Vibrating diaphragm, sound production device and electronic equipment
By using air-pressure formed composite membranes in acoustic products, combined with the laminated structure of hydrogenated nitrile rubber and EPDM rubber, the problem of high application cost of EPDM rubber is solved, and good damping and rebound properties are achieved. Meet acoustic performance requirements.
Patent Information
- Application Number
- CN202410866354.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-08
AI Technical Summary
The application of EPDM rubber in acoustic products suffers from the problem of high cost, and its vulcanization process needs to be carried out in an oxygen-free environment, which limits the production process and cost, resulting in the inability to be widely promoted.
A composite membrane formed by air pressure is formed by stacking hydrogenated nitrile rubber film layers and EPDM rubber film layers, isolating oxygen during the air pressure forming process, and utilizing the carboxyl groups in the hydrogenated nitrile butadiene rubber film layer for cross-linking. , forming a composite membrane with good damping and resilience properties.
It reduces production costs and realizes the effective application of EPDM rubber in acoustic products. It has both good damping and rebound properties and meets acoustic performance requirements.
Smart Images

Figure CN118748768A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of acoustic technology, and in particular to a diaphragm, a sound-generating device and an electronic device. Background Art
[0002] Ethylene Propylene Diene Monomer (EPDM) is formed by copolymerization of ethylene, propylene and a small amount of non-conjugated dienes. It has good elasticity and is usually used in diaphragm materials. However, since the vulcanizing agent of EPDM can only be sulfur-containing compounds or peroxide compounds, its vulcanization process belongs to free radical polymerization and cannot react in the presence of oxygen, the diaphragm of EPDM material can only be formed by molding, and the production cost is too high, so the diaphragm of EPDM material cannot be promoted and applied in acoustic products. Summary of the invention
[0003] The main purpose of the present invention is to provide a diaphragm, a sound-generating device and an electronic device, aiming to solve the technical problem of high cost of using EPDM rubber in acoustic products, and the diaphragm can have good rebound and damping properties to improve the sound effect.
[0004] To achieve the above object, the present invention provides a diaphragm, wherein the diaphragm is a composite film formed by air pressure, and the composite film comprises a hydrogenated nitrile rubber film layer and an EPDM rubber film layer stacked;
[0005] When the EPDM rubber film layer is located on the outer layer of the composite film, the EPDM rubber film layer is attached to a molding die and subjected to air pressure molding to obtain the composite film;
[0006] The main components of the hydrogenated nitrile rubber film layer are shown in the following formula (I):
[0007]
[0008] Wherein, x, y, z, m, and n represent the number of each group respectively, x, y, and z are natural numbers and are not zero at the same time, and m and n are positive integers;
[0009] The original polymerizable monomer of R is an ethylenically unsaturated monocarboxylic acid or an ethylenically unsaturated dicarboxylic acid.
[0010] In one embodiment, the ethylenically unsaturated monocarboxylic acid comprises acrylic acid, methacrylic acid, ethacrylic acid, crotonic acid or cinnamic acid;
[0011] And / or, the ethylenically unsaturated dicarboxylic acid comprises fumaric acid, maleic acid, glutaconic acid, allylmalonic acid, mesaconic acid, tolconic acid, itaconic acid or taconic acid.
[0012] In one embodiment, the mass content of the carboxylic acid groups in the hydrogenated nitrile rubber film layer is 0.5 wt % to 5 wt %.
[0013] In one embodiment, the composite film further comprises at least one of a reinforcing agent, an antioxidant, a dye, a plasticizer, an anti-ultraviolet additive, an antistatic agent, a cross-linking agent, a vulcanizing agent and a vulcanization accelerator.
[0014] In one embodiment, the reinforcing agent includes at least one of talc, silicon dioxide and carbon black, and the weight proportion of the reinforcing agent in the composite film is 20wt% to 65wt%;
[0015] And / or, the antioxidant includes at least one of antioxidant N-445, antioxidant 246, antioxidant 4010, antioxidant SP, antioxidant RD, antioxidant ODA, antioxidant OD and antioxidant WH-02, and the antioxidant is added in an amount of 0.5-10 parts by mass;
[0016] And / or, the cross-linking agent includes at least one of hexamethylenediamine, hexamethylenediamine salt, hexamethylenediamine carbamate, triethylenetetramine, 2,2'-methylenedianiline and di-o-tolylguanidine.
