Poly (aspartic acid) cross-linking body and production method thereof
Through the reaction of polysuccinimide and specific compounds, a poly(aspartic acid) cross-linked body lacking ester bonds is formed, which solves the problem of shape failure of water-absorbent resin after hydrolysis and achieves high water absorption and biodegradability. Simplified processing.
Patent Information
- Application Number
- CN202280090615.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-16
- Filing Date
- 2022-11-24
- Publication Date
- 2024-10-08
AI Technical Summary
Existing water-absorbent resins lose their gel shape after hydrolysis, and the use of polar aprotic solvents requires complex processing and recycling facilities, making it difficult to achieve biodegradability and efficient water absorption.
By reacting polysuccinimide with compounds containing specific functional groups and multifunctional epoxy compounds, a poly(aspartic acid) cross-linked body lacking ester bonds is formed, which maintains the gel shape and is stable in water, using water or aqueous solvents Carry out the reaction and avoid hydrolysis.
It achieves high water absorption and water retention of poly(aspartic acid) cross-linked body, avoids shape failure caused by hydrolysis of ester bonds, simplifies the processing process, and is suitable for biodegradable materials.
Smart Images

Figure BDA0004971305760000031 
Figure BDA0004971305760000032 
Figure BDA0004971305760000041
Abstract
Description
Technical Field
[0001] The present invention relates to a cross-linked poly (aspartic acid) product and a production method thereof.
[0002] This application claims the benefit of PCT Application No. PCT / CN2022 / 076421 filed on February 16, 2022, which is hereby incorporated by reference in its entirety. Background Art
[0003] Water-absorbent resins are resins that can absorb water several tens to several thousands of times their own weight, and are used in a wide range of fields, such as sanitary products, disposable diapers, and medical products such as poultices. Typical examples thereof include acrylic water-absorbent resins, but they are not biodegradable, so disposal (incineration or dumping) after use has become a problem. For this reason, there is a strong need for novel water-absorbent resins with biodegradability.
[0004] For example, a method for producing a cross-linked poly(amino acid) by reacting the poly(amino acid) with a polyepoxide as a cross-linking agent has been disclosed (eg, Patent Document 1).
[0005] There has been disclosed a method for producing a polymer having a poly(aspartic acid) backbone whose chains are partially cross-linked by a diamine using the diamine as a cross-linking agent (for example, Patent Document 2).
[0006] [Prior art literature]
[0007] [Patent Document]
[0008] [Patent Document 1]
[0009] Japanese Unexamined Patent Application Publication No. 2000-63511
[0010] [Patent Document 2]
[0011] Japanese Unexamined Patent Application Publication No.2019-89898 Summary of the invention
[0012] Problem that the invention aims to solve
[0013] However, in the method described in Patent Document 1, the crosslinked portion has an ester bond. These ester bonds are hydrolyzed over time, thereby disadvantageously causing failure to maintain the gel shape.
[0014] In the method described in Patent Document 2, a polar aprotic solvent is used. This requires facilities for treating the organic solvent and recovering the organic solvent.
[0015] The present invention provides a poly(aspartic acid) crosslinker that can maintain gel shape, water absorption, and water retention because it does not undergo hydrolysis over time due to the lack of ester bonds, and a method for producing the poly(aspartic acid) crosslinker.
[0016] Solutions for solving problems
[0017] The present invention includes the following aspects.
[0018] [1] The poly(aspartic acid) crosslinker is a reaction product of polysuccinimide (PSI), a compound (A: a1-A1-a2) containing a first functional group (a1) and a second functional group (a2), and a multifunctional epoxy compound (B), wherein the poly(aspartic acid) crosslinker comprises a PSI-a1(A) bond formed by an addition reaction of the first functional group (a1) and the polysuccinimide (PSI), and the poly(aspartic acid) crosslinker comprises a PSI-a1(A) bond formed by an addition reaction of the second functional group (a2). The poly(aspartic acid) crosslinker comprises a crosslinked structure (PABAP) represented by PSI-a1-A1-a2-B-a2-A1-a1-PSI, the crosslinked structure (PABAP) is partially hydrolyzed, and the second functional group of the compound (A) does not react with polysuccinimide (PSI) or has a lower reactivity with polysuccinimide (PSI) than the first functional group.
[0019] [2] In the crosslinked poly(aspartic acid) described in [1], the first functional group (a1) is an amino group (NH 2 -), the second functional group (a2) is selected from amino (NH 2 -) and phosphonooxy ((OH) 2 P(=O)-O-), and when the second functional group (a2) is an amino group (NH 2 -), the reactivity of the second functional group with polysuccinimide (PSI) is lower than that of the first functional group (a1).
[0020] [3] In the crosslinked poly(aspartic acid) described in [1] or [2], the first functional group (a1) is an amino group (NH 2 -), the second functional group (a2) is an amino group (NH 2 -), and in the compound (A), the amino group of the second functional group (a2) is an amino group in the structure represented by formula (1).
[0021] [Chemical formula 1]
[0022]
[0023] In formula (1), G is a carboxylic acid group or a salt thereof.
[0024] [4] In the crosslinked poly(aspartic acid) according to any one of [1] to [3], compound (A) is at least one selected from the group consisting of lysine, ornithine, and arginine.
[0025] [5] A water-absorbing composition comprising the crosslinked poly(aspartic acid) according to any one of [1] to [4].
[0026] [6] A thickening composition comprising the crosslinked poly(aspartic acid) according to any one of [1] to [4].
[0027] [7] A method for producing a poly(aspartic acid) crosslinker, the method comprising the following steps: forming a crosslinker by reacting polysuccinimide (PSI) with a compound (A: a1-A1-a2) containing a first functional group (a1) and a second functional group (a2) and a multifunctional epoxy compound (B) in water or an aqueous solvent, wherein the second functional group of the compound (A) does not react with polysuccinimide (PSI) or has a lower reactivity with polysuccinimide (PSI) than the first functional group.
[0028] [8] In the method for producing a crosslinked poly(aspartic acid) described in [7], the first functional group (a1) is an amino group (NH 2 -), the second functional group (a2) is selected from amino (NH 2 -) and phosphonooxy ((OH) 2 P(=O)-O-), and when the second functional group (a2) is an amino group (NH 2 -), the reactivity of the second functional group with polysuccinimide (PSI) is lower than that of the first functional group (a1).
[0029] [9] In the method for producing a crosslinked poly(aspartic acid) described in [7] or [8], the first functional group (a1) is an amino group (NH 2 -), the second functional group (a2) is an amino group (NH 2 -), and in compound (A), the amino group of the first functional group (a1) is NH 2 -CH 2 -, and the amino group of the second functional group (a2) is the amino group in the structure represented by formula (1).
[0030] [Chemical formula 2]
[0031]
[0032] In formula (1), G is a carboxylic acid group or a salt thereof.
[0033]
[10] The method for producing a crosslinked poly(aspartic acid) according to any one of [7] to [9], wherein the compound (A) is one or more selected from the group consisting of lysine, ornithine, and arginine.
