Nonaqueous secondary battery
By using an optimized non-aqueous electrolyte and a polypropylene-based microporous membrane in a non-aqueous secondary battery, the problems of insufficient volatility and ion conductivity of the acetonitrile electrolyte are solved, and efficient battery performance is achieved.
Patent Information
- Application Number
- CN202380023386.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-08
AI Technical Summary
When existing non-aqueous secondary batteries use non-aqueous electrolytes containing acetonitrile, there are volatility problems and insufficient ion conductivity, which affects battery performance.
A non-aqueous electrolyte containing 10% to 90% by volume of acetonitrile is used. Organic polymers and specific lithium salts are added to optimize the viscosity and ion conductivity of the electrolyte, and a polypropylene-based microporous membrane is used as a spacer. , forming an efficient battery structure.
It effectively suppresses the volatility of the electrolyte, improves the ion conductivity and overall performance of the battery, and realizes a non-aqueous secondary battery with high output and long life.
Smart Images

Figure CN118749149A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a non-aqueous secondary battery. Background Art
[0002] Non-aqueous secondary batteries, mainly lithium-ion batteries, have the major characteristics of being small, high-capacity, and high-output, and are widely used as power sources for various portable electronic devices.
[0003] In order to realize the small-sized, high-capacity battery, it is important to select a separator to be arranged between the electrodes. In the past, paper, woven fabric, nonwoven fabric, glass mat, etc. were used as separators, but they have problems in structure and safety. In recent years, separators with small pore sizes such as polyolefin microporous membranes have been used to improve safety by shutting down the function and suppressing the short circuit between the electrodes.
[0004] Furthermore, conventionally, non-aqueous electrolytes used for non-aqueous secondary batteries use cyclic carbonate or cyclic ester solvents, but there is a problem that the impregnation of the separator with the electrolyte is poor.
[0005] However, in recent years, the impregnation property into the spacer has been improved by diluting a chain carbonate in a non-aqueous electrolyte solution using a cyclic carbonate or cyclic ester solvent and then adding a surfactant.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Publication No. 2014-13659.
[0009] Patent document 2: Japanese Patent Application Publication No. 2000-133309. Summary of the invention
[0010] Problems to be solved by the invention
[0011] Compared with the non-aqueous electrolyte using ester as solvent as described above, the non-aqueous electrolyte containing acetonitrile has high ion conductivity, and therefore, by being applied to a non-aqueous secondary battery, high output performance can be obtained. On the other hand, it has been newly discovered that when a non-aqueous electrolyte containing acetonitrile having a low boiling point is used compared with the commonly used ester solvent, there is a problem of volatility in the process of manufacturing a non-aqueous secondary battery.
[0012] Patent Document 1 reports that by including polymers having reactive functional groups such as acrylates and methacrylates in a non-aqueous electrolyte, the reduction decomposition reaction on the surface of the negative electrode active material is suppressed, thereby improving the battery characteristics. However, there is no mention of issues related to the volatility of the non-aqueous electrolyte.
[0013] Patent Document 2 reports that by including an organic polymer with a molecular weight of 20,000 or less in a non-aqueous electrolyte, the reduction decomposition reaction on the surface of the negative electrode active material is suppressed, thereby improving battery characteristics. However, there is no mention of issues related to the volatility of the non-aqueous electrolyte.
[0014] The present invention has been made in view of the above problems, and an object of the present invention is to provide a nonaqueous secondary battery having low volatility of the nonaqueous electrolyte solution and high ion conductivity even when the nonaqueous electrolyte solution containing acetonitrile is used.
[0015] Another object of the present invention is to provide a non-aqueous electrolyte solution containing acetonitrile that can realize the non-aqueous secondary battery.
[0016] Means for solving problems
[0017] One embodiment of the present invention is as follows.
[0018] [1] A non-aqueous secondary battery comprising a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions, a negative electrode containing a material capable of absorbing and releasing lithium ions, a non-aqueous electrolyte, and a separator,
[0019] The non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer.
[0020] The non-aqueous solvent contains 10% by volume or more and 90% by volume or less of acetonitrile,
[0021] The lithium salt includes a lithium imide salt, and the content of the lithium salt is 0.5 mol / L or more and 2 mol / L or less relative to the non-aqueous electrolyte solution,
[0022] The viscosity average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less,
[0023] The non-aqueous electrolyte has a viscosity of 2 mPa·s or more and 500 mPa·s or less at 25° C., an ion conductivity of 13 mS / cm or more, and Z represented by the following formula (1) is 70 or more.
[0024] Z = viscosity of electrolyte (mPa·s)×ion conductivity of electrolyte (mS / cm) (1).
[0025] [2] The non-aqueous secondary battery according to item 1, wherein the organic polymer has at least one of a polyether structure and an ester structure.
[0026] [3] The non-aqueous secondary battery according to item 1 or 2, wherein the organic polymer comprises at least one of polyethylene oxide and poly(methyl methacrylate).
[0027] [4] The nonaqueous secondary battery according to any one of items 1 to 3, wherein the viscosity average molecular weight of the organic polymer is 90,000 to 650,000.
[0028] [5] The nonaqueous secondary battery according to any one of items 1 to 4, wherein the content of the organic polymer is 0.1% by mass or more and 10% by mass or less relative to the total amount of the nonaqueous electrolyte.
[0029] [6] The nonaqueous secondary battery according to any one of items 1 to 5, wherein the content of the organic polymer is 0.1 mass % or more and 3 mass % or less relative to the total amount of the nonaqueous electrolyte.
[0030] [7] The nonaqueous secondary battery according to any one of items 1 to 6, wherein the area of at least one of the positive electrode and the negative electrode is 100 cm 2 above.
[0031] [8] A non-aqueous secondary battery as described in any one of items 1 to 7, wherein a wound body formed by winding a stack with the separator sandwiched between the positive electrode and the negative electrode, a stack formed by alternately stacking positive and negative electrode sheets via the separator, and a stack formed by alternately inserting positive electrodes and negative electrodes between zigzag separators is housed in the battery exterior.
[0032] [9] A non-aqueous secondary battery according to any one of items 1 to 8, wherein the viscosity of the non-aqueous electrolyte at 25°C is greater than or equal to 2.5 mPa·s and less than or equal to 150 mPa·s, and the ion conductivity at 25°C is greater than or equal to 10 mS / cm and less than or equal to 40 mS / cm.
[0033]
[10] A non-aqueous secondary battery as described in any one of items 1 to 9, wherein the lithium salt further includes lithium hexafluorophosphate (LiPF6), and the non-aqueous secondary battery includes the lithium-containing imide salt and the LiPF6 at a molar concentration of the LiPF6 less than the lithium-containing imide salt.
[0034]
[11] The nonaqueous secondary battery according to any one of items 1 to 10, wherein the nonaqueous solvent contains 20% by volume or more and 90% by volume or less of acetonitrile.
[0035]
[12] The non-aqueous secondary battery according to any one of items 1 to 11, wherein the porosity of the separator is 20% or more and 90% or less, and the air permeability resistance is 20 sec / 100 cm 3 Above and 500 seconds / 100cm 3 the following.
[0036]
[13] A non-aqueous secondary battery as described in any one of items 1 to 12, wherein a porous layer containing an inorganic filler is provided on one or both sides of the separator, the inorganic filler being at least one selected from the group consisting of aluminum oxide, basic aluminum oxide, and aluminum silicate.
[0037]
[14] A non-aqueous secondary battery as described in any one of items 1 to 13, wherein the separator has a polypropylene-based microporous membrane, in which a polymer matrix containing the polypropylene extends in a direction perpendicular to the membrane thickness, fibrils containing the polypropylene are formed between the polymer matrix, and micropores are formed between a plurality of the fibrils.
[0038]
[15] A non-aqueous secondary battery as described in any one of items 1 to 14, wherein the separator has a polypropylene-based microporous membrane, and the pore size ratio a / b of the average long pore diameter a of the microporous membrane to the pore diameter b orthogonal to the average long pore diameter a is greater than or equal to 0.5 and less than or equal to 30.
[0039]
[16] A non-aqueous electrolyte for a non-aqueous secondary battery having a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions, a negative electrode containing a material capable of absorbing and releasing lithium ions, a non-aqueous electrolyte, and a separator, wherein:
[0040] The non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer.
[0041] The non-aqueous solvent contains 10% by volume or more and 90% by volume or less of acetonitrile,
[0042] The lithium salt includes a lithium imide salt, and the content of the lithium salt is 0.5 mol / L or more and 2 mol / L or less relative to the non-aqueous electrolyte solution,
[0043] The viscosity average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less,
[0044] The non-aqueous electrolyte has a viscosity of 2 mPa·s or more and 500 mPa·s or less at 25° C., an ion conductivity of 13 mS / cm or more, and Z represented by the following formula (1) is 70 or more.
[0045] Z = viscosity of electrolyte (mPa·s)×ion conductivity of electrolyte (mS / cm) (1).
[0046] In addition, the present invention relates to the following aspects.
[0047] [1A] A nonaqueous secondary battery comprising a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions, a negative electrode containing a material capable of absorbing and releasing lithium ions, a nonaqueous electrolyte, and a separator, wherein:
[0048] The non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer.
[0049] The non-aqueous solvent contains 5 volume % or more and 90 volume % or less of acetonitrile,
[0050] The lithium salt includes a lithium imide salt, and the content of the lithium salt is 1 mol / L or more and 2 mol / L or less relative to the non-aqueous electrolyte solution,
[0051] The organic polymer has at least one of a polyether structure and a five-membered ring lactam structure.
[0052] The viscosity average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less,
[0053] The spacer has a polypropylene microporous membrane,
[0054] In the polypropylene-based microporous membrane, a polymer matrix containing polypropylene extends in one direction perpendicular to the membrane thickness, and fibrils containing the polypropylene and micropores between a plurality of the fibrils are present between the polymer matrix.
[0055] [2A] The non-aqueous secondary battery according to item 1A, wherein the organic polymer comprises at least one of polyethylene oxide and polyvinyl pyrrolidone.
[0056] [3A] The nonaqueous secondary battery according to item 1A or 2A, wherein the content of the organic polymer is 0.1 mass % or more and 10 mass % or less relative to the total amount of the nonaqueous electrolyte solution.
[0057] [4A] The non-aqueous secondary battery according to any one of items 1A to 3A, wherein the viscosity of the non-aqueous electrolyte at 25°C is greater than or equal to 1.5 mPa·s and less than or equal to 40 mPa·s, and the ion conductivity at 25°C is greater than or equal to 10 mS / cm and less than or equal to 40 mS / cm.
[0058] [5A] The non-aqueous secondary battery according to any one of items 1A to 4A, wherein the pore size ratio a / b of the average long pore size a of the polypropylene-based microporous membrane to the pore size b orthogonal to the average long pore size a is 0.5 or more and 30 or less.
[0059] [6A] The non-aqueous secondary battery according to any one of items 1A to 5A, wherein the porosity of the separator is 30% or more and 80% or less, and the air permeability resistance is 100 sec / 100 cm 3 Above and 500 seconds / 100cm 3 the following.
[0060] [7A] A non-aqueous secondary battery as described in any one of items 1A to 6A, wherein the lithium salt further includes lithium hexafluorophosphate (LiPF6), and the non-aqueous secondary battery includes the lithium-containing imide salt and the LiPF6 at a molar concentration of the LiPF6 less than the lithium-containing imide salt.
[0061] In addition, the present invention also relates to the following aspects.
[0062] [1B] A non-aqueous secondary battery comprising a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions, a negative electrode containing a material capable of absorbing and releasing lithium ions, a non-aqueous electrolyte, and a separator, wherein:
[0063] The non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer.
[0064] The non-aqueous solvent contains 5 volume % or more and 90 volume % or less of acetonitrile,
[0065] The lithium salt includes a lithium imide salt, and the content of the lithium salt is 1 mol / L or more and 2 mol / L or less relative to the non-aqueous electrolyte solution,
[0066] The organic polymer has at least one of a polyether structure and a five-membered ring lactam structure.
[0067] The viscosity average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less,
[0068] The separator is a microporous film including at least one of polyethylene and polypropylene, and has a porous layer including an inorganic filler on one or both surfaces of the microporous film.
[0069] [2B] The non-aqueous secondary battery according to item 1B, wherein the organic polymer comprises at least one of polyethylene oxide and polyvinyl pyrrolidone.
[0070] [3B] The nonaqueous secondary battery according to item 1B or 2B, wherein the content of the organic polymer is 0.1 mass % or more and 10 mass % or less relative to the total amount of the nonaqueous electrolyte solution.
[0071] [4B] The non-aqueous secondary battery according to any one of items 1B to 3B, wherein the viscosity of the non-aqueous electrolyte at 25°C is 1.5 mPa·s or more and 40 mPa·s or less, and the ion conductivity at 25°C is 10 mS / cm or more and 40 mS / cm or less.
[0072] [5B] The nonaqueous secondary battery according to any one of items 1B to 4B, wherein the inorganic filler is at least one selected from the group consisting of aluminum oxide, basic aluminum oxide, and aluminum silicate.
[0073] [6B] The non-aqueous secondary battery according to any one of items 1B to 5B, wherein the porosity of the separator is 20% or more and 90% or less, and the air permeability resistance is 20 sec / 100 cm 3 Above and 500 seconds / 100cm 3 the following.
[0074] [7B] A non-aqueous secondary battery as described in any one of items 1B to 6B, wherein the lithium salt further includes lithium hexafluorophosphate (LiPF6), and the non-aqueous secondary battery includes the lithium-containing imide salt and the LiPF6 at a molar concentration of the LiPF6 less than the lithium-containing imide salt.
[0075] Effects of the Invention
[0076] According to the present invention, even when a non-aqueous electrolyte solution containing acetonitrile is used, the volatility of the non-aqueous electrolyte solution is suppressed and a non-aqueous secondary battery having high ion conductivity can be provided.
[0077] Furthermore, according to the present invention, it is possible to provide a non-aqueous electrolyte solution containing acetonitrile that can realize the non-aqueous secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 It is a plan view schematically showing an example of the non-aqueous secondary battery according to the present embodiment.
[0079] Figure 2 yes Figure 1 A cross-sectional view of a non-aqueous secondary battery taken along line AA.
[0080] Figure 3 This is a scanning electron microscope (SEM) image of a microporous membrane made of polypropylene. DETAILED DESCRIPTION
[0081] Hereinafter, a mode for implementing the present invention (hereinafter referred to as "the present embodiment") is described in detail. The present invention is not limited to the following embodiments, and various modifications can be made without departing from the main purpose thereof. In this specification, the numerical range recorded using "~" includes the numerical values recorded before and after it. In the present embodiment, the upper limit value or lower limit value recorded in a certain numerical range in the staged numerical range can be replaced with the upper limit value or lower limit value of the numerical range in other staged records. In the present embodiment, the upper limit value or lower limit value recorded in a certain numerical range can also be replaced with the value recorded in the embodiment. In the present embodiment, the proportions, shapes, lengths, etc. of the various parts shown in the drawings are sometimes exaggerated to further achieve clarity.
[0082] [Non-aqueous secondary battery]
[0083] The nonaqueous secondary battery of this embodiment comprises: a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions; a negative electrode containing a material capable of absorbing and releasing lithium ions; a nonaqueous electrolyte; and a separator.
