogen permeation, and it is almost difficult to reuse it through the method of re-modification. The present invention conducts centralized recovery and treatment of the perfluorosulfonic acid ionomers in the catalyst layer and the proton exchange membrane, and finally obtains a perfluorosulfonic acid resin solution, which can be used for the subsequent synthesis of perfluorosulfonic acid ionomers or recast membranes. The recovery method provided by the present invention has the characteristics of simple process flow, high recovery efficiency, low impurity content, and low environmental pollution, and is particularly suitable for the recovery of large quantities of waste membrane electrodes in practical application fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a general schematic diagram of the waste fuel cell membrane electrode recovery process in the present invention;
[0025] Figure 2 This is a schematic diagram of the waste proton exchange membrane fuel cell membrane electrode recovery method of the present invention. DETAILED DESCRIPTION
[0026] The present invention provides a method for recycling key materials of waste fuel cell membrane electrode, comprising the following steps:
[0027] Separating the gas diffusion layer in the waste proton exchange membrane fuel cell membrane electrode to obtain a gas diffusion layer and a proton exchange membrane-catalyst layer composite material layer;
[0028] Immersing the gas diffusion layer in a first solvent for a first stripping treatment to obtain a first liquid suspension; performing solid-liquid separation on the first liquid suspension to obtain a microporous layer filter residue and a filtrate, wherein the microporous layer filter residue includes a noble metal catalyst and carbon powder, and the filtrate includes a perfluorosulfonic acid ionomer;
[0029] Immersing the proton exchange membrane-catalyst layer composite material layer in a second solvent for a second stripping treatment to obtain a proton exchange membrane and a second liquid suspension;
[0030] The proton exchange membrane is sequentially subjected to acid immersion heat treatment, hydrothermal treatment, drying, crushing and dissolving to obtain a perfluorosulfonic acid resin solution;
[0031] The second liquid suspension is mixed with water and subjected to heating treatment, and the obtained mixed liquid is subjected to solid-liquid separation to obtain a catalytic layer filter residue; the catalytic layer filter residue and the microporous layer filter residue are burned and then leached to obtain a leaching solution enriched with precious metals.
[0032] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.
[0033] The invention separates the gas diffusion layer in the waste proton exchange membrane fuel cell membrane electrode to obtain the gas diffusion layer and the proton exchange membrane-catalytic layer composite material layer.
[0034] In the present invention, the separation method is preferably to manually tear off the gas diffusion layer from the waste proton exchange membrane fuel cell membrane electrode.
[0035] After obtaining the gas diffusion layer, the present invention immerses the gas diffusion layer in a first solvent for a first stripping treatment to obtain a first liquid suspension; the first liquid suspension is subjected to solid-liquid separation to obtain a microporous layer filter residue and a filtrate, wherein the microporous layer filter residue includes a precious metal catalyst and carbon powder, and the filtrate includes a perfluorosulfonic acid ionomer.
[0036] After a fuel cell has been running for a long period of time, some ionomers and precious metals will adhere to the surface of the gas diffusion layer inside the battery (the side close to the catalyst layer). The present invention takes the stripping of the gas diffusion layer from the discarded proton exchange membrane fuel cell membrane electrode as the first step to recover key materials. The stripped gas diffusion layer will adhere to some perfluorosulfonic acid polyionomers, precious metal catalysts and a small amount of carbon powder in the microporous layer. In order to improve the efficiency of membrane electrode recovery, the present invention incorporates these materials into the membrane electrode recovery material.
[0037] In the present invention, the first solvent is preferably one or more of water, ethanol, methanol, isopropanol, n-propanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide, the water is preferably deionized water, and the first solvent is more preferably ethanol or N,N-dimethylformamide. In the present invention, the amount of the first solvent used is based on completely submerging the gas diffusion layer.
[0038] In the present invention, the first stripping treatment preferably includes sequentially performing ultrasound, scraping and rinsing, and the specific operation is preferably: immersing the gas diffusion layer in a first solvent, performing ultrasound treatment, and then sequentially performing scraping and rinsing on the gas diffusion layer; the number of ultrasound treatments is preferably 3 times, and the time for each ultrasound treatment is preferably 20 minutes. Through the first stripping treatment, the present invention separates the perfluorosulfonic acid ionomer and the noble metal catalyst adhered to the surface of the gas diffusion layer together with part of the carbon powder on the surface of the microporous layer from the gas diffusion layer to obtain a first liquid suspension.