[0017] In one embodiment, the total thickness of the composite film is 20 μm to 120 μm;
[0018] And / or, the thickness of the hydrogenated nitrile rubber film layer accounts for 20% to 70% of the total thickness of the composite film.
[0019] In one embodiment, the glass transition temperature of the EPDM rubber film layer is -30°C to -60°C;
[0020] And / or, the room temperature storage modulus of the composite film is 2 MPa to 50 MPa.
[0021] In one embodiment, the density of the composite film is 1.1 g / cm 3 ~1.5g / cm 3 ;
[0022] And / or, the stress retention rate of the composite film during stress relaxation is greater than or equal to 55%.
[0023] In one embodiment, the composite film is formed into a double-layer composite structure, and the composite film includes a layer of the hydrogenated nitrile rubber film layer and a layer of the EPDM rubber film layer;
[0024] Alternatively, the composite film is formed into a three-layer composite structure, the composite film includes two layers of the hydrogenated nitrile rubber film layers and one layer of the EPDM rubber film layer, and the two layers of the hydrogenated nitrile rubber film layers are arranged on opposite sides of the EPDM rubber film layer.
[0025] The present invention also provides a sound-generating device, which includes the diaphragm as described above.
[0026] In one embodiment, the sound-generating device includes a magnetic circuit system and a vibration system; the vibration system includes a voice coil, a first diaphragm and a second diaphragm; the first diaphragm and the second diaphragm are respectively arranged at the two axial ends of the voice coil, one end of the voice coil drives the first diaphragm to vibrate and produce sound, and the other end of the voice coil is connected to one end of the second diaphragm to balance the vibration of the voice coil, and the first diaphragm and / or the second diaphragm are the diaphragms described above.
[0027] The present invention further provides an electronic device, which includes the sound-generating device as described above.
[0028] The present invention provides a diaphragm, a sound-generating device and an electronic device. The diaphragm is a composite film formed by air pressure, and the composite film comprises a hydrogenated nitrile rubber film layer and an EPDM rubber film layer which are stacked. When the EPDM rubber film layer is located on the outer layer of the composite film, the EPDM rubber film layer is fitted to a molding mold and subjected to air pressure forming to obtain the composite film, and the hydrogenated nitrile rubber film layer contains a carboxyl group. A composite film is formed by compounding a hydrogenated nitrile rubber film layer containing a carboxyl group and an EPDM rubber film layer. During air pressure molding, the EPDM rubber film layer is fitted with a molding mold, that is, the EPDM rubber film layer is located between the hydrogenated nitrile rubber film layer and the molding mold. The hydrogenated nitrile rubber film layer can isolate oxygen and provide an oxygen-free environment for the vulcanization of the EPDM rubber. The hydrogenated nitrile rubber contains carboxyl groups and can be cross-linked in an air environment to form a hydrogenated nitrile rubber film layer with good damping performance. Therefore, the composite film can take into account good damping and rebound performance and meet the acoustic performance requirements. In addition, since air pressure molding is used instead of compression molding, the production cost is reduced, thereby solving the problem of excessively high cost of EPDM rubber in acoustic products. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present drawings or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present drawings. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.
[0030] Figure 1 A schematic diagram of the structure of a composite membrane according to an embodiment of the present invention;
[0031] Figure 2 It is a schematic diagram of gas pressure forming of a composite film with a double-layer composite structure according to an embodiment of the present invention;
[0032] Figure 3 A schematic diagram of the structure of a composite film with a three-layer composite structure according to an embodiment of the present invention;
[0033] Figure 4 A cross-sectional view of an embodiment of a sound-generating device according to the present invention;
[0034] Figure 5 It is a cross-sectional view of another embodiment of the sound-generating device according to the present invention.
[0035] Description of Figure Numbers:
[0036] L1, hydrogenated nitrile rubber film layer; L2, EPDM rubber film layer;
[0037] 100, sound-generating device; 110, housing; 120, diaphragm;
[0038] 121, a first diaphragm; 122, a second diaphragm;
[0039] 130. Voice coil; 140. Magnetic circuit system.
[0040] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0041] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with the accompanying drawings and embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.