[0034] Effects of the Invention
[0035] The present invention can provide a poly(aspartic acid) crosslinker that can maintain its gel shape as well as its water absorption and water retention properties because it does not undergo hydrolysis over time due to the lack of ester bonds. DETAILED DESCRIPTION
[0036] [Poly(aspartic acid) cross-linked]
[0037] The poly(aspartic acid) crosslinker according to an embodiment of the present invention (hereinafter, also referred to as "the crosslinker according to the present embodiment") is a reaction product of polysuccinimide (PSI), a compound (A: a1-A1-a2) containing a first functional group (a1) and a second functional group (a2), and a multifunctional epoxy compound (B). The crosslinker contains a PSI-a1(A) bond formed by an addition reaction of the first functional group (a1) with the polysuccinimide (PSI). The crosslinker contains a B-a2(A) bond formed by a reaction of the second functional group (a2) with the multifunctional epoxy compound (B). The crosslinker contains a crosslinked structure (PABAP) represented by PSI-a1-A1-a2-B-a2-A1-a1-PSI. A portion of the crosslinked structure (PABAP) (e.g., an unreacted PSI portion) is hydrolyzed. The second functional group of the compound (A) does not react with polysuccinimide (PSI) or has a lower reactivity with polysuccinimide (PSI) than the first functional group.
[0038] [Polysuccinimide (PSI)]
[0039] The polysuccinimide (PSI) according to the present embodiment is a polymer represented by the following formula (2).
[0040] [Chemical formula 3]
[0041]
[0042] In this formula, n=10 to 10,000.
[0043] The method for producing polysuccinimide (PSI) is not limited to a specific method. For example, polysuccinimide (PSI) is produced by heating aspartic acid to 170°C to 190°C by a condensation reaction in the presence of phosphoric acid in a vacuum. In order to obtain polysuccinimide with a higher molecular weight, the polysuccinimide produced as described above can be treated with a condensing agent such as dicyclohexylcarbodiimide. The molecular weight of polysuccinimide is not limited to a specific value. For example, polysuccinimide preferably has a weight average molecular weight of more than 20,000, more preferably more than 50,000, and even more preferably more than 70,000. Polysuccinimide preferably has a molecular weight of less than 500,000, more preferably less than 200,000. In this case, the weight average molecular weight is a value determined by gel permeation chromatography (GPC) based on polystyrene standards.
[0044] [Compound (A)]
[0045] The first functional group (a1) of the compound (A) according to this embodiment is preferably an amino group (NH 2 The amino group of the first functional group (a1) is more preferably NH 2 -CH 2 -Amino group in.
[0046] The second functional group (a2) of the compound (A) according to this embodiment is preferably an amino group (NH 2 -) or phosphonooxy ((OH) 2 The second functional group (a2) is more preferably an amino group (NH 2 -). When the second functional group (a2) is an amino group (NH 2 -), the amino group of the second functional group (a2) is even more preferably an amino group in a structure represented by the following formula (1).
[0047] [Chemical formula 4]
[0048]
[0049] In formula (1), G is a carboxylic acid group or a salt thereof.
[0050] When G is a salt of a carboxylic acid group, examples of the salt include alkali metal salts such as sodium salts and potassium salts; alkaline earth metal salts such as calcium salts and magnesium salts; organic base salts such as amine salts; and basic amino acid salts such as lysine salts and arginine salts. Among them, alkali metal salts are preferred, and sodium salts and potassium salts are more preferred.
[0051] In which the first functional group (a1) of the compound (A) according to this embodiment is an amino group (NH 2 -) and wherein the second functional group (a2) of the compound (A) according to this embodiment is also an amino group (NH2 -), the amino group of the second functional group of the compound (A) is preferably less reactive with polysuccinimide (PSI) than the amino group of the first functional group. In other words, examples of the compound (A) include diamines each having a different terminal structure containing such an amino group. Examples thereof include asymmetric diamines.
[0052] Wherein the first functional group (a1) of the compound (A) according to this embodiment is NH 2 -CH 2 - and wherein the amino group of the second functional group (a2) is the amino group in the structure represented by the above-mentioned formula (1), an example of the compound (A) is a compound represented by the following formula (3).
[0053] [Chemical formula 5]
[0054]
[0055] In the formula, n=1-10, preferably 2-8, more preferably 3-5.
[0056] The compound (A) according to the present embodiment may be a salt of a carboxylic acid group of a compound represented by the above formula (3). In this case, examples of the salt include alkali metal salts such as sodium salts and potassium salts; alkaline earth metal salts such as calcium salts and magnesium salts; organic base salts such as amine salts; and basic amino acid salts such as lysine salts and arginine salts. Among them, alkali metal salts are preferred, and sodium salts and potassium salts are more preferred.
[0057] In the case where the first functional group (a1) of the compound (A) according to this embodiment is an amino group and where the second functional group (a2) is also an amino group, where the first functional group (a1) is NH 2 -CH 2 An example of the compound (A) in which the amino group in the second functional group (a2) is an amino group in the structure represented by the above-mentioned formula (1) is a compound represented by the following formula (4).
[0058] [Chemical formula 6]
[0059]
[0060] In the formula, L is a divalent linking group, preferably one or more divalent linking groups, such as -CH 2 - and C=O, more preferably -CH 2 -, and n is an integer of 1 to 10, preferably an integer of 2 to 8, more preferably an integer of 3 to 5.
[0061] The compound (A) according to the present embodiment may be a salt of a carboxylic acid group of a compound represented by the above formula (4). In this case, examples of the salt include alkali metal salts such as sodium salts and potassium salts; alkaline earth metal salts such as calcium salts and magnesium salts; organic base salts such as amine salts; and basic amino acid salts such as lysine salts and arginine salts. Among them, alkali metal salts are preferred, and sodium salts and potassium salts are more preferred.
[0062] In the case where the first functional group (a1) of the compound (A) according to this embodiment is an amino group and the second functional group (a2) is a phosphonooxy group ((OH) 2 In the case of a P(=O)-O-) group, an example of the compound (A) is a compound represented by the following formula (5).
[0063] [Chemical formula 7]
[0064]
[0065] In the formula, L is a divalent linking group, preferably one or more divalent linking groups, such as -CH 2 - and C=O, more preferably -CH 2 -, and n is an integer of 1 to 10, preferably an integer of 2 to 8, more preferably an integer of 3 to 5.
[0066] The compound (A) according to the present embodiment may be a salt of a phosphonooxy group of a compound represented by the above formula (5). In this case, examples of the salt include alkali metal salts such as sodium salts and potassium salts; alkaline earth metal salts such as calcium salts and magnesium salts; organic base salts such as amine salts; and basic amino acid salts such as lysine salts and arginine salts. Among them, alkali metal salts are preferred, and sodium salts and potassium salts are more preferred.
[0067] Examples of the compound (A) according to the present embodiment include lysine, ornithine, and arginine.
[0068] When the compound (A) according to the present embodiment contains an amino group, an acidic salt of the compound (A) may be used as a raw material. Examples of the acidic salt of the compound (A) include hydrochlorides such as lysine hydrochloride, ornithine hydrochloride, and arginine hydrochloride, and similar sulfates.