[0039] In the present invention, the solid-liquid separation method is preferably to perform suction filtration and centrifugal separation in sequence. In the present invention, the main components of the microporous layer filter residue are precious metal catalyst and a small amount of carbon powder, and the perfluorosulfonic acid ionomer enters the filtrate, and the filtrate can be recycled.
[0040] After obtaining the proton exchange membrane-catalytic layer composite material layer, the present invention immerses the proton exchange membrane-catalytic layer composite material layer into a second solvent for a second stripping treatment to obtain a proton exchange membrane and a second liquid suspension.
[0041] In the present invention, the second solvent is preferably one or more of water, ethanol, methanol, isopropanol, n-propanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide, the water is preferably deionized water, and the second solvent is more preferably ethanol or N,N-dimethylformamide. In the present invention, the second solvent is based on completely submerging the proton exchange membrane-catalyst layer composite material layer.
[0042] In the present invention, the second stripping treatment includes sequentially performing ultrasound, scraping and rinsing, and the specific operation is preferably: immersing the proton exchange membrane-catalytic layer composite material layer in a second solvent, performing multiple ultrasounds, and then sequentially scraping and rinsing the proton exchange membrane-catalytic layer composite material layer; the number of ultrasounds is preferably more than 3 times, and the time of each ultrasound is preferably 15 to 20 minutes. The present invention peels off the catalytic layer and the proton exchange membrane in the proton exchange membrane-catalytic layer composite material layer through the second stripping treatment.
[0043] After the proton exchange membrane is obtained, the present invention sequentially performs acid immersion heat treatment, hydrothermal treatment, drying, crushing and dissolving on the proton exchange membrane to obtain a perfluorosulfonic acid resin solution.
[0044] Before the acid leaching heat treatment, the present invention preferably washes the proton exchange membrane with ethanol and ultrapure water to further remove residual impurities on the membrane surface.
[0045] In the present invention, the acid dip solution used in the acid dip heat treatment is preferably one or more of sulfuric acid, hydrochloric acid and nitric acid, more preferably sulfuric acid, and the concentration of the acid dip solution is preferably 1.5-3 mol / L, more preferably 2 mol / L; the amount of the acid dip solution is based on the complete immersion of the proton exchange membrane. In the present invention, the temperature of the acid dip heat treatment is preferably 80-150°C, more preferably 90-100°C, and the time is preferably 12-24h, more preferably 12-15h; the acid dip heat treatment is preferably carried out under rotary heating conditions. The present invention preferably places the proton exchange membrane after the acid dip heat treatment into deionized water for the hydrothermal treatment, and the resistivity of the deionized water is preferably 18MΩ·cm, and the amount of the deionized water is based on the complete immersion of the proton exchange membrane. In the present invention, the temperature of the hydrothermal treatment is preferably 80 to 150° C., more preferably 90 to 100° C., and the time is preferably 12 to 24 hours, more preferably 12 to 15 hours; the hydrothermal treatment is preferably carried out under rotary heating conditions.
[0046] After a long period of attenuation of the membrane electrode, the proton exchange membrane may contain impurities or residual manufacturing agents, which will affect the subsequent recovery of the ionomer material. The present invention performs acid immersion heat treatment on the proton exchange membrane in a low-concentration acid immersion solution to remove impurities, such as removing cationic impurities contained therein, and also can increase some acid groups to improve the proton transfer efficiency during the reuse of the ionomer; and then the hydrothermal treatment is used to remove other ions remaining on the surface of the proton exchange membrane to complete the cleaning of the membrane.
[0047] After the hydrothermal treatment, the present invention preferably rinses the obtained proton exchange membrane with deionized water and then dries it. In the present invention, the drying is preferably carried out in a drying oven, and the drying is based on drying the proton exchange membrane.
[0048] In the present invention, the crushing is preferably carried out by at least one of the following tools: a paper cutter, a shredder, a pulverizer. In the present invention, the solvent used for the dissolution is preferably one or more of toluene, xylene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide and N-methylpyrrolidone. In practical applications, after the life of the membrane electrode is terminated, it is difficult to reuse the proton exchange membrane, and the regeneration of the membrane will increase the complexity of the process, and the proton conductivity of the proton exchange membrane cannot be guaranteed. Therefore, the present invention, on the basis of separating the proton exchange membrane, crushes and dissolves the membrane to finally obtain an ionomer resin solution.
