Strain adjusting system and method based on flexible sensor and actuator and application
By improving the preparation method of flexible bending sensors and actuators, combined with a highly sensitive three-layer film structure and nickel-titanium shape memory alloy, an integrated system is formed, which solves the problems of low sensitivity and application limitations in the existing technology and achieves high efficiency. , precise strain adjustment and diverse applications.
Patent Information
- Application Number
- CN202410861351.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing flexible bending sensors and actuators have deficiencies in sensitivity, preparation process, cost, environmental adaptability and functional integration. Especially under small strain conditions, they have low sensitivity, complex preparation and high cost, making it difficult to meet the needs of diverse applications.
By improving the preparation method of flexible bending sensors and flexible actuators, combining flexible bending sensors and actuators to form an integrated system, using highly sensitive three-layer film structure sensors and nickel-titanium shape memory alloy actuators, signal monitoring and Closed-loop operation of feedback control.
It improves the sensitivity of the sensor and the strain capacity of the actuator, achieves efficient and precise strain adjustment, adapts to a variety of complex environments, and broadens the application scenarios, especially showing significant technical advantages in assisted plant growth systems.
Smart Images

Figure CN118749327A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field related to flexible sensors and actuators, and in particular, to a strain regulation system, method and application based on flexible sensors and actuators. Background Art
[0002] The statements in this section merely provide background information related to the present disclosure and do not necessarily constitute prior art.
[0003] In modern sensor technology, flexible bending sensors and flexible actuators have shown broad application prospects in many fields due to their unique performance. Flexible bending sensors can convert strain into electrical signals, have soft and stretchable characteristics, and are suitable for various complex usage scenarios. However, there are still many problems in the practical application of flexible bending sensors in the prior art: First, the sensitivity of flexible bending sensors is low under small strain conditions, and the resistance change rate is not high, which limits their application in precision measurement. Secondly, the preparation process of this type of sensor is relatively complicated, the required materials are expensive, and it is difficult to achieve large-scale production. In addition, poor environmental adaptability is also a significant disadvantage. The sensor is difficult to work stably in various complex environments, and the flexible bending sensor cannot fit closely to the surface of the monitored object, affecting its measurement accuracy and stability.
[0004] Flexible actuators can transform the alloy lattice by external stimulation (such as electrical stimulation), thereby causing strain, and are widely used in a variety of intelligent devices and systems. However, existing flexible actuators also face many technical bottlenecks. For example, they are usually unable to complete the corresponding strain through small current stimulation, which limits their application in low-power devices. Flexible actuators made by existing chemical preparation methods are difficult to withstand large loads, and the strain generated is too small, and the application environment is limited. At present, most existing flexible sensors can only be used to monitor signals, and the range of motion and strain type of the actuators are also greatly limited, which cannot meet the needs of diverse applications.
[0005] In summary, the existing flexible bending sensors and flexible actuators have obvious deficiencies in sensitivity, preparation process, cost, environmental adaptability, functional integration, etc.; although flexible bending sensors and flexible actuators each have a wide range of applications, the existing technology lacks a system that combines the two. Summary of the invention
[0006] In order to solve the above problems, the present disclosure proposes a strain regulation system, method and application based on flexible sensors and actuators. Through the improved preparation method of flexible bending sensors and flexible actuators, the performance of flexible bending sensors and flexible actuators are improved, and the flexible bending sensors are combined with flexible actuators to form an integrated system, which innovatively realizes the integrated operation from signal monitoring to feedback control.
[0007] In order to achieve the above objectives, the present disclosure adopts the following technical solutions:
[0008] One or more embodiments provide a strain regulation system based on a flexible sensor and an actuator, comprising: a flexible bending sensor, a flexible actuator, and a processor, wherein the flexible bending sensor and the flexible actuator are respectively arranged on the surface of an object to be detected;
[0009] The bending of the object surface is detected by a flexible bending sensor; the processor controls the flexible actuator to generate corresponding bending strain after judging the bending detection result.
[0010] One or more embodiments provide a strain adjustment method of a strain adjustment system based on a flexible sensor and an actuator, comprising the following steps:
[0011] Detect the bending of the object surface based on flexible sensors;
[0012] Compare the search results with the set threshold;
[0013] The actuator is controlled to generate corresponding bending strain according to the comparison result of the detection data.
[0014] One or more embodiments provide an application of the strain regulation system based on the above-mentioned flexible sensor and actuator in a system for assisting plant growth;
[0015] The flexible bending sensor is attached to the upper surface of the blade. When the blade is bent and strained, the flexible bending sensor generates a resistance change, thereby obtaining a voltage change signal.
[0016] The flexible actuator is attached to the back of the blade and generates bending strain when electrically stimulated.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present disclosure designs a sensing and feedback execution system by combining a flexible bending sensor with high sensitivity, low hysteresis, and softness that can adapt to the surface of an object with a flexible actuator that can generate large bending strain with a small current stimulation and can withstand a large load. The system sets the sensor signal change amount to a threshold for judgment. When the detected bending exceeds the set threshold, the processor outputs high and low level signals through a relay to quickly control the flexible actuator to generate corresponding bending strain. This closed-loop control mechanism ensures that the system can respond and adjust quickly to maintain the desired bending state of the object surface.
[0019] By organically combining the flexible bending sensor with the flexible actuator, not only the performance of a single device is improved, but also efficient and precise strain regulation is achieved through a closed-loop control system, demonstrating significant technical advantages and broad application potential.
[0020] The advantages of the present disclosure and the advantages of additional aspects will be described in detail in the following specific embodiments. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings constituting a part of the present disclosure are used to provide a further understanding of the present disclosure. The exemplary embodiments of the present disclosure and the description thereof are used to explain the present disclosure but do not constitute a limitation of the present disclosure.