[0069] As compound (A) according to the present embodiment, dipeptides can be used. Examples of dipeptides include dipeptides each having a basic amino acid residue at the C-terminus, such as glycine-lysine (isopeptide bond), alanine-lysine (isopeptide bond), glycine-ornithine (isopeptide bond) and alanine-ornithine (isopeptide bond); and dipeptides each having a basic amino acid residue at the N-terminus, such as lysine-glycine, lysine-alanine, ornithine-glycine and ornithine-alanine.
[0070] For example, glycine-lysine is a dipeptide represented by the following formula (6), and lysine-glycine is a dipeptide represented by the following formula (7).
[0071] [Chemical formula 8]
[0072]
[0073] [Multifunctional Epoxy Compound (B)]
[0074] Examples of the polyfunctional epoxy compound according to the present embodiment include polyglycidyl ethers of (C2-C6) alkane polyols and poly(alkylene glycols), such as ethylene glycol diglycidyl ether, diethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, diglycerol polyglycidyl ether, polyglycerol polyglycidyl ether, propylene glycol diglycidyl ether, and butanediol diglycidyl ether; (C4-C8) diepoxyalkylenes and diepoxyalkylenes, such as sorbitol polyglycidyl ether, pentaerythritol polyglycidyl ethers, erythritol polyglycidyl ether, trimethylolethane polyglycidyl ether, trimethylolpropane polyglycidyl ether, 1,2,3,4-diepoxybutane, 1,2,4,5-diepoxypentane, 1,2,5,6-diepoxyhexane, 1,2,7,8-diepoxyoctane, 1,4- and 1,3-divinylbenzene epoxides; and (C6-C15) polyphenol polyglycidyl ethers, such as 4,4'-isopropylidene diphenol diglycidyl ether (also known as bisphenol A diglycidyl ether) and hydroquinone diglycidyl ether.
[0075] Further examples thereof include multifunctional epoxy compounds available from Nagase ChemteX Corporation, such as EX-810, EX-861, EX-313, EX-614B, and EX-512.
[0076] [Method for producing a crosslinked poly(aspartic acid)]
[0077] The method for producing a poly(aspartic acid) crosslinker according to the present embodiment (hereinafter, also referred to as "the production method according to the present embodiment") includes a step of forming a crosslinker by reacting polysuccinimide (PSI) with a compound (A: a1-A1-a2) containing a first functional group (a1) and a second functional group (a2) and a polyfunctional epoxy compound (B) in water or an aqueous solvent. The polysuccinimide (PSI), the compound (A) containing a first functional group (a1) and a second functional group (a2), and the polyfunctional epoxy compound (B) are the same as those described in the poly(aspartic acid) crosslinker according to the present embodiment. Preferred examples thereof are also the same.
[0078] In the production method according to the present embodiment, the order of reaction of polysuccinimide (PSI), compound (A), and polyfunctional epoxy compound (B) is not limited to any specific order. Examples thereof include the following three production methods.
[0079] (i) A production method comprising the steps of reacting polysuccinimide (PSI) with a compound (A) to obtain a reaction product (P1) of polysuccinimide (PSI) and the compound (A), and reacting the reaction product (P1) obtained in the above steps with a polyfunctional epoxy compound (hereinafter, referred to as "method (i)").
[0080] (ii) A production method in which polysuccinimide (PSI) and compound (A) are first mixed, and then a polyfunctional epoxy compound is added thereto at a constant rate while allowing the reaction to proceed (hereinafter, referred to as "method (ii)").
[0081] (iii) A production method in which polysuccinimide (PSI), the compound (A), and a polyfunctional epoxy compound are mixed together and then reacted (hereinafter, referred to as "method (iii)").
[0082] From the viewpoint of easy control of the structure of the resulting poly(aspartic acid) crosslinked product, method (i) or method (ii) is preferred. Method (i) is more preferred.
[0083] The production method according to the present embodiment will be described in detail taking the above-mentioned method (i) as an example.
[0084] In the step of producing the reaction product (P1) in method (i), compound (A) is first preferably dissolved in water. For example, water is preferably used in an amount of 5 to 50 parts by mass, more preferably 7 to 15 parts by mass, based on 1 part by mass of compound (A). The aqueous solution is mixed with polysuccinimide. Regarding the mixing ratio, compound (A) is preferably used in an amount of 0.5 to 10 parts by mass, more preferably 1 to 5 parts by mass, and even more preferably 1.5 to 3 parts by mass, based on 10 parts by mass of polysuccinimide.
[0085] In the mixture after the feed, an organic or inorganic base compound such as NaOH or amine is added to adjust the pH of the aqueous solution to preferably 8 to 13, more preferably 9 to 12. In the obtained product, the percentage of the unit of the added compound (A) is preferably 2% to 30%, more preferably 5% to 15%, and even more preferably 8% to 12% of the total units. The percentage of the unit of the added compound (A) can be determined by the -CH 2 The integral value of the peak of the proton of -Ib is the same as that of -CH 2Alternatively, the percentage of the unit added by compound (A) can be determined by the ratio of twice the value of the integrated value Ic of the peak derived from the protons of -CH- in compound (A) to the integrated value Ia (Ic×2 / Ia).
[0086] In the step of reacting the reaction product (P1) with a polyfunctional epoxy compound in method (i), the feed amount of the polyfunctional epoxy compound is preferably 2 to 10 parts by mass, more preferably 3 to 8 parts by mass, based on 100 parts by mass of the reaction product (P1).
[0087] As the reaction product (P1), a solid form of the reaction product (P1) obtained by separating the reaction product (P1) from the reaction solution prepared in the step of forming the reaction product (P1) can be used. In this case, it is preferred to prepare an aqueous solution of the reaction product (P1) in advance before adding the polyfunctional epoxy compound.
[0088] As the reaction product (P1), the polyfunctional epoxy compound may be added to the reaction solution without isolating the reaction product (P1) from the reaction solution prepared in the step of forming the reaction product (P1).
[0089] The temperature of the reaction between the reaction product (P1) and the polyfunctional epoxy compound may be 30 to 100° C., and preferably 40 to 80° C., more preferably 50 to 70° C. At 60° C., the reaction time may be, for example, 40 to 600 minutes, and preferably 60 to 300 minutes.
[0090] In order to isolate the poly(aspartic acid) crosslinked body formed by the reaction, generally known and customary separation operations such as recrystallization, reprecipitation, filtration, and concentration can be used.
[0091] For example, for thickening composition applications, the size (average particle size) of the poly(aspartic acid) crosslinker is preferably, but not necessarily, 150 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less. For example, in the application of "water-absorbent compositions" for diapers and sanitary products, the size is preferably in the range of 1 to 5,000 μm, more preferably in the range of 10 to 1,000 μm, and even more preferably in the range of 100 to 800 μm.