[0049] After obtaining the second liquid suspension, the present invention mixes the second liquid suspension with water and performs a heating treatment, and performs solid-liquid separation on the obtained mixed liquid to obtain a catalyst layer filter residue.
[0050] In the present invention, the second liquid suspension is mainly composed of perfluorosulfonic acid ionomer and precious metal catalyst, and most of them coexist in the solution in a coated form. In order to avoid environmental pollution and generation of harmful gases, it is necessary to separate the ionomer from the precious metal and recycle them separately.
[0051] In the present invention, the volume ratio of the water to the solvent in the second liquid suspension is preferably 1:1 to 1:4, more preferably 1:1, 1:2, 1:3 or 1:4, the water is preferably deionized water, and the water is added to wash away the impurity ions remaining on the catalyst surface to prevent the impurity ions from affecting the recovery of key materials. In the present invention, the temperature of the heat treatment is preferably 120 to 200 ° C, more preferably 150 to 180 ° C, the time is preferably 18 to 30 hours, more preferably 20 to 24 hours; the heat treatment is preferably carried out under the condition of rotary heating. The heat treatment is carried out in a mixed solution of solvent and water, the purpose of which is to separate the precious metal catalyst and the perfluorosulfonic acid ionomer in the catalytic layer filter residue. The higher the temperature, the more intense the thermal motion of the molecules. The present invention uses this feature to achieve the separation of the ionomer and the catalyst, thereby preventing the generation of harmful gases that pollute the environment during the subsequent high-temperature burning of the carbon material.
[0052] In the present invention, the solid-liquid separation method is preferably: using a filter membrane with a pore size of 0.1 μm to filter the mixed solution obtained by the heating treatment to obtain a catalyst layer filter residue and a filtrate. In the present invention, the main component of the catalyst layer filter residue is a precious metal catalyst, and the main component of the filtrate is a perfluorosulfonic acid ionomer. In the present invention, the filtrate is preferably subjected to rotary evaporation drying, crushing and dissolving in sequence to obtain a perfluorosulfonic acid resin solution.
[0053] In the embodiment of the present invention, it is necessary to detect the content of perfluorosulfonic acid ionomer in the filter residue and the filtrate to prove the successful separation of the ionomer and the noble metal catalyst, and the detection method can use X-ray fluorescence spectrometry (XRF), inductively coupled plasma analysis (ICP) or X-ray diffraction (XRD). In the present invention, the content of S in the catalyst layer filter residue is not higher than 2wt.%.
[0054] After obtaining the catalytic layer filter residue, the present invention burns the catalytic layer filter residue and the microporous layer filter residue and then leaches to obtain a leaching solution enriched with precious metals.
[0055] Before burning, the present invention preferably dries the catalytic layer filter residue and the microporous layer filter residue, and the drying is preferably vacuum drying. In the present invention, the burning temperature is preferably 450-550°C, and the time is preferably 8-12 hours. The present invention preferably grinds the catalytic layer filter residue into fine powder and places it in a crucible for burning. The present invention fully oxidizes the carbon material in the catalytic layer filter residue and the microporous layer filter residue into carbon dioxide and discharges it through the burning, thereby removing carbon substances.
[0056] In the present invention, the leaching preferably includes a first leaching and a second leaching in sequence. In the present invention, the leaching solution used in the first leaching is preferably an inorganic acid, and the inorganic acid is preferably one or more of hydrochloric acid, sulfuric acid, nitric acid, perchloric acid and chlorous acid. The concentration of the inorganic acid is preferably 2 to 8 mol / L, more preferably 2 to 3 mol / L, the temperature of the first leaching is preferably 80°C, and the time is preferably 2 hours. The present invention removes base metal impurities through the first leaching. After the first leaching is completed, centrifugal separation is performed, and the filter residue is collected, and the filter residue is subjected to a second leaching. In the present invention, the leaching solution used in the second leaching is preferably an inorganic acid solution containing an oxidant, and the oxidant in the inorganic acid solution containing an oxidant is preferably one or more of hydrogen peroxide, sodium peroxide, nitric acid and potassium permanganate, and the inorganic acid is preferably hydrochloric acid or sulfuric acid; the concentration of the oxidant in the inorganic acid solution containing an oxidant is preferably 1.5-8 mol / L, more preferably 1.5-2 mol / L, the concentration of the inorganic acid is preferably 2-10 mol / L, more preferably 2-3 mol / L, and the molar ratio of the oxidant to the inorganic acid is preferably 0.5-10:1; the temperature of the second leaching is preferably 60-80°C, and the time is preferably 3h. After the second leaching is completed, a leaching solution enriched in precious metals is obtained by solid-liquid separation. Most of the precious metal catalysts in the catalyst layer of the proton exchange membrane fuel cell are platinum catalysts. After the above treatment, a leaching solution enriched in platinum is obtained. In the present invention, the leaching solution enriched in precious metals is used as a platinum precursor solution after adjusting the pH value.