[0022] Figure 1 is a flow chart of preparing a flexible bending sensor provided by one or more embodiments of the present disclosure;
[0023] Figure 2 is a schematic diagram of a three-layer structure of a flexible bending sensor provided by one or more embodiments of the present disclosure;
[0024] Figure 3 is a SEM (scanning electron microscope) image of a flexible bending sensor electrode layer provided by one or more embodiments of the present disclosure;
[0025] Figure 4 is the resistance change rate of the flexible bending sensor provided by one or more embodiments of the present disclosure under bending strain;
[0026] Figure 5 is the response time and recovery time of the flexible bending sensor provided by one or more embodiments of the present disclosure;
[0027] Figure 6 is the minimum detection limit of the flexible bending sensor provided by one or more embodiments of the present disclosure;
[0028] Figure 7 is the spatial variation of strain of the flexible actuator provided in Example 3 of the present disclosure when it contracts while being energized;
[0029] Figure 8is the change of temperature over time of the flexible actuator provided in Example 3 of the present disclosure during the first power-on activation and the second activation process;
[0030] Fig. 9 The surface temperature of the flexible actuator provided in Example 3 of the present disclosure varies with the magnitude of the current flowing through it;
[0031] Fig.10 is the bending angle of the flexible actuator provided in Example 3 of the present disclosure when different currents are applied;
[0032] Fig.11 is the maximum load of the flexible actuator provided in Example 3 of the present disclosure when different currents are applied;
[0033] Fig.12 It is a schematic diagram of a perception feedback assisted plant growth system composed of a flexible bending sensor and an actuator provided in Example 1 of the present disclosure. DETAILED DESCRIPTION
[0034] The present disclosure is further described below in conjunction with the accompanying drawings and embodiments.
[0035] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present disclosure. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present disclosure belongs.
[0036] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present disclosure. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof. It should be noted that, in the absence of conflict, the various embodiments in the present disclosure and the features in the embodiments can be combined with each other. The embodiments will be described in detail below in conjunction with the accompanying drawings.
[0037] In order to solve some technical problems existing in the above background technology, the present invention designs a preparation method of a flexible bending sensor and a flexible actuator. The flexible bending sensor disclosed in the present invention has high sensitivity, small hysteresis, and is soft and adaptable to the surface of an object; the flexible actuator has a small current stimulation that can produce a large bending strain and can withstand a large load. Both devices have broken some of the above limitations and have a wider range of application scenarios. In addition, the present invention combines the two, based on the strain adjustment system of the flexible sensor and the actuator, to realize the sensing and feedback execution. The sensor is responsible for the sensing function. After collecting the sensor signal with a single-chip microcomputer, the 80C51 processor is used to judge the data, and the sensor signal change is set to a threshold judgment. The judgment result is controlled by the 80C51 processor to control the high and low level output of the relay to control the flexible actuator. The following is an explanation with a specific embodiment.
[0038] Example 1
[0039] In the technical solutions disclosed in one or more embodiments, Figures 1 to 12 As shown, the strain regulation system based on the flexible sensor and the actuator comprises: a flexible bending sensor, a flexible actuator and a processor, wherein the flexible bending sensor and the flexible actuator are respectively arranged on the surface of the object to be detected;
[0040] The bending of the object surface is detected by a flexible bending sensor; the processor controls the flexible actuator to generate corresponding bending strain after judging the bending detection result.
[0041] A further technical solution, a flexible bending sensor, comprises:
[0042] From bottom to top, they are the bottom film, electrode film and top film;
[0043] The bottom film is a TPU film as a tape film; the electrode film is a silver electrode film; the top film is a TPU / CNTs spinning film, which is a TPU spinning film wrapped with a carbon nanotube film;
[0044] Among them, the bottom layer TPU film is the encapsulation layer, which is mainly used to fix the applied object and achieve adhesion with the sensor. The TPU sticker is very thin and will not affect the strain range, avoiding inflexible strain.
[0045] The electrode film, or electrode layer, is fixed at both ends of the bottom film. This design makes the object more flexible. The uneven microstructure design can improve the sensitivity of different strains. The SEM image of the electrode surface is as follows: Figure 3 As shown; At the same time, the sensitivity of small-range strain is improved and the detection limit is small. The test results are as follows Figure 4 , and the sensitivity of the three-layer film also improves the response speed, such as Figure 5 shown.
[0046] The flexible bending sensor provided in this embodiment adopts a three-layer membrane structure, in which the bottom TPU film, electrode film and top TPU / CNTs spinning film cooperate with each other to ensure that the sensor has extremely high sensitivity, accuracy and extremely fast response time. The silver electrode film with sandpaper microstructure and the three-dimensional tubular carbon nanotubes with good electrical properties further enhance the detection capability of the sensor. This highly sensitive design enables the sensor to accurately detect tiny bending changes, ensuring that the system can provide accurate data when monitoring the bending of the surface of an object in real time.
[0047] The flexible bending sensor of this embodiment can adapt to a variety of surfaces and environments: the softness and high adaptability of the flexible bending sensor enable it to be applied to various complex surfaces without being restricted to specific shapes or materials. This feature enables the system to have broad application prospects in multiple fields, such as medical equipment, robots, wearable devices, electronic skin, etc.
[0048] A further technical solution, a flexible actuator, comprises: a nickel-titanium shape memory alloy as a substrate, and a flexible substance wrapped outside the substrate;
[0049] Optionally, the wrapped flexible substance is silicone rubber;
[0050] In this embodiment, the flexible actuator uses nickel-titanium shape memory alloy as a matrix and is wrapped with flexible silicone rubber, so that the actuator is more flexible when generating bending strain. SMA shape memory alloy can restore a predetermined shape when heated; SMA shape memory alloy can provide a large force under a small DC stimulation that does not affect the external environment, so that the actuator can be applied to multiple load-required scenarios and provide a stable actuation effect.
[0051] A further technical solution is to apply the flexible sensor and the flexible actuator on both sides of the orthogonal direction of the object's bending, respectively. The flexible sensor can identify the bending condition in real time when the object is bent, and the bending strain of the flexible actuator assists the actuation strain.
[0052] Furthermore, a strain adjustment method of the strain adjustment system based on the above-mentioned flexible sensor and actuator comprises the following steps:
[0053] Detect the bending of the object surface based on flexible sensors;
[0054] Compare the search results with the set threshold;
[0055] The actuator is controlled to generate corresponding bending strain according to the comparison result of the detection data.