[0042] An embodiment of the present invention provides a diaphragm, wherein the diaphragm is a composite film formed by air pressure. Figure 1 A schematic diagram of the structure of a composite membrane is shown in FIG. Figure 1 As shown, the composite film includes a hydrogenated nitrile rubber film layer L1 and an EPDM rubber film layer L2 which are stacked; when the EPDM rubber film layer L2 is located at the outer layer of the composite film, the EPDM rubber film layer L2 is bonded to a molding mold for air pressure molding to obtain the composite film; the main components of the hydrogenated nitrile rubber film layer L1 are shown in the following formula (I):
[0043]
[0044] Wherein, x, y, z, m, and n represent the number of each group respectively, x, y, and z are natural numbers and are not zero at the same time, and m and n are positive integers; the original polymerized monomer of R is an ethylenically unsaturated monocarboxylic acid or an ethylenically unsaturated dicarboxylic acid.
[0045] Hydrogenated nitrile rubber (HNBR) refers to the product obtained by hydrogenating the carbon-carbon double bond on the nitrile rubber molecular chain. Its saturation is higher than that of nitrile rubber, and it has good oil resistance, heat resistance, ozone resistance, chemical corrosion resistance, and high strength. The hydrogenated nitrile rubber film used in the present embodiment also has a monomer containing a carboxyl group in its molecular structure. Due to the introduction of the carboxyl group, the hydrogenated nitrile rubber can be cross-linked and cured by the carboxyl group. This process can be carried out in an air environment, so the hydrogenated nitrile rubber film can be air-pressed. The above-mentioned x, y, and z are not zero at the same time, and the specific values of x, y, and z vary with the structure and degree of hydrogenation of the butadiene monomer used. M represents the number of acrylonitrile monomers. N represents the number of ethylenically unsaturated monocarboxylic acids or ethylenically unsaturated dicarboxylic acid monomers containing carboxyl groups.
[0046] EPDM refers to a copolymer of ethylene, propylene and non-conjugated dienes. The vulcanization process of EPDM belongs to free radical polymerization, which needs to be carried out in an environment isolated from oxygen and can only be formed by compression molding. In this embodiment, the EPDM film layer and the hydrogenated nitrile rubber film layer are compounded by air pressure molding. During the air pressure molding process, the hydrogenated nitrile rubber film layer is placed on the side in contact with the air to isolate the EPDM film layer from the air, so that the vulcanization process of the EPDM film layer can proceed smoothly.
[0047] The composite film includes a hydrogenated nitrile rubber film layer L1 and an EPDM rubber film layer L2 which are stacked. When the EPDM rubber film layer L2 is located at the outer layer of the composite film, the EPDM rubber film layer L2 is fitted with a molding die for air pressure molding. The outer layer of the composite film refers to the film layer of the composite film in contact with the outside world. The composite film includes at least two layers. When the number of layers is two, both layers belong to the outer layer, and when the number of layers is further increased, the film layers on both sides of the composite film in contact with the outside world are the outer layers. By setting the fitting method between the film layer and the molding die during the air pressure molding process, it can be ensured that the EPDM rubber is vulcanized in an oxygen-isolated environment. The EPDM rubber film layer L2 has good resilience, and the hydrogenated nitrile rubber film layer has better damping performance, so the composite film can have both performances.
[0048] Figure 1 The composite membrane shown in is a double-layer composite structure, such as Figure 1 As shown, in one practicable manner, the composite membrane is formed into a double-layer composite structure, including a hydrogenated nitrile rubber membrane layer L1 and an EPDM rubber membrane layer L2. Figure 2 Schematic diagram of air pressure molding of a composite film with a double-layer composite structure, Figure 2As shown, the EPDM rubber film layer L2 is bonded to the mold surface of the molding mold, and the hydrogenated nitrile rubber film layer L1 is exposed to the punching air. The air enters from the air pressure channel and is compressed to pressurize the composite film, so that the composite film is tightly attached to the mold surface, and after cooling and shaping, it forms a shape corresponding to the mold.
[0049] Figure 3 The schematic diagram of the structure of the composite membrane with three-layer composite structure is as follows: Figure 3 As shown, in an practicable manner, the composite film is formed into a three-layer composite structure, including two hydrogenated nitrile rubber film layers L1 and one EPDM rubber film layer L2, and the two hydrogenated nitrile rubber film layers L1 are arranged on opposite sides of the EPDM rubber film layer L1. In this three-layer composite structure, the EPDM rubber is located in the inner layer of the composite film, and both sides are wrapped by the hydrogenated nitrile rubber film layer. During the air pressure molding process, both sides of the composite film can be used as the side that fits the molding mold, providing an oxygen-isolated environment for the EPDM rubber film layer.