[0084] Moreover, the non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer. In a non-aqueous secondary battery having a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions, a negative electrode containing a material capable of absorbing and releasing lithium ions, a non-aqueous electrolyte and a separator, the non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer, the non-aqueous solvent contains 10 volume % or more and 90 volume % or less of acetonitrile, the lithium salt contains a lithium imide salt, and, relative to the non-aqueous electrolyte, the content of the lithium salt is 0.5 mol / L or more and 2 mol / L or less, the viscosity-average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less, the viscosity of the non-aqueous electrolyte at 25°C is 2 mPa·s or more and 500 mPa·s or less, the ion conductivity is 13 mS / cm or more, and the Z value represented by the following formula (1) is 70 or more.
[0085] Z = viscosity of electrolyte (mPa·s) × ion conductivity of electrolyte (mS / cm) (1)
[0086] According to this aspect, even when a nonaqueous electrolyte solution containing acetonitrile is used, the volatility of the nonaqueous electrolyte solution is low and a nonaqueous secondary battery having high ion conductivity can be provided.
[0087] The nonaqueous electrolyte solution of the present embodiment can be used to constitute a nonaqueous secondary battery.
[0088] The nonaqueous secondary battery of the present embodiment is configured by housing a positive electrode, a negative electrode, a separator, and a nonaqueous electrolyte in an appropriate battery casing.
[0089] Specifically, the nonaqueous secondary battery of this embodiment may be Figure 1 and 2 The non-aqueous secondary battery 100 shown. Here, Figure 1 is a top view schematically showing a non-aqueous secondary battery, Figure 2 is along Figure 1 Cross-sectional view along line AA.
[0090] Figure 1 , Figure 2 The non-aqueous secondary battery 100 shown is composed of a bag-type battery cell. The non-aqueous secondary battery 100 contains a stacked electrode body formed by stacking a positive electrode 150 and a negative electrode 160 via a separator 170 and a non-aqueous electrolyte (not shown) in a space 120 of a battery exterior 110. The battery exterior 110 is composed of, for example, an aluminum laminate film, and the upper and lower films are heat-fused to the periphery of the space formed by the two aluminum laminate films to encapsulate. The stacked body formed by stacking the positive electrode 150, the separator 170, and the negative electrode 160 in this order is impregnated with a non-aqueous electrolyte. However, in this Figure 2 In order to avoid complicating the drawing, the layers constituting the battery exterior 110 and the layers of the positive electrode 150 and the negative electrode 160 are not shown separately.
[0091] The aluminum laminate film constituting the battery exterior 110 is preferably an aluminum laminate film obtained by coating both surfaces of an aluminum foil with a polyolefin-based resin.
[0092] The positive electrode 150 is connected to the positive electrode lead 130 in the non-aqueous secondary battery 100. Although not shown, the negative electrode 160 is also connected to the negative electrode lead 140 in the non-aqueous secondary battery 100. One end of the positive electrode lead 130 and the negative electrode lead 140 are respectively led to the outside of the battery casing 110 so as to be connected to external equipment, etc., and their ionomer parts are heat-fused together with one side of the battery casing 110.
[0093] Figure 1 and 2 The positive electrode 150 and the negative electrode 160 of the non-aqueous secondary battery 100 shown in the figure each have a laminated electrode body, and the number of laminated sheets of the positive electrode 150 and the negative electrode 160 can be appropriately increased by capacity design. In the case of a laminated electrode body having a plurality of positive electrodes 150 and negative electrodes 160, the tabs of the same pole can be joined to each other by welding or the like, and then joined to a lead body by welding or the like and taken out of the battery. As the tab of the same pole, the method of forming the exposed part of the collector, the method of forming the metal sheet by welding to the exposed part of the collector, etc. can be used.
[0094] The positive electrode 150 is composed of a positive electrode current collector and a positive electrode active material layer, and the negative electrode 160 is composed of a negative electrode current collector and a negative electrode active material layer.
[0095] The positive electrode active material layer contains a positive electrode active material, and the negative electrode active material layer contains a negative electrode active material.
[0096] The positive electrode 150 and the negative electrode 160 are arranged such that the positive electrode active material layer and the negative electrode active material layer face each other via the separator 170 .
[0097] Hereinafter, each element constituting the nonaqueous secondary battery of the present embodiment will be described in order.
[0098] [positive electrode]
[0099] In the nonaqueous secondary battery of this embodiment, the positive electrode contains one or more positive electrode active materials capable of occluding and releasing lithium ions, and the positive electrode current collector may have a positive electrode active material layer on one or both surfaces as desired.
[0100] [Positive electrode collector]
[0101] The positive electrode current collector is composed of metal foil such as aluminum foil, nickel foil, stainless steel foil, etc. The positive electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the positive electrode current collector is preferably 5 μm to 40 μm, more preferably 7 μm to 35 μm, and further preferably 9 μm to 30 μm.
[0102] [Positive electrode active material layer]
[0103] The positive electrode active material layer contains a positive electrode active material, and may contain a conductive auxiliary agent and / or a binder as necessary.
[0104] (Positive electrode active material)
[0105] The positive electrode active material layer preferably contains a material capable of absorbing and releasing lithium ions as the positive electrode active material. When such a material is used, high voltage and high energy density tend to be obtained, which is preferred.
[0106] Examples of the positive electrode active material include positive electrode active materials containing at least one transition metal element selected from the group consisting of Ni, Mn and Co, and preferably at least one selected from lithium-containing metal oxides represented by the following general formula (a).
[0107] Li p Ni q Co r Mn s M t O u (a)
[0108] {Wherein, M is at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr, and Ba, and is in the range of 0<p<1.3, 0<q<1.2, 0<r<1.2, 0≤s<0.5, 0≤t<0.3, 0.7≤q+r+s+t≤1.2, and 1.8<u<2.2, and p is a value determined by the charge and discharge state of the battery}.
[0109] In addition, examples of positive electrode active materials include:
[0110] Lithium cobalt oxide represented by LiCoO2;
[0111] Lithium manganese oxides represented by LiMnO2, LiMn2O4 and Li2Mn2O4;
[0112] Lithium nickel oxide represented by LiNiO2;
[0113] LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.2 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.75 Co 0.15 Mn 0.15 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.85 Co 0.075 Mn 0.075 O2、LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.81 Co 0.1 Al 0.09 O2, and LiNi 0.85 Co 0.1 Al 0.05 O2 represented by Li z A lithium-containing composite metal oxide represented by MO2 (wherein M includes at least one transition metal element selected from the group consisting of Ni, Mn and Co, and represents two or more metal elements selected from the group consisting of Ni, Mn, Co, Al and Mg, and z represents a number greater than 0.9 and less than 1.2);
[0114] MnO2, FeO2, FeS2, V2O5, V6O 13 , TiO2, TiS2, MoS2, and NbSe2 as the representative metal oxides or metal chalcogenides with tunnel structure and layered structure;
[0115] sulfur; and
[0116] Conductive polymers represented by polyaniline, polythiophene, polyacetylene and polypyrrole; etc.
[0117] In particular, when the Ni content ratio q of the Li-containing metal oxide represented by the general formula (a) is 0.5<q<1.2, both a reduction in the amount of Co used, which is a rare metal, and a high energy density can be achieved, which is preferred.
[0118] Here, the higher the Ni content ratio of the Li-containing metal oxide, the more it tends to deteriorate under low voltage conditions. In the positive electrode active material of the lithium-containing metal oxide represented by the general formula (a), there are active sites that cause oxidative degradation of the non-aqueous electrolyte, but these active sites sometimes unintentionally consume the compound added to protect the negative electrode on the positive electrode side.
[0119] In addition, these additive decomposition products that enter the positive electrode side and accumulate not only become the main cause of the increase in the internal resistance of the non-aqueous secondary battery, but also accelerate the degradation of the lithium salt. Furthermore, the protection of the negative electrode surface becomes insufficient. In order to deactivate the active sites that substantially oxidize and degrade the non-aqueous electrolyte, it is preferred that a component that controls or neutralizes the Jahn-Teller distortion coexists. Therefore, it is preferred that the positive electrode active material contains at least one metal selected from the group consisting of Al, Sn, In, Fe, V, Cu, Mg, Ti, Zn, Mo, Zr, Sr and Ba.
[0120] For the same reasons as above, it is preferred that the surface of the positive electrode active material is coated with a compound containing at least one metal element selected from the group consisting of Zr, Ti, Al and Nb. In addition, it is more preferred that the surface of the positive electrode active material is coated with an oxide containing at least one metal element selected from the group consisting of Zr, Ti, Al and Nb. Since it does not hinder the permeation of lithium ions, it is further preferred that the surface of the positive electrode active material is coated with at least one oxide selected from the group consisting of ZrO2, TiO2, Al2O3, NbO3 and LiNbO2.
[0121] It should be noted that the positive electrode active material may be a lithium-containing compound other than the lithium-containing metal oxide represented by the general formula (a). As such a lithium-containing compound, for example, a composite oxide containing lithium and a transition metal element, a metal sulfide compound having lithium, a metal phosphate compound containing lithium and a transition metal element, and a metal silicate compound containing lithium and a transition metal element may be cited. From the viewpoint of obtaining a higher voltage, as a lithium-containing compound, in particular, a metal phosphate compound containing lithium and at least one transition metal element selected from the group consisting of Co, Ni, Mn, Fe, Cu, Zn, Cr, V and Ti is preferably used.
[0122] More specifically, examples of the lithium-containing compound include compounds represented by the following formula (XXa), the following formula (XXb), and the following formula (XXc).
[0123] Li v M I D2(XXa)
[0124] {wherein, D represents a chalcogen element, M I represents one or more transition metal elements including at least one transition metal element, and the v value is determined by the charge and discharge state of the battery and represents a number between 0.05 and 1.10.
[0125] Li w M II PO4(XXb)
[0126] {In the formula, M II Indicates one or more transition metal elements. The w value is determined by the charge and discharge state of the battery and is a number between 0.05 and 1.10.}
[0127] The following formula (XXc):
[0128] Li t M III u SiO4(XXc)
[0129] {In the formula, M III represents one or more transition metal elements, the t value is determined by the charge and discharge state of the battery and represents a number from 0.05 to 1.10, and u represents a number from 0 to 2.
[0130] The lithium-containing compound represented by the above formula (XXa) has a layered structure, and the compounds represented by the above formulas (XXb) and (XXc) have an olivine structure. For the purpose of stabilizing the structure, these lithium-containing compounds can be substances in which a part of the transition metal elements is replaced by Al, Mg or other transition metal elements, substances in which these metal elements are contained in the grain boundaries, substances in which a part of the oxygen atoms are replaced by fluorine atoms, substances in which other positive electrode active materials are coated on at least a part of the surface of the positive electrode active material, etc.
[0131] The positive electrode active material can be used alone or in combination of two or more. The positive electrode active material layer preferably contains at least one transition metal element selected from Ni, Mn and Co from the viewpoint of being able to reversibly and stably store and release lithium ions and to achieve high energy density.
[0132] When a lithium-containing compound and other positive electrode active materials are used together as the positive electrode active material, the ratio of the lithium-containing compound to the total positive electrode active material is preferably 80% by mass or more, more preferably 85% by mass or more.
[0133] (Conductive additive)
[0134] As the conductive aid, for example, graphite, carbon black represented by acetylene black and Ketjen black, and carbon fiber can be cited. The content of the conductive aid is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, relative to 100 parts by mass of the positive electrode active material.
[0135] When the content of the conductive aid is too much, the volume energy density decreases, and when the content of the conductive aid is too little, the formation of the electron conduction path becomes insufficient. In particular, compared with the negative electrode active material layer, the electron conductivity of the positive electrode active material layer is low, so when the amount of the conductive aid is insufficient, when the non-aqueous secondary battery is discharged or charged at a high current value, it becomes impossible to take out the specified battery capacity. Therefore, in applications requiring high output and / or fast charging, it is preferred to increase the content of the conductive aid within a range where the reaction based on the movement of electrons does not become a rate-regulating reaction.
[0136] (Adhesive)
[0137] Examples of the binder include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, carboxymethyl cellulose, styrene butadiene rubber, and fluororubber. The binder content is preferably 6 parts by mass or less, more preferably 0.5 to 4 parts by mass, relative to 100 parts by mass of the positive electrode active material.
[0138] [Formation of Positive Electrode Active Material Layer]
[0139] By dispersing a slurry containing a positive electrode mixture in a solvent, the positive electrode mixture is applied to the positive electrode collector and dried (removing the solvent), wherein the positive electrode mixture is a mixture of a positive electrode active material and a conductive aid and / or a binder as needed, and pressed as needed to form a positive electrode active material layer. As such a solvent, a known solvent can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.
[0140] [negative electrode]
[0141] The negative electrode in the nonaqueous secondary battery of the present embodiment contains a material capable of occluding and releasing lithium ions, and may have a negative electrode active material layer on one or both sides of the negative electrode current collector as desired.
[0142] [Negative electrode current collector]
[0143] The negative electrode current collector is composed of metal foil such as copper foil, nickel foil, stainless steel foil, etc. In addition, the negative electrode current collector may be carbon-coated on the surface or processed into a mesh shape. The thickness of the negative electrode current collector is preferably 5 to 40 μm, more preferably 6 to 35 μm, and further preferably 7 to 30 μm.
[0144] [Negative Electrode Active Material Layer]
[0145] The negative electrode active material layer contains a negative electrode active material, and may contain a conductive aid and / or a binder as necessary.
[0146] (Negative electrode active material)
[0147] As negative electrode active materials, for example, in addition to amorphous carbon (hard carbon, soft carbon); graphite such as artificial graphite and natural graphite; carbon materials represented by pyrolytic carbon, coke, glassy carbon, sintered organic polymer compounds, mesophase carbon microspheres, carbon fibers, activated carbon, carbon colloids, and carbon black, metal lithium, metal oxides, metal nitrides, lithium alloys, tin alloys, Si materials, intermetallic compounds, organic compounds, inorganic compounds, metal complexes, organic polymer compounds, etc. can be cited. The negative electrode active material can be used alone or in combination of two or more. As the above-mentioned Si material, for example, silicon, Si alloys, Si oxides, etc. can be cited.
[0148] From the viewpoint of increasing the battery voltage, it is preferred that the negative electrode active material layer contain a + ) A material that absorbs lithium ions at a lower potential is used as a negative electrode active material.
[0149] The non-aqueous electrolyte of this embodiment has the advantage of being able to suppress various deterioration phenomena accompanying the volume change of the negative electrode during repeated charge and discharge cycles even when the Si material is used as the negative electrode active material. Therefore, in the non-aqueous secondary battery of this embodiment, from the viewpoint of having a high capacity from the Si material and excellent charge and discharge cycle characteristics, it is also a preferred method to use a Si material represented by a silicon alloy as the negative electrode active material.
[0150] In this embodiment, the negative electrode active material may include Si material, particularly SiO x (wherein, 0.5≤x≤1.5). The Si material may be in any form of a crystalline, low-crystalline, or amorphous form. In addition, when the Si material is used as the negative electrode active material, it is preferred that the conductivity between the active material particles is improved if the surface of the active material is coated with a conductive material.