[0056] In this embodiment, the flexible sensor can accurately detect the bending condition of the surface of the object in real time and provide high-precision bending data. This real-time detection capability ensures that the system can respond quickly to external changes. By comparing the detection results with the preset threshold, the system can automatically determine whether strain adjustment is required. This automated judgment and adjustment process reduces manual intervention and improves work efficiency. Precise control can be achieved. The system controls the actuator to generate corresponding bending strain according to the comparison results of the detection data, ensuring the accuracy and reliability of the adjustment process. The actuator can accurately adjust the degree of bending as needed, so that the surface of the object can reach the expected bending state. By accurately controlling the strain adjustment, excessive bending or insufficient bending is avoided, and the object to be adjusted can be protected.
[0057] Example 2
[0058] Based on Example 1, this example provides a method for preparing a flexible bending sensor in Example 1, such as Figures 1 to 6 As shown, the following steps are included:
[0059] Step 1, dissolving TPU in an organic solvent, pouring it into a culture dish after magnetic stirring, and placing it in an oven to dry the surface solvent to obtain a TPU elastic adhesive film as a bottom film;
[0060] Step 2, dissolving polyurethane in an organic solvent, preparing a TPU spinning film by an electrospinning process, and putting it into a dispersed multi-walled carbon nanotube solution after hydrophilic treatment, so that the carbon nanotube conductive material is entangled in the TPU spinning film to obtain a TPU / CNTs spinning film;
[0061] Step 3, preparing a silicone rubber film with a microporous structure, and depositing a layer of silver as a silver electrode by magnetron sputtering;
[0062] Step 4, attaching two silver electrodes to the bottom film, and then covering the two silver electrodes with TPU / CNTs spinning film to obtain the prepared flexible bending sensor;
[0063] In this embodiment, the TPU spinning film has good air permeability and will not react when applied to the surface of an object. The TPU nano spinning fiber structure is wrapped with a carbon nanotube conductive material to improve the wearable air permeability and sensitivity. At the same time, the electrospinning preparation process is simple and can be prepared on a large scale.
[0064] Step 1 is the preparation of the bottom film, including: dissolving TPU in an organic solvent, pouring it into a glass culture dish after sufficient magnetic stirring, and placing it in an oven to dry the surface solvent to obtain a TPU elastic adhesive film as the bottom film;
[0065] Specifically, the organic solvent may be any one of N,N-dimethylformamide, tetrahydrofuran, acetone, or a mixture of several organic solvents;
[0066] Optionally, the temperature of the oven may be 60 degrees Celsius;
[0067] In step 2, the method for preparing a TPU / CNTs spinning film of a functional layer comprises:
[0068] Step 21, preparation of a conductive solution: placing multi-walled carbon nanotubes in a glass bottle, dripping in a carbon nanotube oil dispersant, adding deionized water that covers the powder, sealing the glass bottle and performing ultrasonic treatment to obtain an ultrasonically dispersed multi-walled carbon nanotube solution;
[0069] Optionally, the glass bottle can be sealed with a sealing adhesive;
[0070] Among them, the carbon nanotube oil dispersion can be dropped into a glass bottle;
[0071] Optionally, the ultrasonic treatment may be: placing the sealed glass bottle in an ultrasonic tank, ultrasonically treating for 60 minutes, and then ultrasonically treating for 30 minutes using a pulse signal;
[0072] Step 22, preparing a spinning solution, dissolving polyurethane (TPU) in an organic solvent, fully stirring the solution with magnetic force to dissolve, using an electrostatic spinning process to prepare a TPU spinning film, and using ion treatment to make the surface of the spinning film hydrophilic;
[0073] Specifically, the organic solvent is the same as that in step 1, and can be any one of N,N-dimethylformamide, tetrahydrofuran, acetone, or a mixture of several organic solvents;
[0074] Among them, the spinning film thickness can be prepared to be 100μm;
[0075] Optionally, the TPU spinning film is treated with a polydopamine solution to make it hydrophilic;
[0076] A feasible technical solution is a method for preparing a TPU spinning solution, specifically, using granular polyurethane (1185A) as a solute to obtain a solution with a concentration of 8-28wt%, magnetically stirring at 200-500rpm for 8h to obtain a spinning solution, and the temperature control is set to 60-90°C;
[0077] Preferably, the concentration of the TPU spinning solution is 18 wt %.
[0078] A feasible technical solution is the preparation of TPU spinning film, specifically: preparing TPU fiber membrane by electrospinning, the spinning speed is 1-1.5ml / h, the voltage is set to 12KV-18KV, the receiving distance can be set to 12-18cm, and the spinning duration can be 2-6h.
[0079] After spinning, TPU polyurethane is non-toxic and has good biocompatibility. It is breathable and does not easily cause water vapor problems when worn for a long time or applied to the object. The TPU film prepared by the electrospinning process has a unique three-dimensional structural skeleton. The microstructure prepared by this process has a three-dimensional skeleton with many gaps, which provides excellent air permeability, is beneficial to the heat exchange between the object and the external environment, and improves the comfort of application. At the same time, the preparation cost of this microstructure is low, the preparation area is large, and the process is simple and popular, which can realize substantial batch application.
[0080] Step 23, immersing the hydrophilic treated TPU spinning film in the ultrasonically dispersed multi-walled carbon nanotube solution, sealing the bottle mouth with sealing glue, and performing ultrasonic treatment to obtain a TPU / CNTs spinning film as a functional layer;
[0081] Specifically, the hydrophilic treated TPU spinning film is immersed in multi-walled carbon nanotube (CNT) solutions of different concentrations and subjected to ultrasonic treatment for 30-60 minutes, so that the multi-walled carbon nanotubes are wound around the TPU spinning to obtain a TPU / CNTs spinning film.
[0082] A specific implementation example is a method for preparing a TPU / CNTs spinning film from a TPU spinning film, as follows:
[0083] (a) quantitatively diluting multi-walled carbon nanotubes to obtain multi-walled carbon nanotube solutions with different concentrations;
[0084] (b) soaking the hydrophilic treated TPU spinning film in multi-walled carbon nanotube solutions of different concentrations for ultrasonic treatment for 2-6 hours for standby use;
[0085] (c) subjecting the immersed TPU spinning film to ultrasonic treatment in the multi-walled carbon nanotube solution for 45 min with an interval of 10 min, and repeating it twice for standby use;
[0086] (d) The TPU film after ultrasonic treatment in step (c) was immersed for another 45 min to obtain a TPU / CNTs nanofiber membrane.