[0050] Alternatively, the ethylenically unsaturated monocarboxylic acid comprises acrylic acid, methacrylic acid, ethacrylic acid, crotonic acid or cinnamic acid;
[0051] And / or, the ethylenically unsaturated dicarboxylic acid includes fumaric acid, maleic acid, glutaconic acid, allylmalonic acid, mesaconic acid, tolconic acid, itaconic acid or taconic acid.
[0052] By using ethylenically unsaturated monocarboxylic acids or ethylenically unsaturated dicarboxylic acids as the original polymerization monomers, carboxyl groups can be introduced into the hydrogenated nitrile rubber film layer as the basis for subsequent crosslinking and curing. For the same number of monomers, the content of carboxylic acid groups introduced by ethylenically unsaturated dicarboxylic acids is higher than that of ethylenically unsaturated monocarboxylic acids. Carboxylic acid groups can crosslink with other reactive groups to form crosslinking sites. Within a certain range, the more crosslinking sites there are, the more difficult it is for the molecular chain to move, resulting in an increase in the glass transition temperature and an increase in the damping factor; and the higher the mechanical strength of the material, the lower the elongation at break and the elastic recovery rate.
[0053] Optionally, the mass content of carboxylic acid groups in the hydrogenated nitrile rubber film layer is 0.5wt% to 5wt%, for example, the mass content of carboxylic acid groups in the hydrogenated nitrile rubber film layer is 0.5wt%, 0.8wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 4wt%, 5wt%, etc. It is understandable that when the content of carboxyl groups is less than 0.5wt%, the cross-linking sites formed during the vulcanization process are too few, and the mechanical strength of the material is insufficient. When the content of carboxyl groups is greater than 5wt%, the cross-linking density is too large, the elongation at break of the material is reduced, the resilience is poor, and the phenomenon of film breakage is prone to occur during the vibration of the product. When the mass content of carboxylic acid groups in the hydrogenated nitrile rubber film layer is 0.5wt% to 5wt%, not only can moderate cross-linking density be guaranteed, the mechanical strength of the hydrogenated nitrile rubber film layer be improved, but also the resilience of the hydrogenated nitrile rubber film layer can be guaranteed, that is, the mechanical strength and resilience of the hydrogenated nitrile rubber film layer can be taken into account.
[0054] Optionally, the composite film further comprises at least one of a reinforcing agent, an antioxidant, a dye, a plasticizer, an anti-ultraviolet additive, an antistatic agent, a crosslinking agent, a vulcanizing agent and a vulcanization accelerator. By adding the above additives, the processing can be smoothly carried out, or the various properties of the composite film can be improved.
[0055] Reinforcement agent can be used to improve the strength of composite film. In the present embodiment, both hydrogenated nitrile rubber membrane layer and EPDM rubber membrane layer can use reinforcing agent to improve strength. Optionally, reinforcing agent includes at least one of talcum powder, silicon dioxide and carbon black. Taking silicon dioxide as an example, its surface contains groups such as silanol, when it is added to hydrogenated nitrile rubber membrane layer, due to the strong interaction between its surface and hydrogenated nitrile interface, when the material is stressed, the molecular chain is easier to slide on the silicon dioxide surface, but it is not easy to separate from it, and hydrogenated nitrile elastomer and silicon dioxide constitute a strong bond that can slide, so that the mechanical strength is increased.
[0056] Optionally, the mass proportion of the reinforcing agent in the composite film is 20wt% to 65wt%, for example, 20wt%, 25wt%, 30wt%, 40wt%, 45wt%, 50wt%, 60wt%, 65wt%, etc. The elongation at break and tensile strength of the composite films with different silica contents are shown in Table 1 below. It can be seen from Table 1 that when the amount of silica is less than 20wt%, the composite film layer is not strong enough, and the prepared product is easily deformed and not mass-producible; when the amount of silica is higher than 65wt%, the elongation at break is significantly reduced, the material toughness is insufficient, and the prepared diaphragm is prone to film breakage during vibration.