[0057] The present invention makes full use of the ionomer and precious metal adhered to the side surface of the microporous layer after the gas diffusion layer is peeled off, which not only eliminates the interference of the gas diffusion layer on the catalyst recovery (the catalyst layer is recovered after the gas diffusion layer is separated separately, eliminating the influence of carbon fiber and carbon powder in the gas diffusion layer on the recovery of membrane electrode assembly materials), but also improves the recovery efficiency of precious metal catalysts; the present invention uses a mild solvent to separate the catalyst layer from the proton exchange membrane on both sides of the membrane electrode, and then uses drying and filtering and burning to recover the proton exchange membrane and platinum respectively, which has the advantages of simple process flow, high recovery efficiency and low impurity content, and is particularly suitable for the recovery of large quantities of waste membrane electrodes in practical application fields , which helps to alleviate the pressure of scarce resources and the pressure of waste on the environment; the present invention takes into account both economy and environmental friendliness in the process of separating ionomers and precious metal catalysts, such as repeatedly performing solvent thermal treatment on the separated catalyst solution before the high-temperature burning and carbon removal process to achieve the separation of catalyst and polymer, so that no harmful gas HF is generated during the high-temperature burning process, avoiding pollution to the environment, and no need for supporting expensive HF absorption equipment; the precious metal-enriched leachate recovered by the present invention can be directly used as a precious metal precursor in the synthesis process, so in some occasions where precious metal solutions are used, the necessary step of recovering precious metals in the form of metal elements or metal compounds is avoided. The present invention realizes the rapid and efficient recovery of proton exchange membranes and precious metals from waste proton exchange membrane fuel cell membrane electrodes.
[0058] In order to further illustrate the present invention, the method for recycling key materials of waste fuel cell membrane electrode provided by the present invention is described in detail below in combination with examples, but they should not be understood as limiting the scope of protection of the present invention.
[0059] Example 1
[0060] Method for recycling key materials of membrane electrode of proton exchange membrane fuel cell, the process is as follows Figure 2 As shown, the specific steps are as follows:
[0061] (1) Take a single cell test with an active area of 25 cm 2 The membrane electrode of the waste proton exchange membrane fuel cell uses platinum-carbon catalysts for both the cathode and anode, and the cathode platinum loading is 0.3 mg / cm 2 , the anode platinum loading is 0.1 mg / cm 2 , then there is a total of 10 mg of platinum in the membrane electrode;
[0062] (2) manually tearing the gas diffusion layer on the surface of the intact membrane electrode from the surface of the catalyst layer, and immersing it in ethanol sufficient to submerge it, and performing ultrasonic treatment three times, each ultrasonic treatment lasting 20 minutes, and then separating the ionomer and precious metal catalyst adhered to the surface of the gas diffusion layer together with part of the carbon powder on the surface of the microporous layer by repeated scraping and washing, collecting the liquid suspension, and obtaining the microporous layer filter residue by suction filtration and centrifugal separation;
[0063] (3) soaking the remaining proton exchange membrane and catalyst layer in ethanol and performing ultrasonic treatment three times, each ultrasonic treatment lasting 15 minutes. After the soaking is completed, the catalyst layer and the proton exchange membrane are peeled off by scraping and washing. The waste proton exchange membrane is washed with ethanol and ultrapure water, immersed in a 2 mol / L sulfuric acid solution, heat treated at 90° C. for 12 hours, and then heat treated in ultrapure water at 90° C. for 12 hours, and placed in a drying oven for drying.