[0087] In the above scheme, the TPU spinning film immersed in the multi-walled carbon nanotube solution is placed in an ultrasonic environment, and the conductive material can be penetrated by ultrasound;
[0088] In step 4, for electrode preparation, the silicone rubber is evenly mixed and spin-coated on a sandpaper template in a ratio of 1:1 and dried to obtain a silicone rubber film with a microporous structure, and a layer of silver is deposited by magnetron sputtering as a silver electrode;
[0089] Specifically, the A agent and the B agent of silicone rubber (abbreviated as PDMS) were mixed in a mass ratio of 1:1 and stirred evenly, and then dropped into a glass culture dish using a dropper and spin-coated evenly, and after the surface was dried, a 200 nm silver layer was magnetron sputtered;
[0090] In step 4, the specific process of preparing the silver electrode is as follows:
[0091] (a) Mix PDMS A and B in a ratio of 1:1 and stir evenly with a dropper;
[0092] (b) placing the PDMS mixture in a vacuum box to remove the inner bubbles and keep the solution uniform for later use;
[0093] (c) Cut a piece of 800-grit sandpaper of appropriate size, lay it flat on the glass plate, and slowly pour the PDMS mixture into it;
[0094] (d) using a spin coating process at a speed of 200 m / s and a time of 30 s, the mixed solution was evenly coated on the surface of the sandpaper, and then placed in a 60° C. oven for drying for 1 h;
[0095] (e) The silver target was sputtered onto the PDMS surface using a magnetron sputtering process with a power of 40 W and a sputtering time of 10 min. After the sputtering was completed, a soft silver electrode with a microstructure on the surface was obtained.
[0096] The flexible bending sensor prepared based on the above method includes: from bottom to top, a bottom film, an electrode film and a top film; the bottom film is a TPU film as a tape film, the electrode film is a silver electrode film, and the top film is a spun carbon nanotube film.
[0097] The three-layer membrane prepared above is assembled, with the TPU film as the bottom layer, the electrode as the middle layer, and the TPU / CNTs spinning film as the upper layer. After assembly, such a device can not only ensure high sensitivity under high and small strains, but also be designed to fit various application scenarios.
[0098] The above-mentioned flexible bending sensor has a larger strain distance at both ends than in the middle when the strain is small, and has a better response. Therefore, the electrodes are at both ends. When the strain is small, the protruding part of the electrode first contacts the functional layer to form a conductive path, generating a resistance change signal; when the strain is large, most of the protruding part of the electrode contacts the TPU / CNTs spinning film. As the bending angle increases, the silver electrode recessed in the microstructure contacts the TPU / CNTs spinning film, forming more conductive paths, and the resistance further decreases. The concave and convex sandpaper microstructure on the electrode surface, the electrospinning three-dimensional microstructure, and the overall structural design of the sensor are all helpful in improving the sensitivity of the sensor.
[0099] Example 3
[0100] This embodiment provides a method for preparing a flexible actuator in embodiment 1, such as Figures 7 to 11 As shown, the following steps are included:
[0101] Step 1, dope the PDMS reagent A and reagent B at a ratio of 1:10, stir evenly, put into a vacuum box, evacuate and remove bubbles, and obtain a PDMS solution;
[0102] Step 2: Use nickel-titanium shape memory alloy as a substrate, wrap the PDMS solution, and dry it to obtain an SMA actuator wrapped in a soft shell.
[0103] In step 1, the A and B reagents of PDMS were doped at a ratio of 1:10, stirred for 10 minutes, and then placed in a vacuum box to evacuate and remove bubbles;
[0104] Nickel-titanium shape memory alloy (SMA) is a material with shape memory effect;
[0105] In some embodiments, the nickel-titanium shape memory alloy can be selected to have a diameter of 0.8 mm and a cut length of 5 cm;
[0106] In step 2, the method of wrapping the PDMS solution with the nickel-titanium shape memory alloy is as follows:
[0107] Step 21, spin-coat the prepared PDMS solution on a culture dish, the thickness of which may be 0.8-1.6 mm;
[0108] Step 22: When the PDMS on the culture dish is not completely solidified, lay nickel-titanium shape memory alloy on it, and perform step 21 in the same way to spin-coat a layer of PDMS on the other side of the nickel-titanium shape memory alloy to obtain the nickel-titanium shape memory alloy wrapped in the PDMS solution, and put it into a 60°C oven for drying to obtain the SMA actuator wrapped in a soft shell.
[0109] In this embodiment, a nickel-titanium shape memory alloy that can cause stress changes under external stimuli is used as a matrix to memorize corresponding shapes in various application scenarios, thereby achieving strain that meets the scenario.
[0110] In some embodiments, the method of setting a memory shape for a nickel-titanium shape memory alloy may be: bending a martensitic SMA at room temperature into a specific shape, keeping the shape unchanged and annealing at 200° C. for 20 seconds under a heat gun to obtain an actuator SMA substrate with a memory shape;
[0111] Among them, the annealing temperature and annealing time can be determined according to specific circumstances.
[0112] In some other embodiments, the SMA wire may be bent into a U-shape and uniformly heated at 300° C. for 5-8 seconds using a heat gun, so that the SMA wire memorizes the U-shape;
[0113] After the PDMS wraps the SMA evenly, the drying method can be: placing it in a 60°C oven for drying for 40 minutes, thereby obtaining the SMA actuator wrapped with a soft shell;
[0114] In the above scheme, the principle of the SMA actuator is that the SMA wire will produce strain and contraction after being heated and electrically stimulated, and restore its state of bending with the object to the original memory shape, so as to achieve the purpose of assisting the flexible object to strain. The preparation of the flexible actuator of this embodiment is also simple and can be prepared in batches, and the thickness of the actuator can be changed according to the application.
[0115] The performance indicators of flexible actuators depend on application requirements. The actuator needs to undergo bending strain. The load capacity and the relationship between power supply and strain speed can be determined through testing. Compared with chemical actuators, SMA actuators have a large strain range and strong load capacity, which can greatly broaden the application scenarios.
[0116] There are many types of flexible actuators and their preparation methods. Based on the mature industrialization of SMA wire, using SMA as the actuator element instead of using chemical methods is very suitable for application on biological surfaces such as plants. In order to be able to intuitively represent the changes in the actuator strain, such as Figure 6 As shown in the figure, it shows the spatial change before and after the actuator responds. According to the characteristics of SMA, the magnitude of the DC current will have a great influence on the SMA metal strain rate, such as Figure 7 In order to achieve the performance of driving the auxiliary strain of plant leaves, the maximum load under different DC currents was tested with different thicknesses of the actuator, as shown in Figure 1. Figure 8 shown.