[0151] The working potential of silicon is about 0.5V (relative to Li / Li + ), the working potential of graphite is about 0.05V (relative to Li / Li + ), slightly higher. Therefore, when Si material is used, the risk of lithium electrolysis is reduced. Acetonitrile, a non-aqueous solvent used in the present embodiment, is likely to undergo a reduction reaction with lithium metal, causing the generation of gas. Therefore, it is preferred that the negative electrode active material that is difficult to electrolyze lithium is used in combination with a non-aqueous electrolyte containing acetonitrile.
[0152] On the other hand, the negative electrode active material with too high an operating potential has a lower energy density as a battery. Therefore, from the viewpoint of improving energy density, it is preferred that the negative electrode active material has an operating potential of 0.4 V (relative to Li / Li + ) works at lower potentials.
[0153] As the amount relative to the total amount of the negative electrode active material layer, the content of the Si material is preferably in the range of 0.1 mass % or more and 100 mass % or less, more preferably in the range of 1 mass % or more and 80 mass % or less, and further preferably in the range of 3 mass % or more and 60 mass % or less. By adjusting the content of the Si material to within the above range, the balance between the high capacity of the non-aqueous secondary battery and the charge and discharge cycle performance can be ensured.
[0154] (Conductive additive)
[0155] Examples of the conductive aid include graphite, carbon black represented by acetylene black and Ketjen black, and carbon fiber. The content of the conductive aid is preferably 20 parts by mass or less, more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the negative electrode active material.
[0156] (Adhesive)
[0157] As the binder, for example, carboxymethyl cellulose, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyacrylic acid, and fluororubber can be cited. In addition, diene rubbers such as styrene butadiene rubber can also be cited. As an amount relative to 100 parts by mass of the negative electrode active material, the content of the binder is preferably 10 parts by mass or less, and more preferably 0.5 to 6 parts by mass.
[0158] [Formation of Negative Electrode Active Material Layer]
[0159] By dispersing the negative electrode mixture in the solvent, the slurry containing the negative electrode mixture is applied to the negative electrode collector and dried (removing the solvent), wherein the negative electrode mixture is a mixture of the negative electrode active material and the conductive aid and / or binder contained as required, and pressed as required to form a negative electrode active material layer. As such a solvent, a known solvent can be used. For example, N-methyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, water, etc. can be cited.
[0160] [Non-aqueous electrolyte]
[0161] In the present specification, a "non-aqueous electrolyte solution" (hereinafter, also simply referred to as an "electrolyte solution") refers to an electrolyte solution containing 1 mass % or less of water relative to the total amount of the electrolyte solution.
[0162] The electrolyte solution of this embodiment is used for a nonaqueous secondary battery having a positive electrode containing one or more positive electrode active materials capable of occluding and releasing lithium ions, a negative electrode containing a material capable of occluding and releasing lithium ions, a nonaqueous electrolyte solution, and a separator.
[0163] Furthermore, the non-aqueous electrolyte solution contains a non-aqueous solvent, a lithium salt, and an organic polymer.
[0164] The non-aqueous solvent contains 10% by volume or more and 90% by volume or less of acetonitrile.
[0165] The lithium salt includes a lithium imide salt, and a content of the lithium salt is 0.5 mol / L or more and 2 mol / L or less relative to the non-aqueous electrolyte solution.
[0166] The viscosity average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less.
[0167] The non-aqueous electrolyte has a viscosity of 2 mPa·s or more and 500 mPa·s or less at 25° C., an ion conductivity of 13 mS / cm or more, and Z represented by the following formula (1) is 70 or more.
[0168] Z = viscosity of electrolyte (mPa·s)×ion conductivity of electrolyte (mS / cm) (1).
[0169] According to this, it is possible to provide a non-aqueous electrolyte solution containing acetonitrile that can realize the above-mentioned non-aqueous secondary battery.
[0170] Here, Z represented by formula (1) being 70 or more means that the viscosity at 25°C and the ion conductivity at 25°C are within the above ranges, respectively, and a suitable value as viscosity can be obtained, and a sufficiently high value as ion conductivity can be obtained. Such an electrolyte helps to realize the non-aqueous secondary battery of this embodiment.
[0171] Z represented by formula (1) can be derived from the product of the value of "viscosity (mPa·s)" determined by the method described in Examples and the value of "ion conductivity (mS / cm)" determined by the method described in Examples.
[0172] The electrolyte of the preferred embodiment does not contain water as much as possible, and may contain a very small amount of water as long as it does not hinder the scope of the problem to be solved by the present invention. Such a water content is less than 300 mass ppm relative to the total amount of the electrolyte, and more preferably less than 200 mass ppm. Regarding the electrolyte, as long as it has a structure for realizing the solution of the problem of the present invention, regarding other constituent elements, the constituent materials in the known electrolyte for lithium ion batteries can be appropriately selected and applied.
[0173] The electrolyte solution of the present embodiment can contain acetonitrile, a non-aqueous solvent, a lithium salt, an electrode protection additive, a surfactant, and an organic polymer.
[0174] <Non-aqueous solvent>
[0175] The "non-aqueous solvent" described in this embodiment refers to the elements other than lithium salts and various additives removed from the electrolyte. When the electrolyte contains an electrode protection additive, the "non-aqueous solvent" refers to the elements other than lithium salts and additives other than the electrode protection additive removed from the electrolyte. As the non-aqueous solvent, for example, alcohols such as methanol and ethanol; aprotic solvents, etc. can be cited. Among them, as the non-aqueous solvent, aprotic solvents are preferred. The non-aqueous solvent may also include solvents other than non-protonic solvents as long as it does not hinder the scope of the problem to be solved by the present invention.
[0176] For example, the non-aqueous solvent of the electrolyte can contain acetonitrile as a non-protonic solvent. By containing acetonitrile in the non-aqueous solvent, the ionic conductivity of the electrolyte is improved, and therefore, the diffusivity of the lithium ions in the battery can be improved. Therefore, when the electrolyte contains acetonitrile, especially in the positive electrode in which the filling amount of the positive electrode active material is increased by thickening the positive electrode active material layer, the lithium ions can also be well diffused to the area near the collector that is difficult for the lithium ions to reach during high-load discharge. Therefore, sufficient capacity can also be derived during high-load discharge, and a non-aqueous secondary battery with excellent load characteristics can be obtained.
[0177] In addition, by containing acetonitrile in the non-aqueous solvent, the rapid charging characteristics of the non-aqueous secondary battery can be improved. In the constant current (CC)-constant voltage (CV) charging of the non-aqueous secondary battery, the capacity per unit time during the CC charging period is greater than the charging capacity per unit time during the CV charging period. When acetonitrile is used in the non-aqueous solvent of the electrolyte, in addition to increasing the area where CC charging can be performed (extending the time of CC charging), the charging current can also be increased, and therefore, the time from the start of charging of the non-aqueous secondary battery to the fully charged state can be significantly shortened.
[0178] It should be noted that acetonitrile is easily decomposed by electrochemical reduction. Therefore, when using acetonitrile, preferably, as a non-aqueous solvent, other solvents (for example, aprotic solvents except acetonitrile) are used together with acetonitrile, and / or an electrode protection additive for forming a protective coating to an electrode is added.
[0179] As the amount relative to the total amount of the non-aqueous solvent, the content of acetonitrile can be 10 volume % or more and 90 volume % or less. As the amount relative to the total amount of the non-aqueous solvent, the content of acetonitrile is preferably 10 volume % or more, more preferably 15 volume % or more, more preferably 20 volume % or more, more preferably 30 volume % or more, and more preferably 40 volume % or more. This value is more preferably 85 volume % or less, and more preferably 66 volume % or less. When the amount relative to the total amount of the non-aqueous solvent, the content of acetonitrile is 10 volume % or more, there is an increase in ionic conductivity and a tendency to show high output characteristics, and further, it is possible to promote the dissolution of lithium salts. The additive described later suppresses the increase in the internal resistance of the battery, and therefore, when the content of acetonitrile in the non-aqueous solvent is within the above-mentioned range, there is a tendency to keep the excellent performance of acetonitrile and to make high temperature cycle characteristics and other battery characteristics better. On the other hand, as the content of acetonitrile increases, the electrolyte becomes easily volatile, and therefore, the electrolyte amount is insufficient in the process of manufacturing non-aqueous secondary batteries, which may have an adverse effect on battery characteristics. Adding an organic polymer described below contributes to the improvement of volatility.
[0180] As the aprotic solvent other than acetonitrile, for example, cyclic carbonates, fluoroethylene carbonates, lactones, organic compounds having sulfur atoms, chain fluorinated carbonates, cyclic ethers, mononitriles other than acetonitrile, alkoxy-substituted nitriles, dinitriles, cyclic nitriles, short-chain fatty acid esters, chain ethers, fluorinated ethers, ketones, compounds in which a part or all of the H atoms of the aprotic solvent are substituted with halogen atoms, etc. can be cited.
[0181] Examples of the cyclic carbonate include ethylene carbonate, propylene carbonate, 1,2-butenyl carbonate, trans-2,3-butenyl carbonate, cis-2,3-butenyl carbonate, 1,2-pentenyl carbonate, trans-2,3-pentenyl carbonate, cis-2,3-pentenyl carbonate, vinylene carbonate, 4,5-dimethylvinylene carbonate, and vinyl ethylene carbonate;
[0182] Examples of the fluoroethylene carbonate include 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one.
[0183] Examples of lactones include γ-butyrolactone, α-methyl-γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone;
[0184] Examples of the organic compound having a sulfur atom include ethylene sulfite, propylene sulfite, butylene sulfite, pentenyl sulfite, sulfolane, 3-butylene sulfite, 3-methylsulfolane, 1,3-propane sultone, 1,4-butane sultone, 1-propylene-1,3-sultone, dimethyl sulfoxide, tetramethylene sulfoxide, and ethylene glycol sulfite;
[0185] Examples of the chain carbonate include ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, methyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, methyl butyl carbonate, dibutyl carbonate, and ethyl propyl carbonate;
[0186] Examples of the cyclic ether include tetrahydrofuran, 2-methyltetrahydrofuran, 1,4-dioxane, and 1,3-dioxane;
[0187] Examples of mononitriles other than acetonitrile include propionitrile, butyronitrile, valeronitrile, benzonitrile, and acrylonitrile;
[0188] Examples of the alkoxy-substituted nitrile include methoxyacetonitrile and 3-methoxypropionitrile;
[0189] Examples of the dinitriles include malononitrile, succinonitrile, glutaronitrile, adiponitrile, 1,4-dicyanoheptane, 1,5-dicyanopentane, 1,6-dicyanohexane, 1,7-dicyanoheptane, 2,6-dicyanoheptane, 1,8-dicyanooctane, 2,7-dicyanooctane, 1,9-dicyanononane, 2,8-dicyanononane, 1,10-dicyanodecane, 1,6-dicyanodecane, and 2,4-dimethylglutaronitrile;
[0190] As the cyclic nitrile, for example, benzonitrile can be mentioned;
[0191] Examples of the short-chain fatty acid esters include methyl acetate, methyl propionate, methyl isobutyrate, methyl butyrate, methyl isovalerate, methyl valerate, methyl pivalate, methyl 2-methylbutyrate, methyl hexanoate, ethyl acetate, ethyl propionate, ethyl isobutyrate, ethyl butyrate, ethyl isovalerate, ethyl valerate, ethyl pivalate, ethyl 2-methylbutyrate, ethyl hexanoate, propyl acetate, propyl propionate, propyl isobutyrate, propyl butyrate, propyl isovalerate, propyl valerate, propyl pivalate, propyl 2-methylbutyrate, propyl hexanoate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, propyl valerate, propyl pivalate, propyl 2-methylbutyrate, propyl hexanoate, isopropyl acetate, isopropyl propionate, isopropyl isobutyrate, isopropyl butyrate, isopropyl isovalerate, isopropyl valerate, isopropyl pivalate, isopropyl 2-methylbutyrate, isopropyl hexanoate, butyl acetate, butyl propionate, butyl isobutyrate, butyl butyrate, butyl isovalerate, butyl valerate, butyl pivalate, butyl 2-methylbutyrate, butyl hexanoate, isobutyl acetate, isobutyl propionate, isobutyl isobutyrate, isobutyl butyrate, isobutyl isovalerate, isobutyl valerate, isobutyl pivalate, isobutyl 2-methylbutyrate, isobutyl hexanoate, tert-butyl acetate, tert-butyl propionate, tert-butyl isobutyrate, tert-butyl butyrate, tert-butyl isovalerate, tert-butyl valerate, tert-butyl pivalate, tert-butyl 2-methylbutyrate, and tert-butyl hexanoate;
[0192] Examples of the chain ether include dimethoxyethane, diethyl ether, 1,3-dioxolane, diethylene glycol dimethyl ether (diglyme), triethylene glycol trimethyl ether (triglyme), and tetraethylene glycol dimethyl ether (tetraglyme);
[0193] Examples of the fluorinated ether include Rf aa -OR bb (Where Rf aa represents an alkyl group containing a fluorine atom, and R bb represents an organic group that may contain fluorine atoms);
[0194] Examples of ketones include acetone, methyl ethyl ketone, and methyl isobutyl ketone;
[0195] Examples of the compound in which a part or all of the H atoms of the aprotic solvent are substituted with halogen atoms include compounds in which the halogen atom is fluorine; and the like.
[0196] Here, as the fluoride of linear carbonate, for example, can enumerate methyl trifluoroethyl carbonate, dimethyl trifluorocarbonate, diethyl trifluorocarbonate, methyl ethyl trifluorocarbonate, methyl 2,2-difluoroethyl carbonate, methyl 2,2,2-trifluoroethyl carbonate, methyl 2,2,3,3-tetrafluoropropyl carbonate.Above-mentioned fluorinated linear carbonate can be represented by following general formula.
[0197] R cc -OC(O)OR dd
[0198] (Where R cc and R dd It is composed of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, and CH2Rf ee At least one selected from the group consisting of ee is an alkyl group having 1 to 3 carbon atoms in which at least one fluorine atom replaces a hydrogen atom, and R cc and / or R dd contains at least one fluorine atom).
[0199] Examples of the fluorinated short-chain fatty acid ester include fluorinated short-chain fatty acid esters represented by 2,2-difluoroethyl acetate, 2,2,2-trifluoroethyl acetate, and 2,2,3,3-tetrafluoropropyl acetate. The fluorinated short-chain fatty acid ester can be represented by the following general formula.
[0200] R ff -C(O)OR gg
[0201] (Where R ff It is made of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, CF3CF2H, CFH2, CF2Rf hh CFHRf hh and CH2Rf ii At least one selected from the group consisting of gg It is composed of CH3, CH2CH3, CH2CH2CH3, CH(CH3)2, and CH2Rf ii At least one selected from the group consisting of hh is an alkyl group having 1 to 3 carbon atoms which may be formed by replacing a hydrogen atom with at least one fluorine atom, Rf ii is an alkyl group having 1 to 3 carbon atoms in which at least one fluorine atom replaces a hydrogen atom, and R ffand / or R gg Contains at least one fluorine atom, when R ff When it is CF2H, R gg Not CH3).
[0202] The aprotic solvent other than acetonitrile in the present embodiment may be used alone or in combination of two or more.