[0057] Table 1
[0058] Silica content (wt%) 15 20 65 70 Composite film elongation at break (%) 451 432 151 93 Composite film tensile strength (MPa) 7.4 9.2 14.2 16.1
[0059] Anti-aging agent has the effect of delaying the aging of polymer compounds. In the use process of polymer materials, as time goes by, the molecular chain breaks and produces free radicals, which accelerates self-aging. Adding antioxidant can stop the autocatalytic active free radicals produced in polymer products. The antioxidant used in the present embodiment includes at least one of antioxidant N-445, antioxidant 246, antioxidant 4010, antioxidant SP, antioxidant RD, antioxidant ODA, antioxidant OD and antioxidant WH-02. Optionally, the addition of antioxidant in composite film is 0.5-10 mass parts, for example, 0.5 mass parts, 1 mass parts, 3 mass parts, 5 mass parts, 8 mass parts, 10 mass parts, etc. Optionally, the addition of antioxidant in composite film is 1-5 mass parts. Too little addition does not reach the effect of extending the service life, and too much addition, because it can not be better miscible with elastomer, is difficult to be evenly dispersed, causing the mechanical properties of the material to decline.
[0060] The cross-linking agent can cross-link with the carboxyl groups in the hydrogenated nitrile rubber film layer. The cross-linking agent used in this embodiment is an amine cross-linking agent, including at least one of hexamethylenediamine, hexamethylenediamine salt, hexamethylenediamine carbamate, triethylenetetramine, 2,2'-methylenedianiline and di-o-tolylguanidine. The amount of the cross-linking agent can be determined according to the actual content of the carboxylic acid group to ensure that a sufficient number of cross-linking sites can be formed to improve the mechanical strength of the composite film, and too much cross-linking density will not be added to cause the film to break.
[0061] The dye can dye the composite film, and by adding the dye, the diaphragm can be made into different colors to increase the aesthetics. The dye can be selected according to actual needs, and this embodiment does not limit this.
[0062] The plasticizer is used to improve the processing properties of the raw materials for preparing the composite film, improve the wettability, adhesion and fluidity between the components, and facilitate the mixing and processing of the components and the molding of the composite film. Optionally, the plasticizer includes at least one of a petroleum plasticizer, a coal tar plasticizer, a rosin oil plasticizer, a fatty oil plasticizer, a fatty dibasic acid ester, a fatty acid, a phosphate ester, a polyester, an epoxy, etc.
[0063] Anti-ultraviolet additives are used to improve the ability of the diaphragm to resist ultraviolet rays. Rubber products degrade under ultraviolet radiation. By adding ultraviolet absorbers, the diaphragm can have ultraviolet absorption function, thereby effectively resisting ultraviolet rays. Anti-ultraviolet additives include at least one of salicylates, benzophenones, benzotriazoles, triazines, hindered amines, substituted acrylonitriles, etc.
[0064] The addition of antistatic agent can prevent dust from being adsorbed on the surface of the diaphragm without affecting the processing and performance of the diaphragm.
[0065] The vulcanizing agent is used in the vulcanization process of EPDM rubber. The vulcanizing agent used in this embodiment may include a sulfur-containing compound or a peroxide vulcanizing agent. The sulfur-containing compound is such as sulfur and organic disulfide, and the peroxide vulcanizing agent is such as diisopropylbenzene peroxide and di-tert-butyl peroxide.
[0066] The vulcanization accelerator can promote vulcanization, shorten the vulcanization time, lower the vulcanization temperature, and reduce the amount of vulcanizer used. The vulcanization accelerator used includes vulcanization accelerator M, vulcanization accelerator D, or vulcanization accelerator TT.
[0067] Optionally, the total thickness of the composite film is 20 μm to 120 μm, for example, 20 μm, 40 μm, 50 μm, 60 μm, 80 μm, 100 μm, 120 μm, etc. The total thickness of the composite film is controlled within a certain range. If the total thickness is too thin, the mechanical properties of the diaphragm are insufficient and the film is prone to breakage; if the total thickness is too thick, a larger vibration space is occupied, which affects the sound performance of the diaphragm.
[0068] Optionally, the thickness of the hydrogenated nitrile rubber film layer accounts for 20% to 70% of the total thickness of the composite film, for example, 20%, 30%, 40%, 50%, 60%, 70%, etc. It is understandable that when the thickness of the hydrogenated nitrile rubber film layer is less than 20%, it cannot prevent the penetration of oxygen, and the EPDM rubber film layer has the risk of partially not being vulcanized during the vulcanization process. When its thickness is greater than 70%, the stress retention rate of the composite film is low and the resilience performance requirements of the diaphragm cannot be met.
[0069] Optionally, the glass transition temperature of the EPDM rubber film layer is -30°C to -60°C, for example, -30°C, -40°C, -45°C, -50°C, -60°C, etc. Having a lower glass transition temperature can ensure that the prepared diaphragm can be used for a long time in a low temperature environment without the diaphragm being broken due to vibration stretching.