[0117] Example 4
[0118] Based on Example 2, this example provides a specific implementation scheme of a method for preparing a flexible bending sensor of Example 2, comprising the following steps:
[0119] (A1) Preparation of TPU spinning solution: using granular polyurethane (1185A) as a solute to obtain a solution with a concentration of 8-28 wt%, magnetically stirring at 200-500 rpm for 8 h to obtain a spinning solution, and setting the temperature to 60-90° C. to obtain a uniform spinning solution;
[0120] (A2) Preparation of TPU spinning film: TPU spinning film was prepared by electrospinning, with a spinning speed of 1-1.5 ml / h, a voltage of 12 KV-18 KV, a receiving distance of 12-18 cm, and a spinning duration of 4 h;
[0121] (A3) Hydrophilic treatment of TPU spun film: 0.01 g of polydopamine was dissolved in a buffer solution with a pH value of 8.5, and ultrasonic dispersion was performed for 30 min. The TPU spun film prepared in (A2) was immersed in the buffer solution and ultrasonicated for 20 min. After immersion for 4 h, the film was taken out and dried in a dryer at 60° C. for later use.
[0122] (A4) Preparation of TPU / CNTs spinning film: 30 mg of CNTs powder was weighed and added to 24 ml of deionized water, and ultrasonic dispersion was performed for 30 min. Then, the soaked TPU spinning film was ultrasonically treated in a multi-walled carbon nanotube solution for 45 min. The process was repeated twice with an interval of 10 min to obtain a TPU / CNTs nanofiber membrane.
[0123] (A5) Electrode preparation: Mix PDMS agent A and agent B in a ratio of 1:1, stir evenly with a dropper, put the PDMS mixture into a vacuum box to remove the inner bubbles, keep the solution uniform, spread sandpaper flat on a glass plate, slowly pour the PDMS mixture onto the sandpaper using a spin coating process at a speed of 200 m / s for 30 seconds, spin coat the sandpaper surface with the mixture evenly, put the mixture into a 60°C oven and dry it for 1 hour, and sputter the silver target onto the PDMS surface using a magnetron sputtering process at a power of 40 W for 10 minutes. After the sputtering is completed, a soft silver electrode with a microstructure on the surface is obtained;
[0124] In this embodiment, the performance difference of the flexible sensor obtained by changing the preparation conditions is that the spinning duration of the TPU spun film is 4 hours; the obtained flexible sensor has a moderate thickness and a small tensile modulus.
[0125] Based on Example 3, this example provides a specific implementation scheme of a method for preparing a flexible actuator of Example 3, comprising the following steps:
[0126] (B1) Select SMA metal with a diameter of 0.8 mm and a length of 5 cm, bend the SMA wire into a U shape, and use a heat gun to evenly heat it at 300°C for 5-8 seconds to make the SMA memorize the U shape;
[0127] (B2) Mix PDMS A and B in a ratio of 1:10 and stir evenly with a dropper. Place the PDMS mixture in a vacuum box to remove the inner bubbles and keep the solution uniform. Weigh 2-6g of PDMS to evenly wrap the SMA and dry it in a 60℃ oven for 40min to obtain the SMA actuator wrapped in a soft shell.
[0128] Example 5
[0129] Based on Example 2, this example provides a specific implementation scheme of a method for preparing a flexible bending sensor of Example 2, comprising the following steps:
[0130] (A1) Preparation of TPU spinning solution: Granular polyurethane (1185A) was used as a solute to obtain a solution with a concentration of 8%-28% by weight, and magnetic stirring was performed at 200-500 rpm for 8 h to obtain a spinning solution. The temperature was set at 60-90° C. to obtain a uniform spinning solution.
[0131] (A2) Preparation of TPU spinning film: TPU fiber membrane was prepared by electrospinning, the spinning speed was 1-1.5 ml / h, the voltage was set to 12 KV-18 KV, the receiving distance was set to 12-18 cm, and the spinning duration was 4 h;
[0132] (A3) Hydrophilic treatment of TPU spun film: 0.01 g of polydopamine was dissolved in a buffer solution with a pH value of 8.5, and ultrasonic dispersion was performed for 30 min. The TPU spun film prepared in (A2) was immersed in the buffer solution, and ultrasonic dispersion was performed for 20 min. After immersion for 4 h, the film was taken out and dried in a dryer at 60° C. for later use.
[0133] (A4) Preparation of TPU / CNTs spinning film: 30 mg of CNTs powder was weighed and added into 12 ml of deionized water, and ultrasonic dispersion treatment was performed for 30 min. Then, the soaked TPU spinning film was ultrasonically treated in a multi-walled carbon nanotube solution for 45 min, and the process was repeated twice with an interval of 10 min to obtain a TPU / CNTs nanofiber membrane.
[0134] (A5) Electrode preparation: Mix PDMS agent A and agent B in a ratio of 1:1, stir evenly with a dropper, put the PDMS mixture into a vacuum box to remove the inner bubbles, keep the solution uniform, spread sandpaper flat on a glass plate, slowly pour the PDMS mixture onto the sandpaper using a spin coating process at a speed of 200 m / s for 30 seconds, spin coat the sandpaper surface with the mixture evenly, put the mixture into a 60°C oven and dry it for 1 hour, and sputter the silver target onto the PDMS surface using a magnetron sputtering process at a power of 40 W for 10 minutes. After the sputtering is completed, a soft silver electrode with a microstructure on the surface is obtained;
[0135] Compared with Example 4, in the preparation process of TPU / CNTs spinning film in this embodiment, 30 mg of CNTs powder and 12 ml of deionized water are used to prepare the solution. The CNTs solution concentration is higher, and under the same ultrasonic preparation time, the conductivity is better and the initial resistance is reduced, which is beneficial to improve the sensitivity.
[0136] The TPU tape is attached to the bottom surface of the object, the electrodes prepared in (A5) are placed at both ends, the TPU / CNTs film prepared in (A4) is covered on the electrodes, and the electrodes at both ends are fixed.