[0203] From the viewpoint that improves the stability of nonaqueous electrolyte, the nonaqueous solvent in the present embodiment preferably uses more than one in cyclic carbonate and the linear carbonate with acetonitrile.From this viewpoint, the nonaqueous solvent in the present embodiment more preferably uses cyclic carbonate and acetonitrile, further preferably uses cyclic carbonate and linear carbonate with acetonitrile.
[0204] When a cyclic carbonate is used together with acetonitrile, it is particularly preferred that the cyclic carbonate comprises ethylene carbonate, vinylene carbonate and / or fluoroethylene carbonate.
[0205] <Lithium salt>
[0206] The electrolyte solution of this embodiment contains a lithium salt. The content of the lithium salt may be 0.5 mol / L or more and 2 mol / L or less relative to the electrolyte solution.
[0207] The lithium salt in this embodiment includes a lithium-containing imide salt as an imide salt, and the lithium-containing imide salt is preferably composed of LiN(SO2C m F 2m+1 )2{wherein, m is an integer from 0 to 8} represented by an imide salt.
[0208] The lithium salt in this embodiment may further include an imide salt and one or more selected from fluorine-containing inorganic lithium salts, organic lithium salts, and other lithium salts.
[0209] (Imide salt)
[0210] Specifically, the imide salt preferably contains at least one of LiN(SO2F)2 and LiN(SO2CF3)2.
[0211] When acetonitrile is included in the non-aqueous solvent, the lithium salt preferably includes LiPF6, and the saturation concentration of the imide salt relative to acetonitrile is higher than the saturation concentration of LiPF6. Therefore, it is preferred to include LiPF6 and the imide salt at a molar concentration of LiPF6 ≤ imide salt, which can inhibit the association and precipitation of the lithium salt and acetonitrile under low temperature conditions. In particular, it is preferred to include the imide salt and LiPF6 at a molar concentration of LiPF6 < imide salt. In addition, as an amount relative to 1L of non-aqueous solvent, the content of the imide salt is preferably 0.5 mol or more and 2.0 mol or less, and from the viewpoint of ensuring the ion supply amount of the electrolyte solution of this embodiment, it is particularly preferably 0.8 mol or more and 1.5 mol or less.
[0212] When the content of the lithium salt is within the above range, high ion conductivity can be maintained. The ion conductivity is preferably 13 mS / cm or more, more preferably 15 mS / cm or more, and preferably 18 mS / cm or more from the viewpoint of maintaining the output performance of the non-aqueous secondary battery of the present embodiment. The ion conductivity may be, for example, 300 mS / cm or less, 150 mS / cm or less, or 75 mS / cm or less.
[0213] According to the acetonitrile-containing electrolyte containing at least one of LiN(SO2F)2 and LiN(SO2CF3)2, the decrease in ion conductivity in a low temperature range such as -10°C or -30°C can be effectively suppressed, and excellent low temperature characteristics can be obtained.
[0214] Furthermore, as described above, by limiting the content of the imide salt and / or LiPF6, the increase in resistance during high-temperature heating can also be more effectively suppressed.
[0215] (Fluorine-containing inorganic lithium salt)
[0216] The lithium salt in this embodiment may also include a fluorine-containing inorganic lithium salt. Here, "fluorine-containing inorganic lithium salt" refers to a lithium salt that does not contain carbon atoms in the anion, contains fluorine atoms in the anion, and is soluble in acetonitrile. The fluorine-containing inorganic lithium salt forms a passivation film on the surface of the positive electrode collector and is excellent in inhibiting corrosion of the positive electrode collector.
[0217] Examples of fluorine-containing inorganic lithium salts include LiPF6, LiBF4, LiAsF6, Li2SiF6, LiSbF6, Li2B 12 F b H 12-b {wherein b represents an integer of 0 to 3} etc., and one or more selected from these can be used.
[0218] As the fluorine-containing inorganic lithium salt, a compound as a double salt of LiF and a Lewis acid is preferred, wherein, if a fluorine-containing inorganic lithium salt having a phosphorus atom is used, free fluorine atoms are easily released, and thus it is more preferred. A representative fluorine-containing inorganic lithium salt is LiPF6 which dissolves and releases PF6 anions. When a fluorine-containing inorganic lithium salt having a boron atom is used as the fluorine-containing inorganic lithium salt, it is easy to capture excess free acid components that may cause battery degradation, and thus it is preferred. From this point of view, LiBF4 is preferred.
[0219] As the amount relative to 1L of non-aqueous solvent, the content of the fluorinated inorganic lithium salt in the electrolyte of the present embodiment is preferably 0.01 mole or more, more preferably 0.1 mole or more, and further preferably 0.25 mole or more. When the content of the fluorinated inorganic lithium salt is within the above range, there is a tendency that the ion conductivity increases and can exhibit high output characteristics. In addition, the amount relative to 1L of non-aqueous solvent is preferably 2.8 moles or less, more preferably 1.5 moles or less, and further preferably 1.0 moles or less. When the content of the fluorinated inorganic lithium salt is within the above range, there is a tendency that the ion conductivity increases and can exhibit high output characteristics and can suppress the decrease in ion conductivity associated with the increase in viscosity under low temperature conditions, and there is a tendency that the high temperature cycle characteristics and other battery characteristics can be made better while maintaining the excellent performance of the electrolyte.
[0220] The content of the fluorine-containing inorganic lithium salt in the electrolytic solution of the present embodiment may be, for example, 0.05 mol or more and 1.0 mol or less per 1 L of the non-aqueous solvent.
[0221] (Organic lithium salt)
[0222] The lithium salt in this embodiment may include an organic lithium salt. The "organic lithium salt" refers to a lithium salt other than an imide salt that contains a carbon atom in the anion and is soluble in acetonitrile.
[0223] As an organic lithium salt, an organic lithium salt having an oxalic acid group can be cited. As a specific example of an organic lithium salt having an oxalic acid group, for example, organic lithium salts represented by LiB(C2O4)2, LiBF2(C2O4), LiPF4(C2O4) and LiPF2(C2O4)2 can be cited, among which at least one lithium salt selected from lithium salts represented by LiB(C2O4)2 and LiBF2(C2O4) is preferred. In addition, it is more preferred to use one or more of them together with a fluorine-containing inorganic lithium salt. In addition to being added to the electrolyte, the organic lithium salt having an oxalic acid group can also be included in the negative electrode (negative electrode active material layer).
[0224] From the viewpoint of better ensuring the effect of its use, as the amount relative to 1L of non-aqueous solvent, the amount of the organic lithium salt added to the electrolyte in the present embodiment is preferably 0.005 mol or more, more preferably 0.01 mol or more, further preferably 0.02 mol or more, and particularly preferably 0.05 mol or more. However, when the amount of the organic lithium salt having an oxalic acid group in the electrolyte is too much, it is possible to precipitate. Therefore, as the amount relative to 1L of non-aqueous solvent, the amount of the organic lithium salt having an oxalic acid group added to the electrolyte is preferably less than 1.0 mol, more preferably less than 0.5 mol, and more preferably less than 0.2 mol.
[0225] It is known that organic lithium salts having oxalic acid groups are poorly soluble in low-polarity organic solvents, particularly chain carbonates. The content of the organic lithium salt in the electrolyte of this embodiment may be, for example, 0.01 mol or more and 0.5 mol or less relative to 1 L of the non-aqueous solvent.
[0226] It should be noted that the organic lithium salt having an oxalate group sometimes contains a trace amount of lithium oxalate, and further, when mixed as an electrolyte, sometimes reacts with a trace amount of water contained in other raw materials to produce a new white precipitate of lithium oxalate. Therefore, it is preferred to suppress the content of lithium oxalate in the electrolyte of this embodiment to a range below 500ppm.
[0227] (Other lithium salts)
[0228] The lithium salt in this embodiment may include other lithium salts in addition to the above.
[0229] Specific examples of other lithium salts include:
[0230] LiClO4, LiAlO4, LiAlCl4, LiB 10 Cl 10 , inorganic lithium salts whose anions do not contain fluorine atoms, such as lithium chloroborane;
[0231] LiCF3SO3, LiCF3CO2, Li2C2F4(SO3)2, LiC(CF3SO2)3, LiC n F (2n+1) SO3 (where n≥2), organic lithium salts such as lower aliphatic carboxylic acid Li, tetraphenylborate Li, LiB(C3O4H2)2;
[0232] LiPF5(CF3) and other n (C p F 2p+1 ) 6-n [wherein n is an integer of 1 to 5, and p is an integer of 1 to 8] an organic lithium salt represented by;
[0233] LiBF3(CF3) etc. q (C s F 2s+1 ) 4-q [wherein q is an integer of 1 to 3, and s is an integer of 1 to 8] an organic lithium salt represented by;
[0234] Lithium salts combined with polyvalent anions;
[0235] Organic lithium salts represented by the following formula (YYa), the following formula (YYb) and the following formula (YYc), etc.,
[0236] LiC(SO2R jj )(SO2R kk )(SO2R ll )(YYa)
[0237] {In the formula, R jj , R kk and R ll may be the same as or different from each other, and represent a perfluoroalkyl group having 1 to 8 carbon atoms},
[0238] LiN(SO2OR mm )(SO2OR nn )(YYb)
[0239] {In the formula, R mm and R nn may be the same as or different from each other, and represent a perfluoroalkyl group having 1 to 8 carbon atoms}, and
[0240] LiN(SO2R oo )(SO2OR pp )(YYc)
[0241] {In the formula, R oo and R pp may be the same as or different from each other, and represent a perfluoroalkyl group having 1 to 8 carbon atoms},
[0242] One or two or more of these can be used together with the fluorine-containing inorganic lithium salt.
[0243] The amount of other lithium salt added to the electrolyte solution can be appropriately set, for example, in the range of 0.01 mol to 0.5 mol, both inclusive, relative to 1 L of the non-aqueous solvent.
[0244] <Electrode protection additives>
[0245] The electrolyte of this embodiment may include an additive for protecting the electrode (electrode protection additive). The electrode protection additive may substantially overlap with the substance that acts as a solvent for dissolving the lithium salt (i.e., the above-mentioned non-aqueous solvent). The electrode protection additive is preferably a substance that helps to improve the performance of the electrolyte and the non-aqueous secondary battery, but also includes substances that do not directly participate in the electrochemical reaction.
[0246] Specific examples of electrode protection additives include: fluoroethylene carbonate represented by 4-fluoro-1,3-dioxolane-2-one, 4,4-difluoro-1,3-dioxolane-2-one, cis-4,5-difluoro-1,3-dioxolane-2-one, trans-4,5-difluoro-1,3-dioxolane-2-one, 4,4,5-trifluoro-1,3-dioxolane-2-one, 4,4,5,5-tetrafluoro-1,3-dioxolane-2-one, and 4,4,5-trifluoro-5-methyl-1,3-dioxolane-2-one; vinylene carbonate, 4,5-dimethylvinyl carbonate; The present invention also includes cyclic carbonates containing unsaturated bonds represented by esters and vinyl carbonate; lactones represented by γ-butyrolactone, γ-valerolactone, γ-caprolactone, δ-valerolactone, δ-caprolactone, and ε-caprolactone; cyclic ethers represented by 1,4-dioxane; cyclic sulfur compounds represented by vinyl sulfite, propylene sulfite, butylene sulfite, pentylene sulfite, cyclopentane sulfone, 3-cyclobutene sulfone, 3-methylcyclopentane sulfone, 1,3-propane sultone, 1,4-butane sultone, 1-propylene-1,3-sultone, and tetramethylene sulfoxide, and these may be used alone or in combination of two or more.
[0247] The content of the electrode protection additive in the electrolyte solution is preferably 0.1 to 30 volume %, more preferably 0.3 to 15 volume %, and particularly preferably 0.4 to 10 volume %, relative to the total amount of the non-aqueous solvent.
[0248] In the present embodiment, the more the content of the electrode protection additive is, the more the degradation of the electrolyte is suppressed. However, the less the content of the electrode protection additive is, the more the high output characteristics of the non-aqueous secondary battery in a low temperature environment are improved. Therefore, by adjusting the content of the electrode protection additive to the above range, there is a tendency to be able to exert excellent performance based on the high ion conductivity of the electrolyte without damaging the basic function of the non-aqueous secondary battery. In addition, by preparing the electrolyte with such a composition, there is a tendency to make the cycle performance of the non-aqueous secondary battery, the high output performance in a low temperature environment and other battery characteristics better.
[0249] Acetonitrile is easily decomposed by electrochemical reduction. Therefore, the non-aqueous solvent containing acetonitrile preferably contains one or more cyclic aprotic polar solvents as electrode protective additives for forming a protective film for the negative electrode, and more preferably contains one or more cyclic carbonates containing unsaturated bonds.
[0250] As the cyclic carbonate containing unsaturated bonds, vinylene carbonate is preferred, and the content of vinylene carbonate in the electrolyte is preferably 0.1 volume % or more and 10 volume % or less, more preferably 0.2 volume % or more and less than 8 volume %, and further preferably 0.5 volume % or more and less than 6 volume %. Thus, the low-temperature durability can be more effectively improved, and a secondary battery with excellent low-temperature performance can be provided.
[0251] Vinylene carbonate as electrode protection additive suppresses the reduction decomposition reaction of acetonitrile on negative electrode surface.On the other hand, excessive film formation can cause the decline of low temperature performance.Therefore, by adjusting the addition of vinylene carbonate to the above-mentioned range, interface (film) resistance can be suppressed to be relatively low, and the cycle degradation during low temperature can be suppressed.
[0252] <Acid anhydride>
[0253] The non-aqueous secondary battery of the present embodiment decomposes a portion of the electrolyte during the initial charge, and forms a SEI (Solid Electrolyte Interface) on the negative electrode surface and is stabilized. In order to more effectively strengthen the SEI, anhydrides can be added. In the case of acetonitrile as a non-aqueous solvent, there is a tendency that the strength of SEI decreases with increasing temperature, and the addition of anhydrides promotes the strengthening of SEI. Therefore, by using such anhydrides, the increase in internal resistance over time caused by thermal processes can be effectively suppressed.
[0254] Specific examples of the acid anhydride include, for example, chain anhydrides represented by acetic anhydride, propionic anhydride, and benzoic anhydride; cyclic anhydrides represented by malonic anhydride, succinic anhydride, glutaric anhydride, maleic anhydride, phthalic anhydride, 1,2-cyclohexanedicarboxylic anhydride, 2,3-naphthalene dicarboxylic anhydride, or naphthalene-1,4,5,8-tetracarboxylic dianhydride; and mixed anhydrides having a structure formed by dehydration condensation of two different carboxylic acids or different types of acids such as carboxylic acid and sulfonic acid. These may be used alone or in combination of two or more.
[0255] The non-aqueous secondary battery of the present embodiment preferably strengthens SEI before the reduction decomposition of the non-aqueous solvent, therefore, as anhydride, preferably comprises at least one cyclic anhydride that plays a role in the early stage during the initial charge. These cyclic anhydrides can only comprise one or a plurality of species. Alternatively, cyclic anhydrides other than these cyclic anhydrides may also be included. In addition, preferably the cyclic anhydride comprises at least one of succinic anhydride, maleic anhydride and phthalic anhydride.