[0092] [Degree of cross-linking]
[0093] The amount of the compound (A) and the polyfunctional epoxy compound (B) used relative to the polysuccinimide (PSI) according to the present embodiment can be appropriately selected according to the desired degree of crosslinking. For example, in the case of the production method using the above method (i), the degree of crosslinking can be controlled by adjusting the mixing ratio of the polysuccinimide (PSI) and the compound (A) within the above range and also by adjusting the polyfunctional epoxy compound (B). The percentage (percentage added) of the unit of the added compound (A) depends on the application of the poly (aspartic acid) crosslinker finally formed. For example, in applications requiring high levels of water absorption and water retention, the percentage (percentage added) of the unit of the added compound (A) is preferably 1% to 20% of the total units in the polysuccinimide (PSI), more preferably 3% to 15%, and even more preferably 5% to 10%. The percentage added can be measured by NMR.
[0094] [Application of poly(aspartic acid) crosslinkers]
[0095] The crosslinked poly(aspartic acid) according to the present embodiment can be used as a water-absorbent composition contained in an absorbent material of an absorbent article such as a diaper or sanitary product. When the crosslinked poly(aspartic acid) according to the present embodiment is used as the water-absorbent composition, the size (average particle diameter) is preferably 1 to 5,000 μm, more preferably 10 to 1,000 μm, and even more preferably 100 to 800 μm.
[0096] The crosslinked poly(aspartic acid) according to the present embodiment can also be used as a thickening composition. When the crosslinked poly(aspartic acid) according to the present embodiment is used as the thickening composition, the size (average particle size) is preferably 150 μm or less, more preferably 100 μm or less, and even more preferably 80 μm or less.
[0097] [Water-absorbent resin]
[0098] The water-absorbent resin according to one embodiment of the present invention (this embodiment) contains the poly(aspartic acid) crosslinked body according to this embodiment. The water-absorbent resin according to this embodiment may contain, for example, another resin or another known additive in addition to the poly(aspartic acid) crosslinked body according to this embodiment as needed.
[0099] When the poly (aspartic acid) crosslinked body according to the present embodiment is a hydrogel-like crosslinked body, the crosslinked body is dried as needed, and is usually crushed before or after drying to form a water-absorbent resin. The drying method is not limited to a specific method, and can be freely selected from known methods, such as heating drying, freeze drying, reduced pressure drying (in a vacuum), and reduced pressure heating drying. The drying method can change the particle shape, so it is selected according to the purpose. In the case of heating drying, the drying temperature is usually in the range of 60°C to 250°C, preferably in the range of 80°C to 220°C, and more preferably in the range of 100°C to 200°C. In the case of reduced pressure heating drying, the drying temperature is usually in the range of 50°C to 200°C, preferably in the range of 60°C to 150°C, and more preferably in the range of 70°C to 120°C. The drying time varies according to the surface area and water content of the hydrogel-like crosslinked body and the type of dryer, and the drying time is selected so as to achieve the desired water content. It is difficult to reduce the water content of the water-absorbent resin to zero. Therefore, when a water-absorbent resin containing a small amount of water (e.g., 0.3 to 15 wt %, or even 0.5 to 10 wt %) can be handled as a powder, the water-absorbent resin containing such a small amount of water is also referred to as a water-absorbent resin in this specification.
[0100] The water-absorbent resin according to the present embodiment preferably has a poly(aspartic acid) crosslinked body content of 50 to 100% by mass, more preferably 70 to 100% by mass, and even more preferably 90 to 100% by mass. The water-absorbent resin according to the present embodiment may be a poly(aspartic acid) crosslinked body according to the present embodiment.
[0101] [Water-absorbent resin particles]
[0102] The water-absorbent resin particles according to one embodiment (the present embodiment) of the present invention include the water-absorbent resin according to the present embodiment.
[0103] Examples of the shape of the water-absorbent resin particles according to the present embodiment include a substantially spherical shape, a crushed shape, and a particle shape. The size (average particle size) of the water-absorbent resin particles according to the present embodiment is preferably 1 μm to 5,000 μm, more preferably 10 μm to 1,000 μm, and even more preferably 100 μm to 800 μm. The particle size distribution of the water-absorbent resin particles can be adjusted by performing operations such as particle size adjustment using sieve classification.
[0104] In the water-absorbent resin particles according to the present embodiment, a crosslinking agent can be used to crosslink the surface portion of the hydrogel-like crosslinked body (surface crosslinking). Surface crosslinking promotes the control of the water absorption characteristics of the water-absorbent resin particles. Surface crosslinking is preferably performed when the hydrogel-like crosslinked body has a specific water content.
[0105] An example of a crosslinking agent for surface crosslinking (surface crosslinking agent) is a crosslinking agent for the production of a poly(aspartic acid) crosslinker according to the present embodiment. Other compounds each having two or more reactive functional groups may also be exemplified. The crosslinking agent may be used alone or in combination of two or more.
[0106] After the surface cross-linking, water or an aqueous solvent is evaporated by a known method to provide cross-linked body particles as a dry product having a cross-linked surface.
[0107] The water-absorbent resin particles according to the present embodiment can be composed only of crosslinked particles, and can further include various additional components selected from, for example, gel stabilizers, metal chelators, and fluidity improvers (lubricants). Additional components can be arranged inside the crosslinked particles, on the surface of the crosslinked particles, or both. As additional components, fluidity improvers (lubricants) are preferred. Among them, inorganic particles are more preferred. The example of the material of inorganic particles includes silicon dioxide particles, such as amorphous silica, talc, and mica.
[0108] The water-absorbent resin particles may include a plurality of inorganic particles disposed on the surface of the crosslinked particles. For example, the inorganic particles may be arranged on the surface of the crosslinked particles by mixing the crosslinked particles with the inorganic particles. The inorganic particles may be silica particles such as amorphous silica. When the water-absorbent resin particles include inorganic particles disposed on the surface of the crosslinked particles, based on the mass of the crosslinked particles, the ratio of the inorganic particles may be 0.2% by mass or more, 0.5% by mass or more, 1.0% by mass or more, or 1.5% by mass or more, and may be 5.0% by mass or less or 3.5% by mass or less. When the amount of the inorganic particles added is within the above range, it is easy to obtain water-absorbent resin particles with suitable water absorption properties.
[0109] [Absorbent materials]
[0110] The absorbent material according to one embodiment (the present embodiment) of the present invention includes water-absorbent resin particles and a fiber layer containing a fiber material. For example, the absorbent material is a mixture containing water-absorbent resin particles and a fiber material. Examples of the configuration of the absorbent material may include a uniform mixture of water-absorbent resin particles and a fiber material; a configuration in which water-absorbent resin particles are inserted between sheets or layers composed of a fiber material; and other configurations.
[0111] The proportion by mass of the water absorbent resin particles in the absorbent material according to the present embodiment may be 2 to 100 mass%, 10 to 90 mass%, or 10 to 80 mass%, based on the total amount of the water absorbent resin particles and the fiber material.
[0112] The shape of the absorbent material according to the present embodiment is not limited to a specific shape, and may be, for example, sheet-like, tubular, film-like, or fiber-like. The absorbent material (eg, sheet-like absorbent material) may have a thickness of, for example, 0.1 mm to 50 mm, or 0.3 mm to 30 mm.
[0113] The absorbent material according to the present embodiment contains the water-absorbent resin particles according to the present embodiment. In addition to the water-absorbent resin particles according to the present embodiment, the absorbent material according to the present embodiment may further contain other known water-absorbent resin particles. The absorbent material according to the present embodiment preferably contains only the water-absorbent resin particles according to the present embodiment as the water-absorbent resin particles.