[0137] Example 6
[0138] Based on Example 2, this example provides a specific implementation scheme of a method for preparing a flexible bending sensor of Example 2, comprising the following steps:
[0139] (A1) Preparation of TPU spinning solution: Granular polyurethane (1185A) was used as a solute to obtain a solution with a concentration of 8-28 wt %, and magnetic stirring was performed at 200-500 rpm for 8 h to obtain a spinning solution. The temperature was set to 60-90° C. to obtain a uniform spinning solution.
[0140] (A2) Preparation of TPU spinning film: TPU spinning film was prepared by electrospinning, with a spinning speed of 1-1.5 ml / h, a voltage of 12 KV-18 KV, a receiving distance of 12-18 cm, and a spinning duration of 4 h;
[0141] (A3) Hydrophilic treatment of TPU spun film: 0.01 g of polydopamine was dissolved in a buffer solution with a pH value of 8.5, and ultrasonic dispersion was performed for 30 min. The TPU spun film prepared in (A2) was immersed in the buffer solution, and ultrasonic dispersion was performed for 20 min. After immersion for 4 h, the film was taken out and dried in a dryer at 60° C. for later use.
[0142] (A4) Preparation of TPU / CNTs spinning film: 30 mg of CNTs powder was weighed and added to 6 ml of deionized water, and ultrasonic dispersion was performed for 30 min. Then, the soaked TPU spinning film was ultrasonically treated in a multi-walled carbon nanotube solution for 45 min. The process was repeated twice with an interval of 10 min to obtain a TPU / CNTs nanofiber membrane.
[0143] (A5) Electrode preparation: Mix PDMS agent A and agent B in a ratio of 1:1, stir evenly with a dropper, put the PDMS mixture into a vacuum box to remove the inner bubbles, keep the solution uniform, spread sandpaper flat on a glass plate, slowly pour the PDMS mixture onto the surface of the sandpaper using a spin coating process at a speed of 200 m / s for 30 seconds, spin coat the mixture evenly on the surface of the sandpaper, put it into a 60°C oven and dry it for 1 hour, and sputter the silver target onto the PDMS surface using a magnetron sputtering process at a power of 40 W for 10 minutes. After the sputtering is completed, a soft silver electrode with a microstructure on the surface is obtained;
[0144] Compared with Examples 4 and 5, in the preparation process of TPU / CNTs spun film in this embodiment, 30 mg of CNTs powder was added to 6 ml of deionized water to prepare the solution. As the concentration of the CNTs solution increased, the CNTs agglomerated and were not easy to disperse, resulting in a drastic change in resistance in a short period of time during the stretching of the spinning film.
[0145] Example 7
[0146] Based on Example 2, this example provides a specific implementation scheme of a method for preparing a flexible bending sensor of Example 2, comprising the following steps:
[0147] (A1) Preparation of TPU spinning solution: Granular polyurethane (1185A) was used as a solute to obtain a solution with a concentration of 8% by weight, and magnetic stirring was performed at 200-500 rpm for 8 h to obtain a spinning solution. The temperature was set at 60-90° C. to obtain a uniform spinning solution.
[0148] (A2) Preparation of TPU spinning film: TPU spinning film was prepared by electrospinning, with a spinning speed of 1-1.5 ml / h, a voltage of 12 KV-18 KV, a receiving distance of 12-18 cm, and a spinning duration of 4 h;
[0149] (A3) TPU fiber membrane hydrophilic treatment: 0.01 g of polydopamine was dissolved in a buffer solution with a pH value of 8.5, and ultrasonic dispersion was performed for 30 min. The TPU spun film prepared in (A2) was immersed in the buffer solution, and ultrasonic dispersion was performed for 20 min. After immersion for 4 h, the film was taken out and dried in a dryer at 60° C. for later use.
[0150] (A4) Preparation of TPU / CNTs spinning film: 30 mg of CNTs powder was weighed and added to 24 ml of deionized water, and ultrasonic dispersion was performed for 30 min. Then, the soaked TPU spinning film was ultrasonically treated in a multi-walled carbon nanotube solution for 45 min. The process was repeated twice with an interval of 10 min to obtain a TPU / CNTs nanofiber membrane.
[0151] (A5) Electrode preparation: Mix PDMS agent A and agent B in a ratio of 1:1, stir evenly with a dropper, put the PDMS mixture into a vacuum box to remove the inner bubbles, keep the solution uniform, spread sandpaper flat on a glass plate, slowly pour the PDMS mixture onto the surface of the sandpaper using a spin coating process at a speed of 200 m / s for 30 seconds, spin coat the mixture evenly on the surface of the sandpaper, put it into a 60°C oven and dry it for 1 hour, and sputter the silver target onto the PDMS surface using a magnetron sputtering process at a power of 40 W for 10 minutes. After the sputtering is completed, a soft silver electrode with a microstructure on the surface is obtained;
[0152] Compared with Examples 4 to 6, in the preparation process of the TPU spinning solution in this embodiment, granular polyurethane (1185A) is used as a solute to obtain a solution with a concentration of 8% Wt. The effect is that the spinning film has good flexibility, matches the application environment of slight stretching, and reduces the constraint of the sensor on the object being used.
[0153] Example 8
[0154] Based on Example 2, this example provides a specific implementation scheme of a method for preparing a flexible bending sensor of Example 2, comprising the following steps:
[0155] (A1) Preparation of TPU spinning solution: Granular polyurethane (1185A) was used as a solute to obtain a solution with a concentration of 18% by weight, and magnetic stirring was performed at 200-500 rpm for 8 h to obtain a spinning solution. The temperature was set at 60-90° C. to obtain a uniform spinning solution.
[0156] (A2) Preparation of TPU spinning film: TPU fiber membrane was prepared by electrospinning, the spinning speed was 1-1.5 ml / h, the voltage was set to 12 KV-18 KV, the receiving distance was set to 12-18 cm, and the spinning duration was 4 h;
[0157] (A3) Hydrophilic treatment of TPU spun film: 0.01 g of polydopamine was dissolved in a buffer solution with a pH value of 8.5, and ultrasonic dispersion was performed for 30 min. The TPU spun film prepared in (A2) was immersed in the buffer solution, and ultrasonic dispersion was performed for 20 min. After immersion for 4 h, the film was taken out and dried in a dryer at 60° C. for later use.