[0256] According to the electrolyte containing at least one of succinic anhydride, maleic anhydride and phthalic anhydride, a strong SEI can be formed at the negative electrode, and the resistance increase during high-temperature heating can be more effectively suppressed. In particular, it is preferred to contain succinic anhydride. Thus, a strong SEI can be more effectively formed at the negative electrode while suppressing side reactions.
[0257] When the electrolyte solution of this embodiment contains an acid anhydride, its content is preferably in the range of 0.01 mass part to 10 mass parts, more preferably 0.05 mass part to 1 mass part, and further preferably 0.1 mass part to 0.5 mass part, relative to 100 mass parts of the electrolyte solution.
[0258] <Optional additives>
[0259] In this embodiment, for the purpose of improving the charge and discharge cycle characteristics of the non-aqueous secondary battery, enhancing high-temperature storage properties, safety (for example, preventing overcharging, etc.), etc., any additives (acid anhydrides and additives other than electrode protection additives) may be appropriately included in the electrolyte.
[0260] As optional additives, for example, sulfonic acid esters, diphenyl disulfide, cyclohexylbenzene, biphenyl, fluorobenzene, tert-butylbenzene, nitrogen-containing cyclic compounds having no steric hindrance around non-covalent electron pairs (pyridine, 1-methyl-1H-benzotriazole, 1-methylpyrazole, etc.), etc. Phosphoric acid esters are particularly effective as optional additives because they have the effect of suppressing side reactions during storage.
[0261] When the electrolyte of the present embodiment contains any other additives, the content thereof is preferably in the range of 0.01 mass % to 10 mass % relative to the total amount of the electrolyte, more preferably in the range of 0.02 mass % to 5 mass %, and further preferably in the range of 0.05 to 3 mass %. By adjusting the content of any other additives within the above range, there is a tendency to be able to add better battery characteristics without damaging the basic function as a non-aqueous secondary battery.
[0262] <Surfactant>
[0263] The electrolyte of the present embodiment may contain a surfactant. In the present embodiment, the surfactant is a compound having one or more hydrophilic groups and one or more lipophilic groups in one molecule. As surfactants, there are anionic surfactants, cationic surfactants, amphoteric surfactants and nonionic surfactants. Ionized surfactants are limited to surfactants that do not hinder the insertion and detachment of lithium ions into the negative electrode. In addition, from the viewpoint of the solubility of the electrolyte, nonionic surfactants are also preferred as surfactants.
[0264] Examples of the nonionic surfactant include fatty acid ester compounds such as glycerol fatty acid esters, sorbitan fatty acid esters, sucrose fatty acid esters, and saturated fatty acid esters; ethyl diethylphosphonoacetate {EDPA; (C2H5O)2(P=O)-CH2(C=O)OC2H5}, tri(trifluoroethyl) phosphate {TFEP; (CF3CH2O)3P=O}, triphenyl phosphate {TPP; (C6H5O)3P=O}, triallyl phosphate {CH2= Phosphate ester compounds such as triamyl phosphate, tris(2-butoxyethyl) phosphate and tris(2-ethylhexyl) phosphate; ether compounds such as polyoxyethylene alkyl ether, polyoxyalkylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene polycyclic phenyl ether, polyoxyethylene distyrenated phenyl ether, polyoxyethylene-polyoxypropylene glycol; ester ether compounds such as fatty acid polyethylene glycol and polyoxyethylene sorbitan fatty acid ester; alkanolamide compounds such as fatty acid alkanolamide. From the viewpoint of improving the stability of the electrolyte, fatty acid ester compounds or phosphate ester compounds are preferred. As the fatty acid ester compound, ethyl laurate is preferred. In particular, phosphate ester compounds are preferred, among which at least one selected from the group consisting of triamyl phosphate, tris(2-butoxyethyl) phosphate and tris(2-ethylhexyl) phosphate is more preferred, and tris(2-ethylhexyl) phosphate is particularly preferred.
[0265] The number of carbon atoms contained in at least one substituent constituting the hydrophobic part of the nonionic surfactant is preferably 3 or more, and from the viewpoint of reducing the surface tension of the electrolyte, it is more preferably 5 or more, and further preferably 8 or more. In addition, from the viewpoint that the boiling point of the compound becomes high when the number of carbon atoms of the substituent is large, and it is difficult to purify, the number of carbon atoms contained in the substituent is preferably 25 or less, and further preferably 20 or less. In the case of a branched hydrocarbon chain of the substituent, it is set to the total number of carbon atoms contained in the substituent. As a substituent having a carbon number of 3 or more, specifically, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, isopentyl, sec-pentyl, tert-pentyl, 2-butoxyethyl, 2-ethylhexyl, phenyl, etc. can be cited.
[0266] In the present embodiment, the content of surfactant is 0.1% by mass or more and 3% by mass or less relative to the total amount of the electrolyte. Relative to the total amount of the electrolyte, from the viewpoint of improving impregnation, the content of surfactant is more preferably 0.3% by mass or more, and from the viewpoint of maintaining high ionic conductivity, more preferably 2% by mass or less. Similarly, relative to the total amount of the electrolyte, the content of nonionic surfactant is preferably 0.1% by mass or more and 3% by mass or less, more preferably 0.3% by mass or more and 2% by mass or less. If the content of surfactant or nonionic surfactant is more than 0.1% by mass, the effect of suppressing output decline can be obtained more effectively, and if the content is less than 3% by mass, the decline in ionic conductivity is less, and the impact on battery characteristics such as input-output characteristics and battery life becomes less.
[0267] Here, the content of the surfactant can be determined by the electrolyte at room temperature. 1 It was determined by H-NMR measurement (standardization with a standard substance (C6F4H2) and calculation of the surfactant content from the integrated value of the signal of each component detected).
[0268] The inventor has conducted intensive research and found that if the surfactant contains hydroxyl groups, the impregnation of the spacer is improved. On the other hand, it is easy to reduce and decompose at the negative electrode during charging, which becomes the cause of the degradation of battery performance. Further, it is newly discovered that when the surfactant contains hydroxyl groups, bubbles are easily generated in the decompression process after the electrolyte is injected. If the initial charge is performed in a state where the bubbles are not completely discharged, SEI cannot be uniformly formed on the negative electrode surface, resulting in poor initial charge and discharge. The electrolyte containing acetonitrile uniformly forms SEI during the initial charge, so that subsequent charge and discharge actions can be performed. Therefore, when the generation of bubbles leads to an insufficient part of SEI formation during the initial charge, the electrolyte containing acetonitrile is directly related to the poor initial charge or the decline in battery life compared to the electrolyte without acetonitrile. Therefore, in more detail, it is important that the surfactant of the present embodiment does not contain hydroxyl groups in the substituents at the end as substituents.
[0269] <Organic polymer>
[0270] From the viewpoint of preventing the volatilization of the electrolyte, the electrolyte of the present embodiment can contain an organic polymer. As an organic polymer, it is limited to a substance that does not excessively hinder the insertion and separation of lithium ions into the negative electrode. In addition, from the viewpoint of the solubility of the electrolyte, as an organic polymer, it is preferred to have at least one of a polyether structure and an ester structure.
[0271] Examples of organic polymers having a polyether structure include polyethylene oxide, polypropylene oxide, polyethylene glycol monododecyl ether, polyethylene glycol mono-4-nonylphenyl ether, polyethylene glycol monooleyl ether, polyethylene glycol monohexadecyl ether, poly(ethylene glycol) methacrylate, poly(ethylene glycol) diacrylate, poly(ethylene glycol) distearate, O-[(N-succinimidyl) succinyl-aminoethyl]-O'-methyl polyethylene glycol, O-[2-(3-mercaptopropionylamino)ethyl]-O'-methyl polyethylene glycol, poly(ethylene glycol) bis(3-aminopropyl), poly(ethylene glycol) methyl ether, methoxypolyethylene glycol amine, methoxypolyethylene epoxide, poly(ethylene glycol) bis(carboxymethyl) ether, poly(ethylene glycol) dimethyl ether, poly(ethylene glycol) bis(amine), and poly(ethylene glycol) methyl ether acetylene. As organic polymers having an ester structure, poly(methyl methacrylate), poly(ethyl methacrylate), poly(isopropyl methacrylate), poly(tert-butyl acrylate), isobutyl methacrylate (polymer), poly(ethylene glycol) monomethyl ether monomethacrylate, etc. can be cited. One of them can be used alone, or two or more can be used in combination. For example, the organic polymer can include at least one of polyethylene oxide and poly(methyl methacrylate). In addition, the organic polymer can have a branched structure such as a multi-branched structure, and a copolymer such as a block copolymer and a random copolymer can also be used.
[0272] The content of the organic polymer can be 0.1% by mass or more and 10% by mass or less relative to the total amount of the electrolyte. From the viewpoint of improving volatility, it is preferably 0.3% by mass or more, and more preferably 0.5% by mass or more. In addition, from the viewpoint of suppressing the decline in impregnation, it is preferably 6% by mass or less, and more preferably 3% by mass or less.
[0273] The viscosity average molecular weight of the organic polymer is 30,000 to 1,000,000. The viscosity average molecular weight may be 40,000 to 70,000 or 90,000. In addition, from the viewpoint of suppressing the decrease in impregnation properties, the viscosity average molecular weight is preferably 800,000 or less, and more preferably 650,000 or less.
[0274] When the content and viscosity-average molecular weight of the organic polymer are within the above range, the viscosity of the electrolyte can be increased and high ion conductivity can be easily maintained. By increasing the viscosity of the electrolyte, the fluidity of the electrolyte can be easily reduced, and therefore, the heat transfer rate and the diffusion rate in the liquid phase can be easily suppressed. From the viewpoint of suppressing volatility in the process of making non-aqueous secondary batteries, the viscosity at 25°C is preferably 2mPa·s or more, more preferably 3mPa·s or more, and further preferably 4mPa·s or more. In addition, from the viewpoint of suppressing the decrease in impregnation of electrodes and separators, etc., it is preferably 500mPa·s or less, preferably 200mPa·s or less, and further preferably 100mPa·s or less. From the viewpoint of maintaining the output performance of non-aqueous secondary batteries, the ion conductivity at 25°C is preferably 13mS / cm or more, more preferably 15mS / cm or more, and further preferably 18mS / cm or more.
[0275] <Spacer>
[0276] The separator of this embodiment is a member disposed between a plurality of electrodes in a power storage device and having ion permeability and, if necessary, shutdown characteristics. The separator includes a microporous film and / or a microporous laminated film, and may further have an optional functional layer as desired.
[0277] The separator needs to have insulation and ion permeability, and therefore, is usually formed of an insulating material having a porous structure, i.e., paper, a polyolefin nonwoven fabric, or a resin microporous film. In particular, when the separator is used in an electrolyte secondary battery having a positive electrode and a negative electrode capable of absorbing and releasing lithium and an electrolyte obtained by dissolving an electrolyte in a non-aqueous solvent, the separator is excellent in terms of resistance to redox degradation and in terms of being able to construct a dense and uniform porous structure as a separator substrate. Therefore, the separator of the present embodiment can include a polyolefin microporous film.
[0278] The separator of the present embodiment is a microporous film containing at least one of polyethylene and polypropylene, and may have a porous layer containing an inorganic filler on one or both surfaces of the microporous film.
[0279] In the present embodiment, as the polyolefin resin of the material used as the substrate, for example, homopolymers such as polyethylene and polypropylene, a plurality of copolymers of the monomers constituting each homopolymer, and mixtures of these polymers can be cited. As polyethylene, low-density, medium-density and high-density polyethylene can be cited, and from the viewpoint of puncture strength or mechanical strength, high-density polyethylene is preferred. In addition, for the purpose of imparting flexibility, these polyethylenes can be mixed with two or more. The polymerization catalyst used when manufacturing these polyethylenes is not particularly limited either, for example, Ziegler-Natta catalysts, Phillips catalysts and metallocene catalysts can be cited. From the viewpoint of taking into account high mechanical strength and high permeability, the viscosity-average molecular weight of polyethylene is preferably more than 100,000 and less than 12 million, more preferably more than 200,000 and less than 3 million.
[0280] The microporous membrane of this embodiment may be a microporous laminated membrane as desired. The microporous laminated membrane refers to a multilayer membrane having a plurality of polyolefin-based microporous layers laminated thereon or a composite microporous membrane having a polyolefin-based microporous membrane and a microporous membrane containing another resin laminated thereon, and may be referred to as a laminated body hereinafter.
[0281] The method for preparing the substrate containing the polyolefin-based resin as a main component may be a known method. Examples of the preparation method include a dry preparation method and a wet preparation method.
[0282] In the dry preparation method, for example, first, a polyolefin resin such as polypropylene or polyethylene is formed into a film by melt extrusion, then the film is annealed at a low temperature to grow a crystalline region, and in this state, the amorphous region is stretched to form a microporous film as a substrate.
[0283] In the wet production method, for example, a hydrocarbon solvent and other low-molecular-weight materials are first mixed with a polyolefin resin such as polypropylene or polyethylene and then formed into a film. Then, other volatile solvents are used to remove the solvent and low-molecular-weight materials from the film where they aggregate in the amorphous phase and begin to form an island phase, thereby forming a microporous membrane as a substrate.
[0284] For the purpose of controlling strength, hardness, and thermal shrinkage, a porous layer containing an inorganic filler may be disposed on at least one surface of the substrate used in this embodiment. In addition, the porous layer may also contain an organic filler and a fiber compound.
[0285] As an inorganic filler, there is no particular limitation, and preferably a substance with high heat resistance and electrical insulation and electrochemical stability within the use range of lithium ion secondary batteries. As an inorganic filler, for example, aluminum compounds, magnesium compounds and other compounds can be cited. As an aluminum compound, for example, aluminum oxide, aluminum silicate, aluminum hydroxide, basic aluminum oxide, sodium aluminate, aluminum sulfate, aluminum phosphate, hydrotalcite, etc. can be cited. As a magnesium compound, for example, magnesium sulfate, magnesium hydroxide, etc. can be cited. As other compounds, oxide-based ceramics, nitride-based ceramics, clay minerals, silicon carbide, calcium carbonate, barium titanate, asbestos, zeolite, calcium silicate, magnesium silicate, diatomaceous earth, silica sand, glass fiber, etc. can be cited. As oxide-based ceramics, silicon dioxide, titanium dioxide, zirconium oxide, magnesium oxide, cerium oxide, yttrium oxide, zinc oxide, iron oxide, etc. can be cited. As nitride-based ceramics, silicon nitride, titanium nitride, boron nitride, etc. can be cited. Examples of the clay mineral include talc, montmorillonite, sericite, mica, chlorite, bentonite, etc. These may be used alone or in combination of two or more.
[0286] Among the above, from the viewpoint of electrochemical stability and heat resistance, at least one selected from the group consisting of aluminum oxide, basic aluminum oxide and aluminum silicate is preferred. A specific example of aluminum oxide is aluminum oxide. A specific example of basic aluminum oxide is boehmite. A specific example of aluminum silicate is kaolinite, dickite, perlite, halloysite and pyrophyllite.
[0287] In order to improve the tear strength and puncture strength, the substrate used in this embodiment may also be a multi-layer structure formed by overlapping the above substrates. Specifically, a laminate of a polyethylene microporous film and a polypropylene microporous film, or a laminate of a nonwoven fabric and a polyolefin-based microporous film can be cited.