[0114] From the viewpoint that sufficient liquid absorption performance is more easily obtained when the absorbent material is used in the absorbent article described below, the absorbent material according to the present embodiment preferably has a liquid absorption capacity of 50 g to 2,000 g per square meter of absorbent material (i.e., 50 g to 2,000 g / m 2 ), more preferably 100 g to 1,000 g / m 2 From the viewpoint of providing sufficient liquid absorption performance as an absorbent article and particularly inhibiting liquid leakage, the water-absorbent resin particle content is preferably 50 g / m 2 From the viewpoint of suppressing the gel blocking phenomenon, improving the liquid diffusion performance of the absorbent article, and improving the liquid permeation rate, the water-absorbent resin particle content is preferably 2,000 g / m 2 the following.
[0115] [Fiber materials]
[0116] Non-limiting examples of fiber materials include finely pulverized wood pulp; cotton; cotton linters; rayon; wool; acetate fibers; vinylon; cellulose fibers such as cellulose acetate; synthetic fibers such as polyamide, polyester, and polyolefin; and mixtures of these fibers. These fiber materials may be used alone or in combination of two or more. As the fiber material, hydrophilic fibers may be used.
[0117] From the viewpoint of obtaining sufficient liquid absorption performance even when the absorbent material is used in the absorbent article described below, the fiber material content is preferably 50 g to 800 g per square meter of the absorbent material (i.e., 50 g / m 2 Up to 800g / m 2 ), more preferably 100 g / m 2 Up to 600g / m 2 , even more preferably 150g / m 2 Up to 500g / m 2From the viewpoint of providing sufficient liquid absorption performance as an absorbent article, particularly suppressing the occurrence of gel blocking to enhance liquid diffusion performance, and further enhancing the strength of the absorbent material after liquid absorption, the fiber material content is preferably 50 g or more per square meter of absorbent material (i.e., 50 g / m 2 In particular, from the viewpoint of suppressing the reversion after liquid absorption, the fiber material content is preferably 800 g or less per square meter of the absorbent material (i.e., 800 g / m 2 the following).
[0118] In order to enhance shape retention before and during use of the absorbent material, the fibers can be bonded to each other by adding an adhesive binder to the fiber material. Examples of adhesive binders include hot-melt synthetic fibers, hot-melt adhesives, and adhesive emulsions. These adhesive binders can be used alone or in combination of two or more.
[0119] Examples of heat-fusible synthetic fibers include fully fusible binders such as polyethylene, polypropylene, and ethylene-propylene copolymers, and non-fully fusible binders having a side-by-side structure or a core-sheath structure of polypropylene and polyethylene, wherein only the polyethylene portion can be heat-fusible.
[0120] Examples of hot melt adhesives include mixtures of base polymers such as ethylene-vinyl acetate copolymers, styrene-isoprene-styrene block copolymers, styrene-butadiene-styrene block copolymers, styrene-ethylene-butylene-styrene block copolymers, styrene-ethylene-propylene-styrene block copolymers, or amorphous polypropylene with tackifiers, plasticizers, or antioxidants.
[0121] Examples of the adhesive emulsion include polymers of at least one monomer selected from the group consisting of methyl methacrylate, styrene, acrylonitrile, 2-ethylhexyl acrylate, butyl acrylate, butadiene, ethylene, and vinyl acetate.
[0122] [additive]
[0123] The absorbent material according to the present embodiment may further include various additives, such as inorganic powders, deodorants, pigments, dyes, spices, antibacterial agents, and adhesives, all of which are commonly used in the art. These additives can impart various functions to the absorbent material. Examples of inorganic powders include silicon dioxide, zeolite, mica, kaolin, and clay. When the water-absorbent resin particles include inorganic particles, the absorbent material may also include inorganic powders in addition to the inorganic particles in the water-absorbent resin particles.
[0124] [Absorbent products]
[0125] An absorbent article according to one embodiment (present embodiment) of the present invention comprises an absorbent material, a liquid-permeable sheet disposed at the outermost portion on the inflow side of the target liquid to be absorbed, and a liquid-impermeable sheet disposed at the outermost portion on the side opposite to the inflow side of the target liquid to be absorbed. Examples of absorbent articles include diapers (e.g., disposable diapers), toilet training pants, incontinence pads, urine absorbing pads, urine absorbing liners, sanitary products such as sanitary napkins and tampons, sweat-absorbing pads, pet pads, portable toilet pieces, and animal excrement disposal materials.
[0126] In the absorbent article, a liquid-impermeable sheet, an absorbent material, and a liquid-permeable sheet are laminated in this order.
[0127] The absorbent article according to the present embodiment includes the absorbent material according to the present embodiment. In addition to the absorbent material according to the present embodiment, the absorbent article according to the present embodiment may also include another known absorbent material. The absorbent article according to the present embodiment preferably includes only the absorbent material according to the present embodiment as the absorbent material.
[0128] [Liquid-permeable sheet]
[0129] The liquid-permeable sheet is disposed at the outermost portion on the inflow side of the target liquid to be absorbed. The liquid-permeable sheet has, for example, a main surface wider than the absorbent material. The outer edge portion of the liquid-permeable sheet extends around the absorbent material.
[0130] The liquid-permeable sheet may be a sheet formed of a resin or fiber commonly used in the art. From the viewpoint of liquid permeability, softness and strength when the liquid-permeable sheet is used for absorbent articles, the liquid-permeable sheet may contain a synthetic resin, for example, a polyolefin, such as polyethylene (PE) or polypropylene (PP); a polyester, such as poly(ethylene terephthalate) (PET), poly(trimethylene terephthalate) (PTT), poly(ethylene naphthalate) (PEN), poly(butylene adipate terephthalate) (PBAT), poly(butylene succinate) (PBS), poly(butylene succinate adipate) (PBSA), poly(lactic acid) or polyhydroxyalkanoate; a polyamide, such as nylon or rayon. The liquid-permeable sheet may contain synthetic fibers containing one or more of these synthetic resins, or may contain natural fibers containing cotton, silk, hemp, or pulp (cellulose). From the viewpoint of increasing the strength of the liquid-permeable sheet, for example, the liquid-permeable sheet may contain synthetic fibers. The synthetic fibers may be polyolefin fibers, polyester fibers, or a combination thereof. These materials may be used alone or in combination of two or more thereof.
[0131] The liquid permeable sheet may be a nonwoven fabric, a porous sheet, or a combination thereof. A nonwoven fabric is a sheet in which fibers are entangled rather than woven. The nonwoven fabric may be a nonwoven fabric composed of short fibers (i.e., staple fibers) (short fiber nonwoven fabric), or may be a nonwoven fabric composed of long fibers (i.e., filaments) (long fiber nonwoven fabric). The staple fibers may have a fiber length of typically but not limited to several hundred millimeters or less.