[0158] (A4) Preparation of TPU / CNTs spinning film: 30 mg of CNTs powder was weighed and added to 24 ml of deionized water, and ultrasonic dispersion was performed for 30 min. Then, the soaked TPU spinning film was ultrasonically treated in a multi-walled carbon nanotube solution for 45 min. The process was repeated twice with an interval of 10 min to obtain a TPU / CNTs nanofiber membrane.
[0159] (A5) Electrode preparation: Mix PDMS agent A and agent B in a ratio of 1:1, stir evenly with a dropper, put the PDMS mixture into a vacuum box to remove the inner bubbles, keep the solution uniform, spread sandpaper flat on a glass plate, slowly pour the PDMS mixture onto the surface of the sandpaper using a spin coating process at a speed of 200 m / s for 30 seconds, spin coat the mixture evenly on the surface of the sandpaper, put it into a 60°C oven and dry it for 1 hour, and sputter the silver target onto the PDMS surface using a magnetron sputtering process at a power of 40 W for 10 minutes. After the sputtering is completed, a soft silver electrode with a microstructure on the surface is obtained;
[0160] Compared with Examples 4 to 7, in the preparation process of the TPU spinning solution in this example, granular polyurethane (1185A) is used as a solute to obtain a solution with a concentration of 18% Wt, which has the effect of taking into account both mechanical properties and soft stretchability.
[0161] Example 9
[0162] Based on Example 2, this example provides a specific implementation scheme of a method for preparing a flexible bending sensor of Example 2, comprising the following steps:
[0163] (A1) Preparation of TPU spinning solution: Granular polyurethane (1185A) was used as a solute to obtain a solution with a concentration of 28% by weight, and magnetic stirring was performed at 200-500 rpm for 8 h to obtain a spinning solution. The temperature was set at 60-90° C. to obtain a uniform spinning solution.
[0164] (A2) Preparation of TPU spinning film: TPU spinning film was prepared by electrospinning, with a spinning speed of 1-1.5 ml / h, a voltage of 12 KV-18 KV, a receiving distance of 12-18 cm, and a spinning duration of 4 h;
[0165] (A3) Hydrophilic treatment of TPU spun film: 0.01 g of polydopamine was dissolved in a buffer solution with a pH value of 8.5, and ultrasonic dispersion was performed for 30 min. The TPU spun film prepared in (A2) was immersed in the buffer solution, and ultrasonic dispersion was performed for 20 min. After immersion for 4 h, the film was taken out and dried in a dryer at 60° C. for later use.
[0166] (A4) Preparation of TPU / CNTs spinning film: 30 mg of CNTs powder was weighed and added to 6 ml of deionized water, and ultrasonic dispersion was performed for 30 min. Then, the soaked TPU spinning film was ultrasonically treated in a multi-walled carbon nanotube solution for 45 min. The process was repeated twice with an interval of 10 min to obtain a TPU / CNTs nanofiber membrane.
[0167] (A5) Electrode preparation: Mix PDMS agent A and agent B in a ratio of 1:1, stir evenly with a dropper, put the PDMS mixture into a vacuum box to remove the inner bubbles, keep the solution uniform, spread sandpaper flat on a glass plate, slowly pour the PDMS mixture onto the sandpaper using a spin coating process at a speed of 200 m / s for 30 seconds, spin coat the sandpaper surface with the mixture evenly, put the mixture into a 60°C oven and dry it for 1 hour, and sputter the silver target onto the PDMS surface using a magnetron sputtering process at a power of 40 W for 10 minutes. After the sputtering is completed, a soft silver electrode with a microstructure on the surface is obtained;
[0168] Compared with Examples 4 to 8, in the preparation process of the TPU spinning solution in this embodiment, granular polyurethane (1185A) is used as a solute to obtain a solution with a concentration of 28% Wt, which has the effect of obtaining a spinning membrane with stronger mechanical properties and stronger resistance to damage by stretching.
[0169] Example 9
[0170] The strain regulation system of Example 1 can be applied to human body, plants, animals, and human-computer interaction. It has a high sensitivity under small strain conditions and is suitable for monitoring small changes.
[0171] Based on Example 1, this example provides an application of the strain regulation system based on flexible sensors and actuators described in Example 1 in an auxiliary plant growth system, as shown in Figures 12 and 13.
[0172] The flexible bending sensor is attached to the upper surface of the blade. The flexible bending sensor can generate resistance changes when the blade is bent and strained, thereby obtaining a voltage change signal.
[0173] The flexible actuator is attached to the back of the blade, e.g. Fig.10 As shown, bending strain is generated when receiving power stimulation.
[0174] Furthermore, it also includes an acquisition circuit, through which a voltage change signal is acquired. When the transmission signal reaches the threshold of abnormal bending, the judgment result is executed. In order to assist plant growth, the actuator begins to respond and lifts the leaves to a normal position, which is beneficial to the growth trend of the plant. The overall plant bending sensing and feedback execution system, such as Fig. 9 shown.
[0175] In this embodiment, the controller of the acquisition circuit can use an 80C51 single-chip microcomputer, which can collect sensor signals and set thresholds to identify bending signals, and at the same time give a switch signal to open or close the relay, thereby controlling the power supply of the actuator and providing targeted feedback to the plant.
[0176] The ADC0804 module built into the 80C51 series single-chip microcomputer platform is used to collect voltage, which can achieve 8-bit high-precision signal collection. The voltage signal collected by ADC0804 is judged by the threshold, and the signal exceeding the voltage threshold, that is, the bending strain requires actuator auxiliary compensation, is transmitted to the relay as a switch signal. The relay controls whether the power circuit is open.
[0177] Compared with the existing application system design, most application systems can only realize sensor acquisition and identification, and can only reflect the values collected by the sensors. The perception feedback assisted plant growth system composed of flexible bending sensors and flexible actuators can realize acquisition and identification and feedback, process the collected signal data, and the actuator adjusts the bending strain of the application object according to the abnormal signal feedback, thereby realizing auxiliary adjustment of plant growth.
[0178] The above description is only a preferred embodiment of the present disclosure and is not intended to limit the present disclosure. For those skilled in the art, the present disclosure may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.
