Magnesium-iron hydrotalcite-based nano composite material as well as preparation method and application thereof

In the treatment of osteosarcoma, magnesia-iron hydrotalcite-based nanocomposites are used to synthesize MgFe-LDH nanosheets by co-precipitation method and load selenium nanoparticles, which solves the problems of insufficient limb salvage tumor resection and low stability of selenium nanoparticles, and achieves Targeted treatment of tumors and bone regeneration prevents drug-resistant bacterial infections, significantly improving treatment efficiency and safety.

CN118750602APending Publication Date: 2024-10-11QUZHOU INSTITUTE FOR INNOVATION IN RESOURCE CHEMICAL ENGINEERING
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410806701.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing technology is not effective in limb-sparing tumor resection in the treatment of osteosarcoma. Neoadjuvant chemotherapy is accompanied by adverse reactions. Traditional phototherapy has difficulty penetrating. Selenium nanoparticles have low stability and are difficult to effectively inhibit drug-resistant bacterial infection and tumor recurrence.

Method used

Magnesia-iron hydrotalcite-based nanocomposites are used to synthesize MgFe-LDH nanosheets through co-precipitation method, and selenium nanoparticles are loaded on the surface to promote SOD enzyme activation and Fenton reaction, increase ROS generation, and enhance targeted therapy and bone regeneration capabilities. .

Benefits of technology

It achieves specific treatment of tumor tissue, prevents drug-resistant bacterial infection, prevents tumor recurrence, and induces bone regeneration, significantly improving treatment efficiency and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118750602A_ABST
    Figure CN118750602A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of biomedicine, in particular to a magnesium-iron hydrotalcite-based nanocomposite and a preparation method and application thereof.The preparation method comprises the following steps that a mixed metal salt solution containing magnesium salt and iron salt, an alkaline solution and a sodium nitrate solution are mixed and subjected to a coprecipitation reaction, and magnesium-iron hydrotalcite nanosheets are obtained; and stirring and mixing the magnesium-iron hydrotalcite nanosheet and a sodium selenite solution, and then mixing with an L-cysteine aqueous solution to obtain the magnesium-iron hydrotalcite-based nano composite material. H2O2 is converted into highly toxic reactive oxygen species (ROS) through Fe < 3 + >, an efficient tumor targeted chemodynamic therapy (CDT) effect is shown in an acidic tumor microenvironment (TME), the activity of SOD enzyme is remarkably enhanced through loaded SeNPs, O2 <-> is converted into H2O2, and the excellent anti-tumor characteristic is shown.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of biomedicine, and in particular to a magnesium-iron hydrotalcite-based nanocomposite material and a preparation method and application thereof. Background Art

[0002] Osteosarcoma usually occurs in adolescents and children and is the second leading cause of cancer-related death in adolescents, second only to hematological malignancies. Despite significant advances in the concepts and technologies of osteosarcoma treatment, including limb-sparing tumor resection and neoadjuvant chemotherapy, limb-sparing tumor resection often fails to completely eradicate the tumor, while neoadjuvant chemotherapy is associated with many adverse reactions, such as bone marrow suppression. At the same time, minimizing the extent of tumor resection to promote postoperative functional recovery has attracted widespread attention. In addition, periprosthetic infection, especially infection caused by resistant bacteria, can lead to prosthesis failure and refractory systemic inflammatory response, which has a significant impact on the life safety of fragile osteosarcoma patients. In recent years, multifunctional light-based biomaterials that can simultaneously prevent tumor recurrence and induce bone formation have been widely explored, such as photothermal or photodynamic therapy. However, bone tissue is usually covered by thick muscle and skin layers, which makes it difficult for traditional light to penetrate the human body, thus greatly limiting the clinical application of these light-based therapies. In contrast, chemodynamic therapy (CDT), which is activated by the tumor microenvironment (TME) and triggers the Fenton reaction to produce reactive oxygen species (ROS), has extremely high therapeutic efficiency and almost negligible side effects, and has shown great promise in targeting deep tissue tumors.

[0003] Selenium is an essential trace element that plays a key role in physiological bone metabolism. Selenium deficiency has been reported to lead to abnormal bone metabolism and induce osteodystrophy, an endemic osteochondrosis. Selenium nanoparticles (SeNPs) can activate superoxide dismutase (SOD) to convert O 2- , which is converted into H2O2, thereby increasing the H2O2 level within the tumor. However, SeNPs exhibit low stability and are prone to micron-scale aggregation, resulting in impaired biocompatibility and bioreactivity. Therefore, it is crucial to enhance the dispersibility of SeNPs to inhibit aggregation. In addition, SeNPs have been reported to have antibacterial properties against both Gram-positive and Gram-negative bacteria, but their effectiveness against difficult-to-treat drug-resistant bacteria is unclear.