[0132] The liquid-permeable sheet may be at least one nonwoven fabric selected from the group consisting of thermally bonded nonwoven fabrics, air-through nonwoven fabrics, resin-bonded nonwoven fabrics, spunbonded nonwoven fabrics, meltblown nonwoven fabrics, spunbonded / meltblown / spunbonded nonwoven fabrics, air-laid nonwoven fabrics, spunlace nonwoven fabrics, and point-bonded nonwoven fabrics. The liquid-permeable sheet is preferably at least one nonwoven fabric selected from the group consisting of thermally bonded nonwoven fabrics, air-through nonwoven fabrics, spunbonded nonwoven fabrics, and spunbonded / meltblown / spunbonded nonwoven fabrics.
[0133] The liquid permeable sheet can be a thermally bonded nonwoven fabric, a hot air nonwoven fabric, a resin bonded nonwoven fabric, a spunbond nonwoven fabric, a meltblown nonwoven fabric, an air-laid nonwoven fabric, a spunlace nonwoven fabric, a point-bonded nonwoven fabric, or a laminate of two or more nonwoven fabrics selected therefrom. These nonwoven materials can be formed by the above-mentioned synthetic fibers or natural fibers. The laminate of two or more nonwoven fabrics can be, for example, a spunbond / meltblown / spunbond nonwoven fabric, which is a composite nonwoven fabric including spunbond nonwoven fabrics, meltblown nonwoven fabrics, and spunbond nonwoven fabrics laminated in sequence. Among them, from the viewpoint of suppressing liquid leakage, thermally bonded nonwoven fabrics, hot air nonwoven fabrics, spunbond nonwoven fabrics, or spunbond / meltblown / spunbond nonwoven fabrics are preferably used.
[0134] From the viewpoint of the liquid absorption performance of the absorbent article, the nonwoven fabric used as the liquid-permeable sheet preferably has appropriate hydrophilicity.
[0135] The hydrophilic nonwoven fabric as described above can be formed by fibers showing an appropriate degree of hydrophilicity, such as rayon fibers, or can be formed by fibers obtained by subjecting hydrophobic chemical fibers such as polyolefin fibers or polyester fibers to hydrophilization. Examples of methods for obtaining a nonwoven fabric containing hydrophobic chemical fibers that have been subjected to hydrophilization include: a method in which a nonwoven fabric is obtained by a spunbonding method using hydrophobic chemical fibers mixed with a hydrophilic agent, a method in which a spunbonded nonwoven fabric is produced using a hydrophobic chemical fiber in the presence of a hydrophilic agent, and a method in which a spunbonded nonwoven fabric obtained using a hydrophobic chemical fiber is impregnated with a hydrophilic agent. Examples of hydrophilic agents include anionic surfactants such as aliphatic sulfonates and higher alcohol sulfates; cationic surfactants such as quaternary ammonium salts; nonionic surfactants such as polyethylene glycol fatty acid esters, polyglycerol fatty acid esters, and sorbitan fatty acid esters; silicone surfactants such as polyoxyalkylene-modified silicones; and a stain release agent composed of a polyester resin, a polyamide resin, an acrylic resin, or a polyurethane resin.
[0136] From the viewpoint of imparting good liquid permeability, softness, strength, and cushioning properties to the absorbent article and from the viewpoint of increasing the liquid permeability of the absorbent article, the liquid-permeable sheet is preferably a nonwoven fabric which is appropriately bulky and has a large weight per unit area.
[0137] [Liquid impermeable sheet]
[0138] The liquid-impermeable sheet is disposed at the outermost portion on the opposite side of the liquid-permeable sheet of the absorbent article. The liquid-impermeable sheet has, for example, a main surface that is wider than the absorbent material. The outer edge portion of the liquid-impermeable sheet extends around the absorbent material. The liquid-impermeable sheet prevents the liquid that has been absorbed by the absorbent material from leaking to the outside from the liquid-impermeable sheet side.
[0139] Examples of liquid-impermeable sheets include sheets composed of resins such as polyethylene, polypropylene, poly(vinyl chloride), poly(lactic acid), or polyhydroxyalkanoate; sheets composed of nonwoven fabrics such as spunbond / meltblown / spunbond (SMS) nonwoven fabrics in which a waterproof meltblown nonwoven fabric is inserted between high-strength spunbond nonwoven fabric layers; and sheets composed of composite materials of one or more of those resins and nonwoven fabrics such as spunbond nonwoven fabrics or spunlace nonwoven fabrics. The liquid-impermeable sheet is preferably breathable from the viewpoint of, for example, reducing humidity during wear to reduce discomfort to the wearer. As the liquid-impermeable sheet, a sheet composed of a synthetic resin mainly containing a low-density polyethylene (LDPE) resin can be used.
[0140] The dimensional relationship among the absorbent material, the liquid-permeable sheet, and the liquid-impermeable sheet is not particularly limited, and is appropriately adjusted depending on, for example, the use of the absorbent article.
[0141] [Example]
[0142] Although the present invention will be described in more detail below by way of examples, the present invention is not limited to these examples.
[0143] The raw materials, equipment, etc. used in these examples of the present invention will be described below.
[0144] [raw material]
[0145] Aspartic acid: available from Yixing Qiancheng Bio-Engineering Co., Ltd., purity: 99.97%
[0146] Phosphoric acid: Available from Kanto Chemical Co., Inc., purity: 85%
[0147] L-Lysine: Available from Tokyo Chemical Industry Co., Ltd., purity: 97%
[0148] L-Ornithine monohydrochloride: Available from Kanto Chemical Co., Inc., purity: 98%
[0149] Phosphoethanolamine: Available from Tokyo Chemical Industry Co., Ltd., purity: 98%
[0150] Hexamethylenediamine: Available from Kanto Chemical Co., Inc., purity: 98%
[0151] Multifunctional epoxy compound: Available from Nagase ChemteX Corporation, EX-810
[0152] [Evaluation method]
[0153] [Measurement of Weight Average Molecular Weight of Polysuccinimide]
[0154] The weight average molecular weight of polysuccinimide is measured by GPC method (differential refractometer) in terms of polystyrene. G1000HHR column, G4000HHR column, and GMHHR-H column (TSKgel (registered trademark), available from Tosoh Corporation) are used for measurement. Dimethylformamide containing 10 mM lithium bromide is used as an eluent.
[0155] [Evaluation of water absorption]
[0156] The water absorption was evaluated using physiological saline according to the tea bag method (JIS K-7223). The water absorption capacity was calculated by the following formula.
[0157] Water absorption capacity [g-water / g] = {(weight after water absorption) - (blank weight after water absorption) - (sample weight)} / (sample weight)
[0158] [Evaluation of water retention]
[0159] To evaluate water retention, after evaluating the water absorption capacity by the tea bag method, the tea bag was dehydrated in a centrifugal dehydrator at 25°C, 150G x 2 minutes. The weight of the dehydrated tea bag was then measured. The water retention capacity was calculated by the following formula.
[0160] Water retention capacity [g-water / g] = {(weight after dehydration) - (blank weight after dehydration) - (sample weight)} / (sample weight)
[0161] [Evaluation of elastic modulus]
[0162] The elastic modulus was measured with a MCR-102 rotational rheometer (available from Anton Paar) at an angular frequency of 0.1 to 100 (rad / s) using PP-25 parallel plates with a gap of 2 mm at a measurement temperature of 25° C. The storage elastic modulus at an angular frequency of 1.0 (rad / s) was used.