[0288] From the viewpoint of improving the performance of the power storage device and improving the mechanical strength, the lower limit of the porosity of the substrate or the separator is preferably 20% or more, more preferably 35% or more, and the upper limit is preferably 90% or less, more preferably 80% or less. From the viewpoint of ensuring better permeability of the separator, the porosity is preferably set to 20% or more. On the other hand, from the viewpoint of ensuring better puncture strength, the porosity is preferably set to 90% or less.
[0289] In addition, from the same viewpoint, the air permeability (hereinafter also referred to as "air permeability resistance") of the substrate or separator is not particularly limited, but from the viewpoint of improving the performance of the non-aqueous secondary battery, the lower limit is preferably 20 sec / 100 cm 3 More preferably, 50 sec / 100 cm 3 The upper limit is preferably 500 sec / 100 cm 3 Below, more preferably 300sec / 100cm3 From the viewpoint of further suppressing the self-discharge of the non-aqueous secondary battery, it is preferred that the air permeability be set to 10 sec / 100 cm 3 On the other hand, from the viewpoint of obtaining better charge and discharge characteristics, it is preferred that the air permeability be set to 1000 sec / 100 cm 3 These air permeabilities and porosities were measured according to the methods described in the Examples.
[0290] Furthermore, from the perspective of improving the reliability as a spacer and suppressing thermal shrinkage, the lower limit of the puncture strength of the substrate is preferably 200g / 20μm or more, more preferably 300g / 20μm or more, and the upper limit is preferably 2000g / 20μm or less, more preferably 1000g / 20μm or less. From the perspective of further suppressing film breakage caused by active materials that fall off during battery winding, the puncture strength is preferably 200g / 20μm or more. In addition, from the perspective of further suppressing concerns about short circuits caused by expansion and contraction of electrodes accompanying charge and discharge, the puncture strength is also preferably 200g / 20μm or more. On the other hand, from the perspective of being able to further reduce the width shrinkage caused by orientation relaxation during heating, it is preferred that the puncture strength be set to 2000g / 20μm or less.
[0291] The polymer matrix containing polypropylene of the polypropylene-based microporous membrane of the present embodiment extends along a direction perpendicular to the film thickness, and the polypropylene-based microporous membrane has fibrils containing polypropylene between the polymer matrix and micropores between a plurality of the fibrils. The "direction perpendicular to the film thickness" refers to the mechanical direction (hereinafter, sometimes referred to as MD) in which the microporous membrane is continuously formed. The structure of the polypropylene-based microporous membrane can be obtained by dry method manufacturing, and more specifically, can be obtained by a dry method including a step of making a resin molded body containing polypropylene porous by dry method. Figure 3 An example of a SEM image of a polypropylene microporous membrane is shown in FIG. Figure 3 , the polymer matrix structure containing polypropylene extending along the above-mentioned "one direction perpendicular to the film thickness" can be observed.
[0292] The microporous membrane is a monolayer membrane composed of a single polyolefin microporous layer, a microporous monolayer membrane composed of a resin layer other than a polyolefin microporous layer, or a composite microporous monolayer membrane having a polyolefin resin and other resins, and is sometimes also called a microporous layer.
[0293] The polyolefin-based microporous membrane is formed from a polyolefin resin composition containing a polyolefin resin as a main component.
[0294] The polypropylene-based microporous membrane is formed from a polypropylene resin composition containing polypropylene as a main component.
[0295] In this specification, the fact that a film contains a specific material as a main component means that the film contains 50% or more of the material based on the mass of the film.
[0296] In this specification, the microporous membrane containing a polyolefin resin as a main component means that the ratio of the polyolefin resin in the microporous membrane is 50% by mass or more relative to the mass of the microporous membrane. Therefore, the polyolefin resin can form a polymer network in the microporous membrane.
[0297] The polypropylene resin composition containing polypropylene as a main component means that the ratio of the polypropylene in the polypropylene resin composition is 50% by mass or more relative to the mass of the polypropylene resin composition.
[0298] The inventors of the present invention have found that when a polypropylene microporous membrane is combined with an electrolyte containing acetonitrile, in particular, there is a problem of the volatility of the electrolyte. This problem has been studied attentively, and it is found that in a polypropylene spacer with a small pore size, when a spacer with a pore structure parallel to the thickness direction manufactured by a dry method is used, the impregnation of the electrolyte containing acetonitrile becomes extremely low. Therefore, the electrolyte will volatilize before being impregnated in the spacer. In particular, when manufacturing a battery, it is necessary to extend the time of the decompression process and allow the electrolyte to be fully impregnated in the spacer. As a result, it is newly discovered that the low boiling point solvent in the electrolyte volatilizes, which can cause initial defects.
[0299] For the polypropylene-based microporous membrane, from the viewpoint of high strength, the pore diameter ratio a / b of the average long pore diameter a of the microporous membrane and the pore diameter b orthogonal to the average long pore diameter a is preferably 0.5 or more and 30 or less. From the viewpoint of high strength, the pore diameter ratio a / b is more preferably 1 or more and 20 or less, and further preferably 1.5 or more and 15 or less.
[0300] The porosity of the spacer is preferably 30% or more and 80% or less, and / or the air permeability (hereinafter also referred to as "air permeability resistance") is preferably 100 sec / 100 cm 3 Above and 500 seconds / 100cm 3 the following.
[0301] When the porosity is lower than 30%, it is difficult to ensure sufficient ion permeability when the microporous membrane is used for battery applications. In addition, when the porosity is higher than 80%, the microporous membrane sometimes cannot maintain sufficient strength. From this point of view, the porosity of the separator is more preferably 33% to 77%, and more preferably 37% to 73%. In addition, from the viewpoint of obtaining a separator comprising a defect-free homogeneous microporous membrane, it is preferred to adjust the air permeability resistance of the separator to 100 seconds / 100cm3 In addition, from the viewpoint of helping to ensure sufficient ion permeability, it is preferred to adjust the air permeability resistance of the spacer to 500 seconds / 100 cm 3 From this point of view, the air permeability resistance of the spacer is more preferably 120 seconds / 100 cm 3 Above and 450 seconds / 100cm 3 Below, more preferably 150 seconds / 100cm 3 Above and 400 seconds / 100cm 3 the following.
[0302] <Battery exterior>
[0303] The battery casing of the nonaqueous secondary battery in this embodiment can adopt a known structure. For example, a battery can or a laminated film casing can be used as the battery casing.
[0304] As the battery can, for example, a metal can made of steel, stainless steel, aluminum, or a clad material can be used.
[0305] The laminated film outer body can overlap two pieces in a state where the hot melt resin side faces inward, or bend into a state where the hot melt resin side faces inward, so that it can be used as an outer body in a state where the end is sealed by heat sealing. When using a laminated film outer body, the positive lead body (or the positive terminal and the lead pole ear connected to the positive terminal) can also be connected to the positive electrode collector, and the negative lead body (or the negative terminal and the lead pole ear connected to the negative terminal) can be connected to the negative electrode collector. In this case, the laminated film outer body can be packaged in a state where the ends of the positive lead body and the negative lead body (or the lead pole ears connected to the positive terminal and the negative terminal, respectively) are led out to the outside of the outer body.
[0306] As the laminate film outer package, for example, a laminate film having a three-layer structure of hot melt resin / metal film / resin can be used.
[0307] The aluminum laminate film constituting the battery exterior is preferably an aluminum laminate film obtained by coating both surfaces of an aluminum foil with a polyolefin-based resin.
[0308] <Shape of non-aqueous secondary batteries>
[0309] The nonaqueous secondary battery of the present embodiment can be applied to a shape of, for example, a square shape, a rectangular tube shape, a cylindrical shape, an oval shape, a button shape, a coin shape, a flat shape, a laminated shape, or the like.
[0310] The nonaqueous secondary battery of the present embodiment can be particularly preferably applied to a square type, a rectangular tube type, and a laminate type.
[0311] <Method for producing non-aqueous secondary battery>
[0312] The nonaqueous secondary battery in the present embodiment can be manufactured using the above-mentioned electrolyte solution, a positive electrode having a positive electrode active material, a negative electrode having a negative electrode active material, a separator, and a battery exterior as necessary.
[0313] First, a laminate consisting of a positive electrode, a negative electrode and a separator can be formed. For example, a method can be used in which a long positive electrode and a negative electrode are made into a laminate having a long separator sandwiched between the positive electrode and the negative electrode, and the laminate is wound to form a laminate having a wound structure; a method in which a positive electrode and a negative electrode are cut into a plurality of sheets having a predetermined area and shape to obtain positive electrode sheets and negative electrode sheets, and a laminate having a laminate structure in which the obtained positive electrode sheets and negative electrode sheets are alternately stacked via separator sheets; a method in which a long separator is bent to form a laminate having a laminate structure in which positive electrode sheets and negative electrode sheets are alternately inserted between the bent separators; etc.
[0314] Then, the above-mentioned stacked body is housed in a battery exterior (battery case), an electrolyte is injected into the battery case, and the stacked body is immersed in the electrolyte and sealed, thereby manufacturing the nonaqueous secondary battery of the present embodiment.
[0315] It should be noted that when the configuration of the electrode is designed to have a portion where the peripheral end of the negative electrode active material layer overlaps with the peripheral end of the positive electrode active material layer, or when there is a portion with too small a width in the non-opposite portion of the negative electrode active material layer, the position of the electrode is offset when the battery is assembled, so that the charge and discharge cycle characteristics in the non-aqueous secondary battery may be reduced. Therefore, for the electrode body used in the non-aqueous secondary battery, it is preferred that the position of the electrode is fixed in advance with a tape such as a polyimide tape, a polyphenylene sulfide tape, a polypropylene (PP) tape, an adhesive, etc.
[0316] In the present embodiment, when an electrolyte using acetonitrile is used, due to its high ionic conductivity, the lithium ions released from the positive electrode during the initial charge of the non-aqueous secondary battery are likely to diffuse to the entire negative electrode. In a non-aqueous secondary battery, the area of the negative electrode active material layer is usually made larger than the positive electrode active material layer. However, if the lithium ions diffuse to the position in the negative electrode active material layer that is not opposite to the positive electrode active material layer and are retained, the lithium ions will not be released during the initial discharge and will remain on the negative electrode. Therefore, the contribution of the lithium ions that have not been released becomes the irreversible capacity. For such reasons, in a non-aqueous secondary battery using an electrolyte containing acetonitrile, the initial charge and discharge efficiency is sometimes reduced.
[0317] On the other hand, when the area of the positive electrode active material layer is larger than that of the negative electrode active material layer, or both are equal, current concentration is likely to occur at the edge of the negative electrode active material layer during charging, and lithium dendrites are likely to form.
[0318] The ratio of the area of the entire negative electrode active material layer to the area of the portion where the positive electrode active material layer and the negative electrode active material layer are opposite is not particularly limited, but is preferably greater than 1.0 and less than 1.1, more preferably greater than 1.002 and less than 1.09, further preferably greater than 1.005 and less than 1.08, and particularly preferably greater than 1.01 and less than 1.08. In a non-aqueous secondary battery using an electrolyte containing acetonitrile, the initial charge and discharge efficiency can be improved by reducing the ratio of the area of the entire negative electrode active material layer to the area of the portion where the positive electrode active material layer and the negative electrode active material layer are opposite.
[0319] Reducing the ratio of the area of the entire negative electrode active material layer to the area of the portion of the positive electrode active material layer opposite to the negative electrode active material layer refers to limiting the ratio of the area of the portion of the negative electrode active material layer that is not opposite to the positive electrode active material layer. Thus, the amount of lithium ions released from the positive electrode during the initial charge that are retained in the portion of the negative electrode active material layer that is not opposite to the positive electrode active material layer (i.e., the amount of lithium ions that are not released from the negative electrode during the initial discharge and become irreversible capacity) can be reduced as much as possible. Therefore, by designing the ratio of the area of the entire negative electrode active material layer to the area of the portion of the positive electrode active material layer opposite to the negative electrode active material layer within the above range, the initial charge and discharge efficiency of the battery can be improved while achieving the improvement of the load characteristics of the battery brought about by the use of acetonitrile, and further the formation of lithium dendrites can be suppressed.
[0320] The non-aqueous secondary battery in this embodiment can function as a battery through the initial charge, and is stabilized by decomposing part of the electrolyte during the initial charge. There is no particular limitation on the method of the initial charge, and the initial charge is preferably carried out at 0.001 to 0.3C, more preferably at 0.002 to 0.25C, and further preferably at 0.003 to 0.2C. The initial charge can also obtain a preferred result by charging via a constant voltage during the initial charge. By setting the voltage range in which the lithium salt participates in the electrochemical reaction to be longer, a stable and strong SEI is uniformly formed on the electrode surface, which has the effect of suppressing the increase of internal resistance. In addition, the reaction product will not be firmly fixed only to the negative electrode, and in some form it also has a good effect on components other than the negative electrode, such as the positive electrode and the separator. Therefore, it is very effective to consider the electrochemical reaction of the lithium salt dissolved in the electrolyte for the initial charge.
[0321] The non-aqueous secondary battery in this embodiment can also be used as a battery pack formed by connecting a plurality of non-aqueous secondary batteries in series or in parallel. From the perspective of managing the charge and discharge state of the battery pack, the operating voltage range of each battery is preferably 2 to 5V, more preferably 2 to 4.5V, and particularly preferably 2V to 4.3V.
[0322] If the size of the non-aqueous secondary battery becomes larger, it becomes difficult for the electrolyte to penetrate into the entire separator, so it is preferred to leave it to stand for more than 12 hours after injecting the electrolyte. In addition, from the viewpoint of improving the efficiency of the manufacturing process of the non-aqueous secondary battery, it is preferred that after injecting the electrolyte, it is left to stand under reduced pressure, and then the release portion is packaged. Further, from the viewpoint of simplifying the process (degassing process) of removing the gas generated when the film is formed during the initial charge, it is preferred that the release portion is not packaged during the initial charge and discharge, but is carried out under reduced pressure.
[0323] However, by applying the above-mentioned manufacturing process, in the electrolyte containing acetonitrile with high volatility, the amount of electrolyte is easily reduced, and therefore, it is possible to carry out the initial charge and discharge in a state where a part of the electrode and the separator is not immersed in the electrolyte. In this case, in the part that the electrolyte is not impregnated, the charge and discharge reaction will not be adequately carried out, and therefore, it is expected that the battery capacity will be reduced. In addition, when the non-impregnated portion is impregnated in the electrolyte by adding the electrolyte on the way of the initial charge and discharge process, the non-impregnated portion does not smoothly form a coating when the initial charge, and therefore, the reduction and decomposition reaction of the non-aqueous solvent is easily carried out, and thus it is expected that the battery capacity will be reduced.
[0324] The larger the area of the positive electrode or negative electrode, the more difficult it is for the electrolyte to penetrate, and the more gas is generated, so the above manufacturing process is often used. From the perspective of improving the efficiency of the manufacturing process, it is preferred to apply this embodiment to a battery with an area of at least one of the positive electrode and the negative electrode of 100 cm 2 The above non-aqueous secondary battery is more preferably applied to the area of 150cm 2 The above non-aqueous secondary battery is further preferably applied to a 200 cm 2 The above non-aqueous secondary battery.