[0064] (4) collecting the liquid suspension after the proton exchange membrane is stripped in step (3), adding deionized water in a volume ratio of 1:1 to the solvent to the liquid suspension, and rotating and heating at 180° C. for 24 hours, and then using a filter membrane with a pore size of 0.1 μm to separate by suction to obtain a catalyst layer residue, wherein the residue is mostly composed of precious metal catalysts, and the solid polymer has been separated at this time, and the content of perfluorosulfonic acid ionomer in the filtrate and the residue is detected by XRF. The test results show that the element content of S in the filtrate is 21.56%, and the element content of S in the residue is 1.31%, which fully proves that the perfluorosulfonic acid ionomer is successfully filtered into the filtrate, realizing the separation of the catalyst and the ionomer, and avoiding the subsequent burning of the residue to produce harmful gases to pollute the environment;
[0065] (5) The membrane dried in step (3) is crushed by a pulverizer, and then dissolved into a perfluorosulfonic acid resin solution using a solvent toluene solution. The microporous layer filter residue obtained in step (2) and the catalytic layer filter residue obtained in step (4) are dried and ground into fine powder, and then the filter residue is placed in a crucible and calcined in air at 450°C for 8 hours to fully oxidize the carbon material into carbon dioxide and discharge it, thereby obtaining a residual substance in the crucible, wherein the main component of the residual substance is metal platinum, which is weighed to obtain 9.6 mg, and the calculated recovery rate of platinum is 96%; the residual substance is immersed in 2 mol / L hydrochloric acid, reacted at 80°C for 2 hours to remove the base metal therein, and centrifuged to obtain a filter residue; finally, the filter residue is added to 25 mL of a 3 mol / L hydrochloric acid solution (containing 2 mol / L hydrogen peroxide), reacted at 60°C for 3 hours to leach the precious metal, and a chloroplatinic acid solution is obtained.
[0066] Example 2
[0067] Method for recycling key materials of membrane electrode of proton exchange membrane fuel cell, the process is as follows Figure 2 As shown, the specific steps are as follows:
[0068] (1) Take two single cells for testing with an active area of 25 cm 2 The membrane electrode of the waste proton exchange membrane fuel cell uses platinum-carbon catalysts for both the cathode and anode, and the cathode platinum loading is 0.15 mg / cm 2 , the anode platinum loading is 0.05 mg / cm 2 , then the membrane electrode contains a total of 10 mg of precious metal platinum;
[0069] (2) manually tearing the gas diffusion layer on the surface of the intact membrane electrode from the surface of the catalyst layer, and immersing it in N,N-dimethylformamide enough to submerge it, and performing ultrasonic treatment three times, each ultrasonic treatment lasting 20 minutes, and then separating the ionomer and precious metal catalyst adhered to the surface of the gas diffusion layer together with part of the carbon powder on the surface of the microporous layer by repeated scraping and washing, collecting the liquid suspension, and obtaining the microporous layer filter residue by suction filtration and centrifugal separation;
[0070] (3) soaking the remaining proton exchange membrane and catalyst layer in N,N-dimethylformamide for 3 ultrasonic treatments, each ultrasonic treatment lasting 20 minutes. After soaking, the catalyst layer and the proton exchange membrane are peeled off by scraping and washing. The waste proton exchange membrane is washed with ethanol and ultrapure water, immersed in a 3 mol / L sulfuric acid solution, heat treated at 100° C. for 15 hours, and then heat treated in ultrapure water at 100° C. for 15 hours, and then placed in a drying oven for drying.
[0071] (4) collecting the liquid suspension after stripping the proton exchange membrane in step (3), adding deionized water in a volume ratio of 1:2 to the solvent to the liquid suspension, and rotating and heating at 180° C. for 24 hours, and then using a filter membrane with a pore size of 0.1 μm to separate by suction to obtain a catalyst layer filter residue, wherein the filter residue is mostly composed of precious metal catalysts, and the solid polymer has been separated at this time, and the content of perfluorosulfonic acid ionomer in the filtrate and the filter residue is detected by XRF. The test results show that the element content of S in the filtrate is 20.19%, and the element content of S in the filter residue is 1.86%, which fully proves that the perfluorosulfonic acid ionomer is successfully filtered into the filtrate, realizing the separation of the catalyst and the ionomer, and avoiding the subsequent burning of the filter residue to produce harmful gases to pollute the environment;
[0072] (5) The membrane dried in step (3) is crushed by a pulverizer, and then dissolved into a perfluorosulfonic acid resin solution using a solvent toluene solution. The microporous layer filter residue obtained in step (2) and the catalytic layer filter residue obtained in step (4) are dried and ground into fine powder, and then the filter residue is placed in a crucible and calcined in air at 550°C for 12 hours to fully oxidize the carbon material into carbon dioxide and discharge it, thereby obtaining a residual substance in the crucible, wherein the main component of the residual substance is metal platinum, which is weighed to obtain 9.52 mg, and the calculated recovery rate of platinum is 95.2%; the residual substance is immersed in 3 mol / L sulfuric acid, reacted at 80°C for 2 hours to remove the base metal therein, and centrifuged to obtain a filter residue; finally, the filter residue is added to 25 mL of a 3 mol / L hydrochloric acid solution (containing 1.5 mol / L sodium peroxide), reacted at 80°C for 3 hours to leach the precious metal, and a chloroplatinic acid solution is obtained.