[0163] (Synthesis example 1)
[0164] [Synthesis of polysuccinimide]
[0165] In a mortar, 160 parts of aspartic acid and 83 parts of 85% phosphoric acid were mixed together. The mixture was transferred to a tray. The reaction was carried out at 190°C and 1.3 kPa for 6 hours. The reaction mixture was crushed, washed with distilled water until the filtrate was neutral, and dried in vacuum at 80°C to obtain 115 parts of polysuccinimide having a weight average molecular weight of 70,000.
[0166] [Example 1]
[0167] [Synthesis of poly(aspartic acid) crosslinkers]
[0168] [Synthesis of Reaction Product (P1) of PSI and Compound (A)]
[0169] First, 2.23 parts of L-lysine are added to 20 parts of distilled water and dissolved under stirring, and then 10 parts of the polysuccinimide prepared in Synthesis Example 1 are added thereto. While the pH is adjusted to 10 to 11, 9.75 parts of a 36% NaOH aqueous solution are added dropwise under stirring at room temperature. After the dropwise addition is completed, the mixture is stirred for another 15 hours at room temperature. The resulting reaction solution is filtered through a nylon mesh filter with a 59-μm opening to obtain a sodium polyaspartate solution (solid content: 43%) to which lysine is added. NMR analysis reveals that the percentage of the unit to which lysine is added is 9.2% of the total unit.
[0170] [Synthesis of cross-linked products]
[0171] First, 4.64 parts of the sodium polyaspartate solution to which lysine was added prepared in the above step was mixed with 0.106 parts of EX-810 multifunctional epoxy compound (available from Nagase ChemteX Corporation), and the mixture was heated and reacted at 60° C. The elastic modulus measurement at each predetermined reaction time indicated a storage elastic modulus of 1,100 Pa at a reaction time of 60 minutes and a storage elastic modulus of 1,180 Pa at a reaction time of 180 minutes. After the reaction time of 180 minutes, the gel shape was maintained.
[0172] The gel composition obtained at a reaction time of 180 minutes was freeze-dried. The dried composition was ground in a mortar and sieved with a stainless steel sieve (JIS Z-8801) to have a particle size of 150 to 710 μm. The water absorption and water retention were measured to be 45.5 g / g and 29.1 g / g, respectively.
[0173] [Example 2]
[0174] [Synthesis of poly(aspartic acid) crosslinkers]
[0175] [Synthesis of Reaction Product of PSI and Compound (A)]
[0176] First, 2.61 parts of L-ornithine monohydrochloride and 1.29 parts of 48% NaOH aqueous solution were added to 19.3 parts of distilled water and dissolved under stirring, and then 10 parts of the polysuccinimide prepared in Synthesis Example 1 were added thereto. While adjusting the pH to 11 to 12, 9.72 parts of 36% NaOH aqueous solution were added dropwise under stirring at room temperature. After the dropwise addition was completed, the mixture was stirred for another 15 hours at room temperature. The resulting reaction solution was filtered through a nylon mesh filter with a 59-μm opening to obtain a sodium polyaspartate solution (solid content: 50%) to which ornithine was added. NMR analysis revealed that the percentage of the unit to which ornithine was added was 10.1% of the total unit.
[0177] [Synthesis of cross-linked products]
[0178] First, 5.73 parts of the sodium polyaspartate solution to which ornithine was added prepared in the above step was mixed with 0.148 parts of EX-810 multifunctional epoxy compound (available from Nagase ChemteX Corporation), and the mixture was heated and reacted at 60° C. The elastic modulus measurement at each predetermined reaction time indicated a storage elastic modulus of 680 Pa at a reaction time of 60 minutes and a storage elastic modulus of 730 Pa at a reaction time of 180 minutes. After the reaction time of 180 minutes, the gel shape was maintained.
[0179] The gel composition obtained at a reaction time of 180 minutes was freeze-dried. The dried composition was ground in a mortar and sieved with a stainless steel sieve (JIS Z-8801) to have a particle size of 150 to 710 μm. The water absorption and water retention were measured to be 46.0 g / g and 31.2 g / g, respectively.
[0180] [Example 3]
[0181] [Synthesis of Reaction Product of PSI and Compound (A)]
[0182] First, 2.18 parts of ethanolamine phosphate and 1.29 parts of 48% NaOH aqueous solution are added to 19.3 parts of distilled water and dissolved under stirring, and then 10 parts of the polysuccinimide prepared in Synthesis Example 1 are added thereto. While adjusting pH to 11 to 12, 9.72 parts of 36% NaOH aqueous solution are added dropwise at room temperature under stirring. After completing the dropwise addition, the mixture is stirred for another 15 hours at room temperature. The resulting reaction solution is filtered through a nylon mesh filter with 59-μm openings to obtain a polyaspartate sodium solution (solid content: 38%) to which ethanolamine phosphate is added. NMR analysis reveals that the percentage of the unit to which ethanolamine phosphate is added is 5.5% of the total unit.
[0183] [Synthesis of cross-linked products]
[0184] First, 5.50 parts of the sodium polyaspartate solution to which ethanolamine was added prepared in the above step was mixed with 0.445 parts of EX-810 multifunctional epoxy compound (available from Nagase ChemteX Corporation), and the mixture was heated and reacted at 60° C. The elastic modulus measurement at each predetermined reaction time showed a storage elastic modulus of 1,250 Pa at a reaction time of 60 minutes and a storage elastic modulus of 1,310 Pa at a reaction time of 180 minutes. After the reaction time of 180 minutes, the gel shape was maintained.
[0185] The gel composition obtained at a reaction time of 180 minutes was freeze-dried. The dried composition was ground in a mortar and sieved with a stainless steel sieve (JIS Z-8801) to have a particle size of 150 to 710 μm. The water absorption and water retention were measured to be 40.8 g / g and 29.0 g / g, respectively.
[0186] (Comparative Example 1)
[0187] The polysuccinimide prepared in Synthesis Example 1 was hydrolyzed with an aqueous sodium hydroxide solution to prepare an aqueous solution of sodium polyaspartate (solid content: 30%). Hydrochloric acid was added to 5.43 parts of the resulting aqueous solution of sodium polyaspartate to adjust the pH to 5.0. Then, 0.135 parts of an EX-810 multifunctional epoxy compound (available from Nagase ChemteX Corporation) was mixed, and the mixture was heated and reacted at 60°C. The elastic modulus measurement at each predetermined reaction time showed a storage elastic modulus of 42.2 Pa at a reaction time of 60 minutes, a storage elastic modulus of 1,510 Pa at a reaction time of 120 minutes, and a storage elastic modulus of 6.71 Pa at a reaction time of 180 minutes. After a reaction time of 180 minutes, the product was in a liquid state with high fluidity and did not maintain its gel shape. The reason may be that the cross-linked portion of the product is an ester bond, and the product is de-crosslinked.