[0325] It should be noted that, when the positive electrode and the negative electrode constitute a laminate, the "area of the positive electrode" refers to the area after the areas of the positive electrode are added together, and similarly, the "area of the negative electrode" refers to the area after the areas of the negative electrode are added together. From the perspective of improving the performance of the non-aqueous secondary battery involved in this embodiment using the above-mentioned manufacturing process, the above matters are preferred.
[0326] Although the modes for carrying out the present invention have been described above, the present invention is not limited to the above-described embodiments and various modifications can be made to the present invention without departing from the gist of the present invention.
[0327] Example
[0328] The present invention is described in more detail below by way of examples. The present invention is not limited to these examples. Unless otherwise specified, the experiments and measurements in the examples are carried out at room temperature.
[0329] [Examples 1 to 6, Comparative Examples 1 to 11]
[0330] Preparation of non-aqueous electrolyte
[0331] In an inactive environment, various non-aqueous solvents are mixed in a manner to achieve the prescribed concentrations shown in Table 1. Organic polymers are added to the obtained non-aqueous solvents in the proportions shown in Table 1. Furthermore, various lithium salts are added in a manner to achieve the prescribed concentrations to prepare electrolyte solutions (S01) to (S12). The compositions of these electrolyte solutions are shown in Table 1.
[0332] The abbreviations of the non-aqueous solvent, lithium salt, organic polymer and additive in each table are as follows. In addition, the mass % of the organic polymer and the additive represents the mass parts relative to 100 mass parts of the electrolyte. It should be noted that the mass % can be converted into volume % by the following formula (2) and the following formula (3).
[0333] {Value obtained by dividing the mass of the organic polymer by the specific gravity / (100+value obtained by dividing the mass of the organic polymer by the specific gravity)}×100(2)
[0334] {Value obtained by dividing the mass of the additive by the specific gravity / (100 + value obtained by dividing the mass of the additive by the specific gravity)}×100(3)
[0335] (Lithium Salt)
[0336] LiPF6: lithium hexafluorophosphate.
[0337] LiFSI: lithium bis(fluorosulfonyl)imide (LiN(SO2F)2).
[0338] (Non-aqueous solvent)
[0339] AcN: acetonitrile.
[0340] EMC: Ethyl methyl carbonate.
[0341] EC: Ethylene carbonate.
[0342] PC: propylene carbonate.
[0343] GBL: gamma-butyrolactone.
[0344] VC: vinylene carbonate.
[0345] ES: Ethylene sulfite.
[0346] (Organic polymer)
[0347] P0903: Polyethylene oxide (viscosity average molecular weight 6000).
[0348] P2830: Polyethylene oxide (viscosity average molecular weight 20,000).
[0349] SE-8: polyethylene oxide (viscosity average molecular weight: 93,000).
[0350] P1819: Polyethylene oxide (viscosity average molecular weight 100,000).
[0351] P1820: Polyethylene oxide (viscosity average molecular weight 600,000).
[0352] SE-70: polyethylene oxide (viscosity average molecular weight 63,000).
[0353] P3727: Polyethylene oxide (viscosity average molecular weight 1,000,000).
[0354] P3728: Polyethylene oxide (viscosity average molecular weight 2,000,000).
[0355] P1822: poly(methyl methacrylate) (viscosity average molecular weight 120,000).
[0356] P4457: poly(methyl methacrylate) (viscosity average molecular weight 350,000).
[0357] (additive)
[0358] P1022: tri(2-ethylhexyl) phosphate.
[0359] The viscosity average molecular weight of the organic polymer is measured by the following method.
[0360] (1) Viscosity average molecular weight
[0361] The viscosity average molecular weight is evaluated by a viscosity method. The viscosity average molecular weight of an organic polymer is calculated from the limiting viscosity number [η] measured in accordance with JIS K 7367-2:1999.
[0362] Table 1
[0363]
[0364] The ion conductivity and viscosity of the electrolyte prepared as described in (1) above were measured by the following method. It should be noted that for electrolytes where undissolved organic polymers or reprecipitation were observed after adjustment of the electrolyte, "-" was recorded and subsequent measurements and battery evaluations were not performed.
[0365] (2) Determination of ionic conductivity
[0366] An electrolyte solution is prepared as described in (1) above, and a battery cell for measuring ion conductivity "CT-58101B" (trade name) manufactured by DKK Co., Ltd. of East Asia connected to an ion conductivity meter "CM-41X" (trade name) manufactured by DKK Co., Ltd. of East Asia is inserted into a container containing the electrolyte solution, and the ion conductivity of the electrolyte solution at 25°C is measured.
[0367] (3) Viscosity measurement
[0368] The electrolyte solution was prepared as described in (1) above, and the detection terminal of a vibration viscometer "VM-10A" (trade name) manufactured by SEKONIC CORPORATION was inserted into the container containing the electrolyte solution to measure the viscosity of the electrolyte solution at 25°C.
[0369] Table 2 below shows the results of measuring the ion conductivity and viscosity of the electrolytic solutions S01 to S12 at 25° C. and the Z values obtained from the formula (1).
[0370] Table 2
[0371]
[0372] As shown in the above table, the viscosity of the electrolyte solution (Examples 1 to 4) of the present embodiment is 4.1 mPa·s or more, and the ion conductivity is 18.5 mS / cm or more, and Z is 75 or more. On the other hand, the viscosity of Comparative Examples 1 to 3 is low, which is 3.5 mPa·s or less, and Z is 65 or less. In Comparative Examples 4 to 6, undissolved matter was observed after adding organic polymers after adjusting the electrolyte solution, so no measurement was performed. The ion conductivity of Comparative Example 7 is 11.3 mS / cm, and the ion conductivity of Comparative Example 8 is 5.0 mS / cm, both of which are 13.0 mS / cm or less.
[0373] (4) Volatility test
[0374] An aluminum dish was placed on a weighing scale, and 20 μL of the adjusted electrolyte solution was dripped onto it. The weight A immediately after the dripping was measured. The weight B was measured from the start of dripping to 2 minutes later, and the volatility of the electrolyte solution was evaluated from the weight change using the following formula:
[0375] {(weight B-weight A) / weight A}×100.
[0376] (5) Fabrication of non-aqueous secondary batteries
[0377] (5-1) Preparation of positive electrode
[0378] LiFePO4 as a positive electrode active material, acetylene black powder as a conductive aid, and polyvinylidene fluoride (PVDF) as a binder were mixed in a mass ratio of 87:8:5 to obtain a positive electrode mixture.
[0379] N-methyl-2-pyrrolidone as a solvent was added to the obtained positive electrode mixture, and the mixture was further mixed to prepare a slurry containing the positive electrode mixture. The weight per unit area of one side of the slurry containing the positive electrode mixture was adjusted to 20.7 mg / cm 2 The positive electrode active material layer was coated on one or both sides of a 15 μm thick aluminum foil as a positive electrode current collector, and the solvent was dried and removed in a hot air drying oven. Then, the positive electrode active material layer was rolled using a roll press to a density of 1.9 g / cm 3 The positive electrode is obtained by vacuum drying at 120° C. for 12 hours or more.
[0380] (5-2) Preparation of negative electrode
[0381] Graphite as a negative electrode active material, carboxymethyl cellulose (CMC) as a binder, and styrene butadiene rubber (SBR) were mixed at a mass ratio of 97.4:1.1:1.5 to obtain a negative electrode mixture.
[0382] Water as a solvent was added to the obtained negative electrode mixture, and the mixture was further mixed to prepare a slurry containing the negative electrode mixture. The weight per unit area of the slurry containing the negative electrode mixture was adjusted to 8.8 mg / cm 2 The negative electrode active material layer was coated on one or both sides of a 10 μm thick copper foil as the negative electrode current collector, and the solvent was dried and removed in a hot air drying oven. Then, the negative electrode active material layer was rolled using a roller press until the density of the negative electrode active material layer became 1.4 g / cm 3 The negative electrode was obtained by vacuum drying at 80° C. for 12 hours or more.
[0383] (5-3) Preparation of spacer
[0384] <Preparation of polypropylene resin composition>
[0385] Ultra-high molecular weight polypropylene resin (PP, MFR = 0.25) and ethylene / 1-butene copolymer (C2 / C4: density = 0.893 g / cm 2, melting point = 80°C, MFR = 6.7) were dry-blended at a mass ratio of PP: C2 / C4 = 50:50 (mass %), and then melt-kneaded using ZSK40 (manufactured by Coperion, L / D = 46). In order to suppress the decomposition and modification of the resin as much as possible, the area from the resin feeding hopper port to the raw material tank is made completely sealed and nitrogen is continuously introduced from the lower part of the hopper to control the oxygen concentration near the raw material feeding port to be below 50 ppm. In addition, the exhaust section is completely sealed to eliminate the air leakage into the barrel. Due to the effect of reducing the oxygen concentration, the decomposition and modification of the polymer are significantly suppressed under high temperature conditions, and further, the ethylene / 1-butene copolymer can be finely dispersed. After melt-kneading, the strands are pulled out from the die head (8 holes) and the molten kneaded product is cooled in a water cooling bath, and then cut using a pelletizer to obtain pellets.
[0386] <Production of microporous membrane (spacer having three layers of microporous membrane)>
[0387] Ultrahigh molecular weight polypropylene resin (PP, MFR = 0.25) and the above pellets were dry-blended at a mass ratio of PP: pellets = 90:10 (mass %), melted using a 2.5-inch extruder, and supplied to an annular die using a gear pump. Thus, the feed ratio of the resins fed was PP: C2 / C4 = 95:5 (mass %).
[0388] The temperature of the die was set to 240° C., and the molten polymer was cooled by blowing air and then wound on a roll. The thickness of the extruded PP precursor (web film) was 6 μm.
[0389] A high molecular weight polyethylene resin (PE, MFR=0.38) was melted using a 2.5-inch extruder and supplied to an annular die using a gear pump.
[0390] The temperature of the die was set to 210° C., and the molten polymer was cooled by blowing air and then wound on a roll. The thickness of the extruded PE precursor (web film) was 6 μm.
[0391] The obtained PP precursor and the obtained PE precursor were overlapped in three layers of PP precursor / PE precursor / PP precursor and laminated at 120°C to obtain a three-layer laminated roll film. The roll film was annealed at 125°C for 20 minutes. Then, the annealed film was cold stretched to 15% at room temperature, then hot stretched to 150% at 115°C, and relaxed to 103% at 125°C to form a spacer having a structure of a three-layer microporous film. After the above-mentioned stretching and opening, the physical properties of the spacer were measured.
[0392] The physical properties of the spacer prepared above were measured by the following methods.
[0393] [Average long pore diameter (nm), aperture ratio]
[0394] The surface of the microporous membrane is observed by SEM, and the pore size of the SEM image is measured to obtain the average long pore size of the microporous membrane. Specifically, based on 6 images of the microporous membrane surface observed by SEM at 30,000 times, all the long pore sizes of the micropores within the image range of 4.0 μm × 2.8 μm are measured, and the average value is calculated to obtain the average long pore size a. In addition, the pore size of each hole in the direction orthogonal to the long pore size direction is measured, and the average is calculated to obtain the average pore size b. The aperture ratio (a / b) is calculated by dividing the average long pore size by the average pore size. Figure 3 An example of a SEM image of a polypropylene microporous membrane as a spacer is shown in FIG. Figure 3 The pore size and pore size ratio were calculated based on the observations.
[0395] [Measurement of thickness (μm)]
[0396] The thickness of the separator including the microporous membrane was measured at room temperature 23±2° C. using a digital indicator IDC112 manufactured by Mitutoyo Corporation.
[0397] [Porosity (%)]
[0398] A 5 cm×5 cm square sample was cut out from the separator including the microporous film, and the porosity was calculated from the volume and mass of the sample using the following formula.
[0399] Porosity (%) = {(volume (cm 3 )-mass (g) / density of resin composition (g / cm 3 )) / Volume(cm 3 )}×100
[0400] [Breathability resistance (seconds / 100cm 3 )]
[0401] The air permeability resistance of the separator including the microporous membrane was measured using a Gurley permeometer in accordance with JIS P-8117.
[0402] The physical properties of the spacer measured by the above method are as follows: the aperture ratio is 8.1, the film thickness is 25 μm, and the air permeability resistance is 217 seconds / 100 cm 3 , the porosity is 55%.
[0403] (5-4) Assembly of non-aqueous secondary batteries
[0404] In a drying room with a dew point temperature of -80°C to -20°C, the cut positive electrode with leads and the negative electrode with leads are overlapped via the separator to form a stacked electrode body, and the stacked electrode body is contained in an aluminum laminate outer package. Then, after injecting 7.0 g of electrolyte into the outer package, a decompression process is performed to impregnate the electrolyte in the separator. The decompression process is to repeat the operation of evacuating from normal pressure to 60 kPa three times, and immediately returning to normal pressure after reaching 60 kPa. Then, after evacuating from normal pressure to 60 kPa, stand in this state for 30 seconds and return to normal pressure. Finally, the operation of evacuating from normal pressure to 60 kPa three times, and immediately returning to normal pressure after reaching 60 kPa, is repeated. After the decompression process is completed, the outer package is packaged to obtain a non-aqueous secondary battery. Here, the electrode areas were 56 mm wide by 378 mm long and 56 mm wide by 304 mm long for the positive electrode and 58 mm wide by 401 mm long and 58 mm wide by 342 mm long for the negative electrode. The positive electrodes and negative electrodes were alternately stacked and wound with separators interposed therebetween.
[0405] (6) Evaluation of non-aqueous secondary batteries
[0406] First, the non-aqueous secondary battery obtained as described above was subjected to initial charging treatment and initial charge-discharge capacity determination according to the following steps (6-1) and (6-2). Then, the non-aqueous secondary battery was evaluated according to the step (6-2). It should be noted that TOSCAT-300 (trade name) manufactured by Toyo Systems Co., Ltd. and LU-123 (trade name) or BTS-408C (trade name) manufactured by ESPEC were used for charging and discharging.
[0407] Here, 1C refers to a current value at which a fully charged battery is discharged at a constant current and the discharge is expected to be completed in 1 hour.
[0408] (6-1) Initial charge and discharge treatment of non-aqueous secondary batteries
[0409] The ambient temperature of the non-aqueous secondary battery was set to 25°C, and the battery was charged at a constant current equivalent to 0.025C until the battery voltage reached 3.5V. Then, the constant voltage charging was continued for 2 hours while the current was decayed while the battery voltage was maintained at 3.5V, or the constant voltage charging was continued until the charge capacity reached 90% of the designed capacity. After charging, a rest time of 20 minutes was taken, and then the battery was discharged at a constant current of 0.1C until 2.0V.
[0410] (6-2) Fine charge and discharge treatment
[0411] After the treatment of (6-1), the ambient temperature of the non-aqueous secondary battery was set to 25°C, and the battery was charged to 3.5V at a constant current of 0.2C. Then, the battery was charged at a constant voltage for 2 hours while the current was decayed while the voltage was maintained at 3.5V, or the battery was charged at a constant voltage until the current value decayed to 0.05C. After charging, a rest time of 20 minutes was taken. Then, the battery was discharged to 2.0V at a constant current of 0.2C.