[0179] Although the above describes the specific implementation methods of the present disclosure in conjunction with the accompanying drawings, it is not intended to limit the scope of protection of the present disclosure. Technical personnel in the relevant field should understand that on the basis of the technical solution of the present disclosure, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present disclosure.
Claims
1. A strain regulation system based on flexible sensors and actuators, characterized in that: include: A flexible bending sensor, a flexible actuator and a processor, wherein the flexible bending sensor and the flexible actuator are respectively arranged on the surface of the object to be detected; The bending of the object surface is detected by a flexible bending sensor; the processor controls the flexible actuator to generate corresponding bending strain after judging the bending detection result.
2. The strain regulation system based on flexible sensor and actuator as claimed in claim 1, characterized in that: From bottom to top, they are the bottom film, electrode film and top film; The bottom film is TPU film as the tape film; The electrode film is a silver electrode film; The top film is a TPU / CNTs spun film, which is a TPU spun film wrapped with a carbon nanotube film.
3. The strain regulation system based on flexible sensor and actuator as claimed in claim 1, characterized in that: The flexible actuator includes: nickel-titanium shape memory alloy as a matrix, and a flexible substance wrapped outside the matrix.
4. The strain regulation system based on flexible sensor and actuator as claimed in claim 1, characterized in that: The flexible sensor and the flexible actuator are respectively attached to the two sides of the orthogonal direction of the object's bending. The flexible sensor can identify the bending condition in real time when the object bends, and the bending strain of the flexible actuator assists the actuation strain.
5. The strain adjustment method of the strain adjustment system based on the flexible sensor and the actuator according to any one of claims 1 to 4, characterized in that: Detect the bending of the object surface based on flexible sensors; Compare the search results with the set threshold; The actuator is controlled to generate corresponding bending strain according to the comparison result of the detection data.
6. The strain adjustment method of the strain adjustment system based on the flexible sensor and the actuator according to claim 5, characterized in that: A method for preparing a flexible bending sensor comprises the following steps: The TPU is dissolved in an organic solvent, poured into a petri dish after magnetic stirring, and placed in an oven to dry the surface solvent to obtain a TPU elastic adhesive film as a bottom film; The polyurethane is dissolved in an organic solvent, and a TPU spinning film is prepared by an electrospinning process. After a hydrophilic treatment, the film is placed in a dispersed multi-walled carbon nanotube solution, so that the carbon nanotube conductive material is entangled in the TPU spinning film, thereby obtaining a TPU / CNTs spinning film. Prepare a silicone rubber film with a microporous structure, and deposit a layer of silver as a silver electrode by magnetron sputtering; Two silver electrodes were attached to the underlying membrane, and then the TPU / CNTs spun film was covered on the two silver electrodes to obtain the prepared flexible bending sensor.
7. The strain adjustment method of the strain adjustment system based on the flexible sensor and the actuator according to claim 6, characterized in that: The organic solvent is any one of N,N-dimethylformamide, tetrahydrofuran, and acetone, or a mixture of several organic solvents; Alternatively, a method of preparing a TPU spinning solution by dissolving polyurethane in an organic solvent, specifically, using granular polyurethane as a solute to obtain a solution with a concentration of 8-28wt%, magnetically stirring at 200-500rpm for 8h to obtain a spinning solution, and the temperature control is set to 60-90°C; Alternatively, the preparation of TPU spinning film is specifically as follows: preparing TPU fiber membrane by electrospinning, the spinning speed is 1-1.5 ml / h, the voltage is set to 12 KV-18 KV, the receiving distance is set to 12-18 cm, and the spinning duration is 2-6 h; Alternatively, the specific process of preparing the silver electrode is as follows: Mix PDMS A and B in a ratio of 1:1 and stir evenly with a dropper; Put the PDMS mixed solution into a vacuum box to remove the inner bubbles and keep the solution uniform for later use; Cut sandpaper of set size, lay it flat on the glass plate, and slowly pour the PDMS mixture into it; Spin coating was performed with a speed of 200 m / s and a time of 30 s to evenly coat the sandpaper surface with the mixed solution, and then placed in a 60°C oven to dry for 1 h. The silver target was sputtered onto the PDMS surface using a magnetron sputtering process with a power of 40 W and a sputtering time of 10 min. After the sputtering was completed, a soft silver electrode with a microstructure on the surface was obtained.
8. The strain adjustment method of the strain adjustment system based on flexible sensor and actuator according to claim 5, characterized in that: A method for preparing a flexible actuator comprises the following steps: The PDMS reagent A and reagent B are mixed at a ratio of 1:10, stirred evenly, and then placed in a vacuum box to evacuate and remove bubbles to obtain a PDMS solution; The nickel-titanium shape memory alloy is used as a matrix, wrapped with a PDMS solution, and dried to obtain an SMA actuator wrapped in a soft shell.
9. The strain adjustment method of the strain adjustment system based on the flexible sensor and the actuator according to claim 8, characterized in that: The method of wrapping the nickel-titanium shape memory alloy with the PDMS solution is as follows: Step 21, spin-coat the prepared PDMS solution on a culture dish with a thickness of 0.8-1.6 mm; Step 22: When the PDMS on the culture dish is not completely solidified, lay nickel-titanium shape memory alloy on it, and perform step 21 in the same way to spin-coat a layer of PDMS on the other side of the nickel-titanium shape memory alloy to obtain the nickel-titanium shape memory alloy wrapped in the PDMS solution, and put it into a 60°C oven for drying to obtain the SMA actuator wrapped in a soft shell.
10. Application of the strain regulation system based on flexible sensors and actuators according to any one of claims 1 to 4 in a system for assisting plant growth; The flexible bending sensor is attached to the upper surface of the blade. The flexible bending sensor can generate resistance changes when the blade is bent and strained, thereby obtaining a voltage change signal. The flexible actuator is attached to the back of the blade and generates bending strain when stimulated by an electrical source.
Citation Information
Patent Citations
Flexible sensor and flexible signal detecting device
CN109059748A
Bionic sensing and executing integrated flexible actuator and preparation method thereof
CN109866480A
Flexible display apparatus and method for controlling thereof
CN110083298A
Sensing and driving integrated thin plate driver based on shape memory alloy
CN111396274A
Piezoelectric flexible pressure sensor produced from all-organic material and produced method
CN112284576A