[0188] (Comparative Example 2)
[0189] Two parts of the polysuccinimide prepared in Synthesis Example 1 were added to 20 parts of distilled water, and the mixture was stirred to prepare a polysuccinimide dispersion. A mixture of 0.48 parts of hexamethylenediamine, 2.78 parts of a 24% NaOH aqueous solution, and 2.91 parts of distilled water was stirred at room temperature to prepare a diamine crosslinking agent mixture. The diamine crosslinking agent mixture was added dropwise to the polysuccinimide dispersion. Stirring was continued after the dropwise addition was completed, thereby preparing a gel composition. The elastic modulus measurement at each predetermined reaction time showed a storage elastic modulus of 800 Pa at a reaction time of 60 minutes and a storage elastic modulus of 820 Pa at a reaction time of 180 minutes. After the reaction time of 180 minutes, the gel shape was maintained.
[0190] The obtained gel composition was washed with methanol, dried in a vacuum at 60°C, ground in a mortar, and sieved with a stainless steel sieve (JIS Z-8801) so as to have a particle size of 150 to 710 μm. The water absorption and water retention were measured to be 13.9 g / g and 8.9 g / g, respectively. It is presumed that it is difficult to prepare a gel having a designed crosslinking degree by crosslinking with a diamine in water, and thus the product has low water absorption and low water retention.
[0191]
[0192] [Example 4]
[0193] [Water-absorbent resin particles]
[0194] The gel composition obtained in Example 1 was freeze-dried. The dried composition was ground in a mortar and sieved with a stainless steel sieve (JIS Z-8801) so as to have a particle size of 150 μm to 710 μm. Then 100 parts of the resulting water-absorbent resin was mixed with 0.5 parts of Aerosil 200 (hydrophilic amorphous silica, available from Nippon Aerosil Co., Ltd.) to produce water-absorbent resin particles. The water absorption and water retention of the resulting particles were measured and found to be 45.0 g / g and 29.0 g / g, respectively.
[0195] [Example 5]
[0196] [Absorbent material and absorbent article]
[0197] 70 parts of the water-absorbent resin particles obtained in Example 4 and 30 parts of groundwood pulp were dry-blended using a mixer. The resulting mixture was air-laid on a 400-mesh (opening size: 38 μm) wire screen using an air-laid former to produce an absorbent material.
[0198] Subsequently, the liquid-impermeable sheet composed of liquid-impermeable polypropylene, the absorbent material, and the liquid-permeable sheet formed of nonwoven fabric composed of liquid-permeable polypropylene were sequentially bonded to one another using a double-sided tape to produce an absorbent article.
[0199] Industrial Applicability
[0200] The present invention can provide a poly(aspartic acid) crosslinker and a method for producing the poly(aspartic acid) crosslinker, which can maintain gel shape, water absorption, water retention, and other properties because it does not undergo hydrolysis over time due to the lack of ester bonds. The poly(aspartic acid) crosslinker of the present invention can be used for superabsorbent resins for diaper applications, sanitary products, cosmetic additives such as thickeners, and other biodegradable resins (for example, for agriculture and civil engineering).
Claims
1. A poly(aspartic acid) crosslinker, wherein the poly(aspartic acid) crosslinker is the reaction product of: Polysuccinimide (PSI), A compound (A: a1-A1-a2) containing a first functional group (a1) and a second functional group (a2), and A polyfunctional epoxy compound (B), wherein the poly(aspartic acid) crosslinker comprises a PSI-a1(A) bond formed by an addition reaction of the first functional group (a1) and the polysuccinimide (PSI), The poly(aspartic acid) crosslinker comprises a B-a2(A) bond formed by the reaction of the second functional group (a2) and the multifunctional epoxy compound (B), The poly(aspartic acid) crosslinker comprises a crosslinked structure (PABAP) represented by PSI-a1-A1-a2-B-a2-A1-a1-PSI, The cross-linked structure (PABAP) is partially hydrolyzed, and The second functional group of the compound (A) does not react with the polysuccinimide (PSI) or has a lower reactivity with the polysuccinimide (PSI) than the first functional group.
2. The poly(aspartic acid) crosslinker according to claim 1, wherein the first functional group (a1) is an amino group (NH2-), The second functional group (a2) is one or more selected from the group consisting of an amino group (NH2-) and a phosphonooxy group ((OH)2P(=O)-O-), and When the second functional group (a2) is an amino group (NH2-), the reactivity of the second functional group with the polysuccinimide (PSI) is lower than that of the first functional group (a1).
3. The cross-linked poly(aspartic acid) according to claim 1 or 2, wherein the first functional group (a1) is an amino group (NH2-), and The second functional group (a2) is an amino group (NH2-), and Wherein in the compound (A), the amino group of the second functional group (a2) is an amino group in a structure represented by formula (1): [Chemical formula 1] In formula (1), G is a carboxylic acid group or a salt of a carboxylic acid group. 4 . The crosslinked poly(aspartic acid) according to claim 1 , wherein the compound (A) is one or more selected from the group consisting of lysine, ornithine, and arginine.
5. A water-absorbing composition comprising the poly(aspartic acid) crosslinker according to any one of claims 1 to 4.
6. A thickening composition comprising the poly(aspartic acid) crosslinker according to any one of claims 1 to 4.
7. A method for producing a poly(aspartic acid) crosslinker, the method comprising the steps of: A crosslinked product is formed by reacting polysuccinimide (PSI) with a compound (A: a1-A1-a2) containing a first functional group (a1) and a second functional group (a2) and a multifunctional epoxy compound (B) in water or a water-containing solvent, The second functional group of the compound (A) does not react with the polysuccinimide (PSI) or has a lower reactivity with the polysuccinimide (PSI) than the first functional group.
8. The method for producing a poly(aspartic acid) crosslinker according to claim 7, wherein the first functional group (a1) is an amino group (NH2-), The second functional group (a2) is one or more selected from the group consisting of an amino group (NH2-) and a phosphonooxy group ((OH)2P(=O)-O-), and When the second functional group (a2) is an amino group (NH2-), the reactivity of the second functional group with polysuccinimide (PSI) is lower than that of the first functional group (a1).
9. A method for producing a poly(aspartic acid) crosslinker according to claim 7 or 8, wherein the first functional group (a1) is an amino group (NH2-), and The second functional group (a2) is an amino group (NH2-), and Wherein in the compound (A), the amino group of the first functional group (a1) is the amino group in NH2-CH2-, and the amino group of the second functional group (a2) is the amino group in the structure represented by formula (1): [Chemical formula 2] In formula (1), G is a carboxylic acid group or a salt of a carboxylic acid group. 10 . The method for producing a poly(aspartic acid) crosslinked body according to claim 7 , wherein the compound (A) is one or more selected from the group consisting of lysine, ornithine, and arginine.
11. A water-absorbent resin comprising the crosslinked poly(aspartic acid) according to any one of claims 1 to 4. 12 . Water-absorbent resin particles comprising the water-absorbent resin according to claim 11 .
13. An absorbent comprising the water-absorbent resin particles according to claim 12, and a fiber layer containing fibers.
14. An absorbent article provided with a liquid-impermeable sheet, the absorbent according to claim 13, and a liquid-permeable sheet, wherein the liquid-impermeable sheet, the absorbent and the liquid-permeable sheet are arranged in this order.