[0070] Optionally, the room temperature storage modulus of the composite film is 2MPa to 50MPa, for example, 2MPa, 5MPa, 10MPa, 15MPa, 20MPa, 30MPa, 40MPa, 50MPa, etc. Optionally, the room temperature storage modulus of the composite film is 5MPa to 30MPa. The room temperature storage modulus is proportional to the f0 (lowest resonance frequency) of the diaphragm. The larger the room temperature storage modulus, the larger the f0, which will lead to a decrease in the loudness of the sound-generating device and a deterioration in the low-frequency performance. A lower room temperature storage modulus is conducive to providing good low-frequency performance.
[0071] Optionally, the density of the composite film is 1.1 g / cm 3 ~1.5g / cm 3 , for example, 1.1 g / cm 3 , 1.2g / cm3 , 1.3g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 Etc. By controlling the density of the composite film within a suitable range, it is possible to ensure that the mass of the prepared diaphragm is small enough and that the acoustic mid-frequency performance of the micro-speaker meets the requirements.
[0072] Optionally, the stress retention rate of the composite membrane during stress relaxation is greater than or equal to 55%, for example, 55%, 58%, 60%, 65%, 70%, etc. The stress retention rate refers to the ratio of the minimum stress value to the maximum stress value. When the micro speaker is under high water pressure, the diaphragm is stretched and deformed. After a period of pressure, the molecular chain of the diaphragm causes stress loss due to internal friction. If the stress loss is too large, the diaphragm cannot rebound when the external force is withdrawn, causing the diaphragm to deviate from the equilibrium position and the sound quality to decrease. It can be understood that since the diaphragm is composited with a hydrogenated nitrile rubber mold layer and an EPDM rubber membrane layer, the EPDM rubber membrane layer has good resilience. By controlling the stress retention rate of the composite membrane during stress relaxation to be greater than or equal to 55%, it can be ensured that the diaphragm has good resilience, thereby ensuring that the sound-generating device can work normally under high water pressure and meet actual use requirements.
[0073] In this embodiment, the diaphragm is a composite film formed by air pressure, and the composite film includes a stacked hydrogenated nitrile rubber film layer and an EPDM rubber film layer; when the EPDM rubber film layer is located on the outer layer of the composite film, the EPDM rubber film layer is fitted to a molding mold and subjected to air pressure forming to obtain the composite film, and the hydrogenated nitrile rubber film layer contains carboxyl groups. A composite film is formed by compounding a hydrogenated nitrile rubber film layer containing a carboxyl group and an EPDM rubber film layer. During air pressure molding, the EPDM rubber film layer is fitted with a molding mold, that is, the EPDM rubber film layer is located between the hydrogenated nitrile rubber film layer and the molding mold. The hydrogenated nitrile rubber film layer can isolate oxygen and provide an oxygen-free environment for the vulcanization of the EPDM rubber. The hydrogenated nitrile rubber contains carboxyl groups and can be cross-linked in an air environment to form a hydrogenated nitrile rubber film layer with good damping performance. Therefore, the composite film can have good damping and rebound properties and can meet the acoustic performance requirements. In addition, since air pressure molding is used instead of compression molding, the production cost is reduced, thereby solving the problem of excessively high cost of EPDM rubber in acoustic products.
[0074] The present invention also discloses a sound generating device, referring to Figure 4 , the sound generating device 100 includes the diaphragm 120 as described above.
[0075] In this embodiment, the sound-generating device 100 may be a speaker. For example, referring to Figure 4 , Figure 4 This is an example cross-sectional view of a sound-generating device 100 in an embodiment of the present invention, wherein the sound-generating device 100 includes a housing 110, a vibration system disposed in the housing 110, and a magnetic circuit system 140 coordinated with the vibration system, the vibration system includes a diaphragm 120 and a voice coil 130 coupled to one side of the diaphragm 120, and the magnetic field force of the magnetic circuit system 140 drives the voice coil 130 to vibrate so as to drive the diaphragm 120 to make a sound. When the sound-generating device 100 is working, an electrical signal is input into the voice coil 130, and the voice coil 130 is driven by the magnetic field force of the magnetic circuit system 140, and moves with different amplitudes and directions as the signal size and the positive and negative directions change alternately, thereby driving the diaphragm 120 to vibrate and make a sound, so as to complete the process of converting electrical energy-mechanical energy-acoustic energy.