[0412] (6-3) 45°C Cycle Test of Non-aqueous Secondary Batteries
[0413] For the non-aqueous secondary battery that has been charged and discharged using the methods described in (6-1) and (6-2) above, the ambient temperature is set to 45°C. First, the battery is charged at a constant current of 1C and reaches 3.5V, and then charged at a constant voltage of 3.5V until the current decays to 0.05C. A 10-minute rest period is taken after charging. Then, the battery is discharged at 1C until 2.5V. This process of charging and discharging once each is considered as a cycle, and 300 cycles of charging and discharging are performed. The discharge capacity of the 300th cycle when the discharge capacity of the first cycle is set to 100% is used as the discharge capacity retention rate of the 45°C cycle test.
[0414] The electrolyte solutions in Table 1 were used to evaluate the volatility of the electrolyte solutions according to the method described in (4) above. In addition, the cycle performance of the non-aqueous secondary battery was evaluated according to the method described in (6) above. The test results are shown in Table 3.
[0415] Table 3
[0416]
[0417] As shown in Table 3, the weight change of the non-aqueous secondary battery (Comparative Examples 9 to 11) after 2 minutes of dripping the electrolyte is large, which is more than 12.7%, indicating high volatility. Therefore, even if the battery is made, acetonitrile will volatilize in the decompression process, so the discharge capacity retention rate is less than 59%. On the other hand, for the non-aqueous secondary battery (Examples 5 and 6) of the present embodiment, the weight change after 2 minutes of dripping the electrolyte is small, which is less than 10.5%, suppressing volatility. Therefore, the discharge capacity retention rate after 300 cycles of Examples 5 and 6 is 78.5%.
[0418] [Examples 7 to 10 and Comparative Examples 12 to 17]
[0419] In an inactive environment, various non-aqueous solvents are mixed in a manner to achieve the prescribed concentrations shown in Table 4. Organic polymers are added to the obtained non-aqueous solvents in the proportions shown in Table 4. Furthermore, various lithium salts are added in a manner to achieve the prescribed concentrations to prepare electrolyte solutions (S13) to (S19). The compositions of these electrolyte solutions are shown in Table 4.
[0420] Table 4
[0421]
[0422] Table 5 shows the results of measuring the ion conductivity and viscosity of the electrolytic solutions S13 to S19 at 25° C. and the Z values obtained from the formula (1).
[0423] Table 5
[0424]
[0425] As shown in Table 5, the viscosity of the electrolyte solution (Example 7) of the present embodiment is 4.9 mPa·s, and the ion conductivity is 22.0 mS / cm, and Z is 108. The viscosity of the electrolyte solution (Example 8) of the present embodiment is 22.8 mPa·s, and the ion conductivity is 21.9 mS / cm, and Z is 499. On the other hand, the viscosity of the electrolyte solution (Comparative Examples 12 to 14) is low, being 2.2 mPa·s or less, and Z being 49 or less. In particular, the viscosity of Comparative Example 14 is lower than 2.0 mS / cm, and it is presumed that the volatility is high. In Comparative Examples 15 and 16, undissolved matter was observed after the addition of the organic polymer after the electrolyte solution was adjusted, and therefore, no measurement was performed.
[0426] The electrolyte solutions in Table 4 were used to evaluate the volatility of the electrolyte solutions according to the method described in (4) above. In addition, the cycle performance of the non-aqueous secondary battery was evaluated according to the method described in (6) above. The test results are shown in Table 6.
[0427] Table 6
[0428]
[0429] As shown in Table 6, the weight change of the non-aqueous secondary battery (Comparative Example 17) after 2 minutes of dripping the electrolyte is large, which is more than 13.3%, indicating high volatility. Therefore, even if the battery is made, acetonitrile is volatilized in the decompression process, so the discharge capacity retention rate is 41.5%. On the other hand, the weight change of the non-aqueous secondary battery (Examples 9 and 10) of the present embodiment until 2 minutes after the start of dripping the electrolyte is small, which is less than 11.6%, suppressing volatility. In addition, the discharge capacity retention rate after 300 cycles is more than 69.0%.
[0430] [Examples 11 to 23 and Comparative Examples 18 to 27]
[0431] Under an inactive environment, various non-aqueous solvents are mixed in a manner to achieve the prescribed concentrations shown in Table 7. Organic polymers are added to the obtained non-aqueous solvents in the proportions shown in Table 7. Furthermore, various lithium salts are added in a manner to achieve the prescribed concentrations to prepare electrolyte solutions (S20) to (S36). The compositions of these electrolyte solutions are shown in Table 7.
[0432] Table 7
[0433]
[0434] Table 8 below shows the results of measuring the ion conductivity and viscosity of the electrolytic solutions S20 to S36 at 25° C. and the Z values obtained from the formula (1).
[0435] Table 8
[0436]
[0437] As shown in Table 8, the viscosity of the electrolyte solution (Examples 11 to 18) of the present embodiment is 3.3 mPa·s or more, and the ion conductivity is 24.1 mS / cm or more, and Z is 87 or more. On the other hand, when the electrolyte solution (Comparative Examples 18 to 16) was observed, the viscosity of Comparative Example 18 was less than 2.0 mPa·s. The viscosity of Comparative Examples 19 and 21 was low, being 2.5 mPa·s or less, and Z was 67 or less. In Comparative Examples 20 and Comparative Examples 22 to 26, undissolved matter was observed after adding the organic polymer after adjusting the electrolyte solution, and therefore, no measurement was performed.
[0438] The electrolyte solutions in Table 7 were used to evaluate the volatility of the electrolyte solutions according to the method described in (4) above. In addition, the cycle performance of the non-aqueous secondary battery was evaluated according to the method described in (6) above. The test results are shown in Table 9.
[0439] Table 9
[0440]
[0441] As shown in Table 9, the weight change of the non-aqueous secondary battery (Comparative Example 27) after 2 minutes of dripping the electrolyte is large, which is 15.1%, indicating high volatility. Therefore, even if the battery is made, acetonitrile is volatilized in the decompression process, so the discharge capacity retention rate after 300 cycles is 24.0%. On the other hand, the weight change of the non-aqueous secondary battery (Examples 19 to 23) of the present embodiment until 2 minutes after the start of dripping the electrolyte is small, which is less than 13.1%, suppressing volatility. Therefore, the discharge capacity retention rate after 300 cycles is more than 52.0%. Among them, the weight change of Example 22 is 11.4%, which particularly suppresses volatility. Moreover, the discharge capacity retention rate after 300 cycles is 70.0%.
[0442] [Examples 24 to 29 and Comparative Examples 28 to 29]
[0443] In an inactive environment, various non-aqueous solvents are mixed in a manner to obtain the prescribed concentrations shown in Table 10. Organic polymers are added to the obtained non-aqueous solvents in the proportions shown in Table 10. Furthermore, various lithium salts are added in a manner to obtain the prescribed concentrations to prepare electrolyte solutions (S40) to (S43). The compositions of these electrolyte solutions are shown in Table 10.
[0444] Table 10
[0445]
[0446] Table 11 below shows the results of measuring the ion conductivity and viscosity of the electrolytic solutions S40 to S43 at 25° C. and the Z values obtained from the formula (1).
[0447] Table 11
[0448]
[0449] As shown in Table 11, when the electrolyte solutions (Examples 24 to 26) of the present embodiment were observed, the viscosity of Example 24 was 3.9 mPa·s, the ion conductivity was 18.0 mS / cm, and Z was 70. The viscosity of Example 25 was 40.8 mPa·s, the ion conductivity was 13.0 mS / cm, and Z was 530. The viscosity of Example 26 was 6.4 mPa·s, the ion conductivity was 18.2 mS / cm, and Z was 117. On the other hand, the viscosity of the electrolyte solution (Comparative Example 28) was less than 3.0 mPa·s.
[0450] The electrolyte solutions in Table 7 were used to evaluate the volatility of the electrolyte solutions according to the method described in (4) above. In addition, the cycle performance of the non-aqueous secondary battery was evaluated according to the method described in (6) above. The test results are shown in Table 9.
[0451] Table 12
[0452]
[0453] As shown in Table 12, the weight change of the non-aqueous secondary battery (Comparative Example 29) after 2 minutes of dripping the electrolyte is large, which is 12.4%, indicating high volatility. Therefore, even if the battery is made, acetonitrile is volatilized in the decompression process, so the discharge capacity retention rate after 300 cycles is 60.5%. On the other hand, the weight change of the non-aqueous secondary battery (Examples 27 to 29) of the present embodiment until 2 minutes after the start of dripping the electrolyte is small, which is less than 11.5%, suppressing volatility. Therefore, the discharge capacity retention rate after 300 cycles is more than 70.0%. Among them, the weight change of Example 28 is 10.2%, which particularly suppresses volatility. Moreover, the discharge capacity retention rate after 300 cycles is 81.9%.
[0454] As shown in this result, it is clear that by using an electrolyte solution within the scope of the constituent elements of the present invention and a non-aqueous secondary battery, even when using an electrolyte solution containing acetonitrile, it is possible to provide a non-aqueous secondary battery having high ion conductivity while suppressing the volatility of the electrolyte solution.
[0455] Industrial Applicability
[0456] Since the electrolyte within the scope of the constituent elements of the present invention can be used for batteries that require suppressed volatility, it is expected that the non-aqueous secondary battery using the non-aqueous solvent of the present invention can be used as a rechargeable battery for portable devices such as mobile phones, portable audio equipment, personal computers, IC (Integrated Circuit) tags, etc.; a rechargeable battery for automobiles such as hybrid cars, plug-in hybrid cars, and electric cars; a low-voltage power supply such as a 12V power supply, a 24V power supply, and a 48V power supply; a residential power storage system, IoT equipment, etc. In addition, the non-aqueous secondary battery using the non-aqueous solvent of the present invention can also be used for use in cold regions and outdoor use in summer.
[0457] Description of Reference Numerals
[0458] 100: Non-aqueous secondary battery.
[0459] 110: Battery exterior.
[0460] 120: Space for external battery installation.
[0461] 130: Positive electrode lead body.
[0462] 140: Negative electrode lead body.
[0463] 150: Positive electrode.
[0464] 160: Negative pole.
[0465] 170: Spacer.
Claims
1. A non-aqueous secondary battery comprising a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions, a negative electrode containing a material capable of absorbing and releasing lithium ions, a non-aqueous electrolyte, and a separator, wherein: The non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer. The non-aqueous solvent contains 10% by volume or more and 90% by volume or less of acetonitrile, The lithium salt includes a lithium imide salt, and the content of the lithium salt is 0.5 mol / L or more and 2 mol / L or less relative to the non-aqueous electrolyte solution, The viscosity average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less, The non-aqueous electrolyte has a viscosity of 2 mPa·s or more and 500 mPa·s or less at 25° C., an ion conductivity of 13 mS / cm or more, and a Z value represented by the following formula (1) of 70 or more. Z = viscosity of electrolyte (mPa·s)×ion conductivity of electrolyte (mS / cm) (1).
2. The nonaqueous secondary battery according to claim 1, wherein The organic polymer has at least one of a polyether structure and an ester structure.
3. The non-aqueous secondary battery according to claim 1 or 2, wherein: The organic polymer includes at least one of polyethylene oxide and poly(methyl methacrylate).
4. The nonaqueous secondary battery according to claim 1 or 2, wherein: The viscosity average molecular weight of the organic polymer is 90,000 or more and 650,000 or less.
5. The non-aqueous secondary battery according to claim 1 or 2, wherein: The content of the organic polymer is 0.1 mass % or more and 10 mass % or less relative to the total amount of the non-aqueous electrolyte solution.
6. The non-aqueous secondary battery according to claim 1 or 2, wherein: The content of the organic polymer is 0.1 mass % or more and 3 mass % or less relative to the total amount of the non-aqueous electrolyte solution.
7. The nonaqueous secondary battery according to claim 1 or 2, wherein: The area of at least one of the positive electrode and the negative electrode is 100 cm 2 above.
8. The nonaqueous secondary battery according to claim 1 or 2, wherein: A wound body in which the stacked body with the separator sandwiched between the positive electrode and the negative electrode, a stacked body in which positive and negative electrode sheets are alternately stacked via the separator, and a stacked body in which positive and negative electrodes are alternately inserted between zigzag separators are housed in the battery exterior.
9. The nonaqueous secondary battery according to claim 1 or 2, wherein: The non-aqueous electrolyte has a viscosity of 2.5 mPa·s or more and 150 mPa·s or less at 25° C., and an ion conductivity of 10 mS / cm or more and 40 mS / cm or less at 25° C.
10. The nonaqueous secondary battery according to claim 1 or 2, wherein: The lithium salt further comprises lithium hexafluorophosphate, which is LiPF6. The nonaqueous secondary battery includes the lithium-containing imide salt and the LiPF6 at a molar concentration of the LiPF6<the lithium-containing imide salt.
11. The nonaqueous secondary battery according to claim 1 or 2, wherein: The non-aqueous solvent contains 20 volume % or more and 90 volume % or less of acetonitrile.
12. The nonaqueous secondary battery according to claim 1 or 2, wherein: The porosity of the spacer is 20% or more and 90% or less, and the air permeability resistance is 20 seconds / 100 cm 3 Above and 500 seconds / 100cm 3 the following.
13. The nonaqueous secondary battery according to claim 1 or 2, wherein: The separator has a porous layer containing an inorganic filler on one or both sides thereof, The inorganic filler is at least one selected from the group consisting of alumina, basic alumina, and aluminum silicate.
14. The non-aqueous secondary battery according to claim 1 or 2, wherein: The spacer has a polypropylene microporous membrane, In the microporous membrane, the polymer matrix comprising the polypropylene extends in a direction perpendicular to the membrane thickness, Fibrils comprising the polypropylene are formed between the polymer matrices, and, Micropores are formed between the plurality of fibrils.
15. The non-aqueous secondary battery according to claim 1 or 2, wherein: The spacer has a polypropylene microporous membrane, The microporous membrane has a pore diameter ratio a / b of an average long pore diameter a to a pore diameter b orthogonal to the average long pore diameter a of 0.5 or more and 30 or less.
16. A non-aqueous electrolyte for a non-aqueous secondary battery having a positive electrode containing one or more positive electrode active materials capable of absorbing and releasing lithium ions, a negative electrode containing a material capable of absorbing and releasing lithium ions, a non-aqueous electrolyte, and a separator, wherein: The non-aqueous electrolyte contains a non-aqueous solvent, a lithium salt and an organic polymer. The non-aqueous solvent contains 10% by volume or more and 90% by volume or less of acetonitrile, The lithium salt includes a lithium imide salt, and the content of the lithium salt is 0.5 mol / L or more and 2 mol / L or less relative to the non-aqueous electrolyte solution, The viscosity average molecular weight of the organic polymer is 30,000 or more and 1,000,000 or less, The non-aqueous electrolyte has a viscosity of 2 mPa·s or more and 500 mPa·s or less at 25° C., an ion conductivity of 13 mS / cm or more, and a Z value represented by the following formula (1) of 70 or more. Z = viscosity of electrolyte (mPa·s)×ion conductivity of electrolyte (mS / cm) (1).