[0073] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.
Claims
1. A method for recycling key materials of waste fuel cell membrane electrode, characterized in that: The following steps are involved: Separating the gas diffusion layer in the waste proton exchange membrane fuel cell membrane electrode to obtain a gas diffusion layer and a proton exchange membrane-catalyst layer composite material layer; Immersing the gas diffusion layer in a first solvent for a first stripping treatment to obtain a first liquid suspension; performing solid-liquid separation on the first liquid suspension to obtain a microporous layer filter residue and a filtrate, wherein the microporous layer filter residue includes a noble metal catalyst and carbon powder, and the filtrate includes a perfluorosulfonic acid ionomer; Immersing the proton exchange membrane-catalyst layer composite material layer in a second solvent for a second stripping treatment to obtain a proton exchange membrane and a second liquid suspension; The proton exchange membrane is sequentially subjected to acid immersion heat treatment, hydrothermal treatment, drying, crushing and dissolving to obtain a perfluorosulfonic acid resin solution; The second liquid suspension is mixed with water and subjected to heating treatment, and the obtained mixed liquid is subjected to solid-liquid separation to obtain a catalytic layer filter residue; the catalytic layer filter residue and the microporous layer filter residue are burned and then leached to obtain a leaching solution enriched with precious metals.
2. The recycling method according to claim 1, characterized in that: The first solvent is one or more of water, ethanol, methanol, isopropanol, n-propanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide.
3. The recycling method according to claim 1, characterized in that: The second solvent is one or more of water, ethanol, methanol, isopropanol, n-propanol, acetone, N,N-dimethylformamide and dimethyl sulfoxide.
4. The recovery method according to any one of claims 1 to 3, characterized in that: The first stripping treatment and the second stripping treatment both include sequentially performing ultrasound, scraping and rinsing.
5. The recycling method according to claim 1, characterized in that: The acid leaching solution used in the acid leaching heat treatment is one or more of sulfuric acid, hydrochloric acid and nitric acid, and the concentration of the acid leaching solution is 1.5-3 mol / L.
6. The recycling method according to claim 5, characterized in that: The temperature of the acid leaching heat treatment is 80-150° C. and the time is 12-24 hours.
7. The recycling method according to claim 1, characterized in that: The temperature of the hydrothermal treatment is 80-150° C., and the time is 12-24 hours.
8. The recycling method according to claim 1, characterized in that: The mass ratio of the water to the solvent in the second liquid suspension is 1:1 to 1:4; the temperature of the heating treatment is 120 to 200° C., and the time is 18 to 30 hours.
9. The recycling method according to claim 1, characterized in that: The burning temperature is 450-550° C. and the burning time is 8-12 hours.
10. The recycling method according to claim 1, characterized in that: The leaching includes a first leaching and a second leaching in sequence, wherein the leaching liquid used in the first leaching is an inorganic acid, which is one or more of hydrochloric acid, sulfuric acid, nitric acid, perchloric acid and chlorous acid, and the concentration of the inorganic acid is 2 to 8 mol / L, and the leaching liquid used in the second leaching is an inorganic acid solution containing an oxidant, the concentration of the oxidant in the inorganic acid solution containing the oxidant is 1.5 to 8 mol / L, and the concentration of the inorganic acid is 2 to 10 mol / L.
Citation Information
Patent Citations
Method for recovering platinum catalyst from waste membrane electrode of proton exchange membrane fuel cell
CN113363521A
Recycling method of waste proton exchange membrane electrolysis water membrane electrode
CN114678553A
Method for seperating electrolyte and gas diffusion layer from mea and method for recovering platinum group metals
KR1020130000671A
Method for recovering noble metal
US20090226352A1
Cited By
Recovery method of waste proton exchange membrane electrolyzed water membrane electrode
CN120330799A
Membrane electrode catalyst layer stripping device and method, failure detection method and catalyst layer recovery method
CN122013251A