[0076] Optionally, refer to Figure 5 In a specific embodiment of the present invention, the diaphragm 120 may include a first diaphragm 121 and a second diaphragm 122, the sound-generating device includes a magnetic circuit system 140 and a vibration system; the vibration system includes a voice coil 130, a first diaphragm 121 and a second diaphragm 122; the first diaphragm 121 and the second diaphragm 122 are respectively arranged at the axial ends of the voice coil 130, one end of the voice coil 130 drives the first diaphragm 121 to vibrate and produce sound, and the other end of the voice coil 130 is connected to one end of the second diaphragm 122 to balance the vibration of the voice coil 130, and the first diaphragm 121 and / or the second diaphragm 122 are the diaphragms as described above.
[0077] The sound-generating device provided by the present invention solves the technical problem of the high cost of the existing EPDM rubber in acoustic products. Compared with the prior art, the beneficial effects of the sound-generating device provided by the embodiment of the present invention are the same as the beneficial effects of the diaphragm in the above embodiment, which will not be described in detail here.
[0078] Furthermore, the present invention also discloses an electronic device, which includes the above sound-generating device.
[0079] In this embodiment, the electronic devices include mobile phones, laptop computers, tablet computers, VR (Virtual Reality) devices, AR (Augmented Reality) devices, TWS (True Wireless Stereo) headphones, smart speakers, smart wearable devices, etc.
[0080] The electronic device provided by the present invention solves the technical problem of high cost of using EPDM in acoustic products. Compared with the prior art, the beneficial effects of the electronic device provided by the embodiment of the present invention are the same as those of the sound-generating device in the above embodiment, which will not be described in detail here.
[0081] The diaphragm of the present invention is described in detail below with specific embodiments and comparative examples. It is worth noting that the following description is only exemplary and not a specific limitation of the present invention.
[0082] Example 1
[0083] The thickness of the diaphragm is 90 μm, and it includes a hydrogenated nitrile rubber film layer and an EPDM rubber film layer, wherein the thickness of the hydrogenated nitrile rubber film layer is 35 μm, and the thickness of the EPDM rubber film layer is 55 μm. The amount of the reinforcing agent silicon dioxide is 40 wt%, and the curing is performed at 200° C. for 150 seconds.
[0084] Test results: The room temperature storage modulus of the diaphragm is 16.3MPa, the elongation at break is 279.2%, the stress retention rate is 63.1%, and the glass transition temperature of the EPDM rubber membrane layer is -37°C; and it can be formed by air pressure without the problem of the EPDM membrane layer being unable to vulcanize and cross-link.
[0085] Comparative Example 1
[0086] When preparing a single-layer EPDM rubber membrane layer with a thickness of 90 μm, due to the problem of oxygen hindering polymerization, a cross-linking reaction cannot occur during air vulcanization, and a diaphragm product cannot be produced.
[0087] Comparative Example 2
[0088] A hydrogenated nitrile rubber film with a single layer thickness of 90 μm was prepared, the amount of reinforcing agent silicon dioxide was 40 wt%, and the film was vulcanized at 200° C. for 150 s.
[0089] Test results: The room temperature storage modulus is 16.1 MPa, the elongation at break is 178.3%, and the stress retention rate is 50.3%.
[0090] It can be seen from the above Example 1 and Comparative Examples 1-2 that, under the condition of consistent thickness, the solution of Example 1 has higher elongation at break and stress retention rate, which can enable the product to maintain better sound quality after high-level waterproofing.
[0091] Room temperature storage modulus test method: according to ASTM D882 standard, heating rate 3℃ / min, strain 0.2%, tensile mode.
[0092] Elongation at break and tensile strength test method: according to ASTM D882 standard, tensile rate 300mm / min, gauge length 30mm, temperature: 23±2℃; humidity: 50±10%RH.
[0093] Glass transition temperature test method: according to ASTM D882 standard, heating rate 3℃ / min, strain 0.2%, tensile mode, select the temperature corresponding to the loss factor peak as the glass transition temperature.
[0094] Stress retention rate test method: According to ASTM D5026-15 standard, keep warm at 23℃ for 5 minutes, instantly stretch the strain to 10%, relax for 10 minutes, recover for 5 minutes, and take the maximum and minimum stress values on the curve.
[0095] The serial numbers of the above embodiments of the present invention are for description only and do not represent the advantages or disadvantages of the embodiments.
[0096] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A diaphragm, characterized in that: The diaphragm is a composite membrane formed by air pressure, and the composite membrane comprises a hydrogenated nitrile rubber membrane layer and an EPDM rubber membrane layer stacked in layers; When the EPDM rubber film layer is located on the outer layer of the composite film, the EPDM rubber film layer is attached to a molding die and subjected to air pressure molding to obtain the composite film; The main component of the hydrogenated nitrile rubber in the hydrogenated nitrile rubber film layer is shown in the following formula (I): Wherein, x, y, z, m, and n represent the number of each group respectively, x, y, and z are natural numbers and are not zero at the same time, and m and n are positive integers; The original polymerizable monomer of R is an ethylenically unsaturated monocarboxylic acid or an ethylenically unsaturated dicarboxylic acid.
2. The diaphragm according to claim 1, characterized in that The ethylenically unsaturated monocarboxylic acid includes acrylic acid, methacrylic acid, ethacrylic acid, crotonic acid or cinnamic acid; And / or, the ethylenically unsaturated dicarboxylic acid comprises fumaric acid, maleic acid, glutaconic acid, allylmalonic acid, mesaconic acid, tolconic acid, itaconic acid or taconic acid.
3. The diaphragm according to claim 1, characterized in that: The mass content of the carboxylic acid groups in the hydrogenated nitrile rubber film layer is 0.5wt% to 5wt%.
4. The diaphragm according to claim 1, characterized in that The composite film also includes at least one of a reinforcing agent, an antioxidant, a dye, a plasticizer, an anti-ultraviolet additive, an antistatic agent, a cross-linking agent, a vulcanizing agent and a vulcanization accelerator.
5. The diaphragm according to claim 4, characterized in that: The reinforcing agent comprises at least one of talc, silicon dioxide and carbon black, and the weight proportion of the reinforcing agent in the composite film is 20wt% to 65wt%; And / or, the antioxidant includes at least one of antioxidant N-445, antioxidant 246, antioxidant 4010, antioxidant SP, antioxidant RD, antioxidant ODA, antioxidant OD and antioxidant WH-02, and the antioxidant is added in an amount of 0.5-10 parts by mass; And / or, the cross-linking agent includes at least one of hexamethylenediamine, hexamethylenediamine salt, hexamethylenediamine carbamate, triethylenetetramine, 2,2'-methylenedianiline and di-o-tolylguanidine.
6. The diaphragm according to claim 1, characterized in that: The total thickness of the composite film is 20 μm to 120 μm; And / or, the thickness of the hydrogenated nitrile rubber film layer accounts for 20% to 70% of the total thickness of the composite film.
7. The diaphragm according to claim 1, characterized in that: The glass transition temperature of the EPDM rubber film layer is -30°C to -60°C; And / or, the room temperature storage modulus of the composite film is 2 MPa to 50 MPa.
8. The diaphragm according to claim 1, characterized in that: The density of the composite film is 1.1 g / cm 3 ~1.5g / cm 3 ; And / or, the stress retention rate of the composite film during stress relaxation is greater than or equal to 55%.
9. The diaphragm according to claim 1, characterized in that: The composite film is formed into a double-layer composite structure, and the composite film includes a layer of the hydrogenated nitrile rubber film layer and a layer of the EPDM rubber film layer; Alternatively, the composite film is formed into a three-layer composite structure, the composite film includes two layers of the hydrogenated nitrile rubber film layers and one layer of the EPDM rubber film layer, and the two layers of the hydrogenated nitrile rubber film layers are arranged on opposite sides of the EPDM rubber film layer.
10. A sound-generating device, characterized in that: The sound generating device comprises the diaphragm according to any one of claims 1 to 9.
11. The sound generating device according to claim 10, characterized in that: The sound-generating device includes a magnetic circuit system and a vibration system; the vibration system includes a voice coil, a first diaphragm and a second diaphragm; the first diaphragm and the second diaphragm are respectively arranged at the two axial ends of the voice coil, one end of the voice coil drives the first diaphragm to vibrate and produce sound, and the other end of the voice coil is connected to one end of the second diaphragm to balance the vibration of the voice coil, and the first diaphragm and / or the second diaphragm is the diaphragm as described in any one of claims 1 to 9.
12. An electronic device, characterized in that: The electronic device comprises the sound generating device according to claim 10 or 11.