[0004] Layered double hydroxides (LDHs) are a representative two-dimensional layered inorganic nanomaterial composed of adjustable metal elements within the layers and interlayer anions. The positively charged main layer of LDHs exerts electrostatic attraction on the negatively charged nanoparticles, and the temperature and alkalinity of LDHs are specific for targeting the acidic TME. Hydrotalcite-based nanomaterials with CDT efficiency have been widely used for tumor therapy. However, the CDT efficiency of conventional LDH-based nanomaterials is limited by low H2O2 levels and elevated glutathione (GSH) levels in the TME. On the other hand, incorporating osteogenic metal ions into LDHs can endow the nanosheets with the ability to induce bone regeneration, but it is difficult to repair bone defects of critical size relying solely on metal ions. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the present invention aims to provide a magnesium-iron hydrotalcite-based nanocomposite material and its preparation method and application. Based on the special structure and many adjustable functions of hydrotalcite, the present invention proposes to use hydrotalcite as the main body, adjust the specific metal ion composition of the main layer plate, introduce functional ions magnesium and iron into the layer plate, give the layer plate Fenton catalyst performance, and load SeNPs on its surface, so as to activate SOD enzyme to make O 2- Conversion to H2O2 and Fe 3+ The consumption of GSH further improves the efficiency of the Fenton reaction, produces a large amount of highly active ROS, improves the shortcomings of insufficient reactants in traditional CDT, and achieves the purpose of specific treatment of tumor tissue, tissue periprosthetic infection and inducing bone regeneration.

[0006] In order to achieve the above-mentioned object of the invention, the technical solution adopted by the present invention is:

[0007] Provided is a method for preparing a magnesium-iron hydrotalcite-based nanocomposite material, comprising the following steps:

[0008] A mixed metal salt solution, an alkaline solution and a sodium nitrate solution are mixed to perform a coprecipitation reaction to obtain hydrotalcite nanosheets; the metal salt in the mixed metal salt solution includes a magnesium salt and an iron salt; the magnesium salt preferably includes magnesium nitrate, magnesium chloride or magnesium sulfate; the iron salt preferably includes ferric nitrate, ferric chloride or ferric sulfate;

[0009] The hydrotalcite nanosheets, sodium selenite solution and L-cysteine ​​solution are mixed to obtain a selenium nanoparticle-combined MgFe-LDH nanosheet composite material.

[0010] Furthermore, Se nanoparticles combined with MgFe-LDH nanosheet composites were impregnated into BGS to obtain the multifunctional BGS@LDH / Se material.

[0011] Furthermore, the total concentration of magnesium salt and iron salt in the mixed metal salt solution is preferably 20-40 mmol / L, more preferably 30 mmol / L; the molar ratio of magnesium ion to iron ion in the mixed metal salt solution is preferably (2-4): more preferably 2.

[0012] Furthermore, the alkaline solution is preferably a sodium hydroxide aqueous solution; the concentration of the alkaline solution is preferably 0.10-0.20 mol / L, more preferably 0.15 mol / L. The molar ratio of the total molar amount of metal ions in the mixed metal salt solution to the alkali in the alkaline solution is preferably (4-6), more preferably 5. The alkaline solution is used to provide the necessary alkaline environment for the synthesis of MgFe-LDH.

[0013] Furthermore, the sodium nitrate solution is preferably prepared by mixing sodium formate and deionized water; the concentration of sodium nitrate in the sodium nitrate solution containing formamide is preferably 9-12 mmol / L, more preferably 10 mmol / L; the molar ratio of sodium nitrate to the total molar amount of the mixed metal salt solution is preferably 1:(2-4), more preferably 1:3. Sodium nitrate is used to provide NO 3- The charge balance of the laminate is maintained, and the sodium ions in the sodium nitrate will not affect the metal elements of the hydrotalcite laminate.

[0014] Furthermore, the process of mixing the mixed metal salt solution, the alkaline solution and the sodium nitrate solution is preferably: the mixed metal salt solution and the alkaline solution are simultaneously dripped into the sodium nitrate solution. The simultaneous dripping preferably ensures that the amount of the mixed metal salt solution and the alkaline solution added at the same time is substantially the same; the dripping speed is preferably 1 to 3 μL / s, more preferably 2 μL / s. The dripping method can fully ensure the mixing of the metal salt solution and the alkaline solution, so that the nucleation process can proceed smoothly, forming a good crystalline structure of the hydrotalcite, and ensuring the synergistic therapeutic effect of the subsequent materials.

[0015] Furthermore, during the dropping process, the mixed metal salt solution and the alkaline solution begin to co-precipitate to generate yellow flocs, which are MgFe-LDH.

[0016] Furthermore, the coprecipitation reaction time is preferably 15 to 30 minutes, more preferably 25 minutes; the pH value of the coprecipitation reaction is preferably 9 to 10. After the coprecipitation reaction is completed, the obtained product is preferably centrifuged and washed in sequence to obtain MgFe-LDH. The washing process is preferably washed with deionized water, and the number of deionized water washings is preferably 3 times.

[0017] Furthermore, after obtaining MgFe-LDH, MgFe-LDH and sodium selenite solution are stirred and mixed, and then mixed with L-cysteine ​​aqueous solution to obtain MFL-Se.

[0018] Furthermore, the molar ratio of the sodium selenite solution, the L-cysteine ​​solution and the magnesium-iron hydrotalcite nanosheets MgFe-LDH is (0.05-0.1): (0.1-0.3): (0.03-0.05), preferably 0.1:0.2:0.04.

[0019] Furthermore, in order to achieve the loading of SeNPs, MgFe-LDH is preferably used in the form of a hydrotalcite nanosheet colloidal solution. The preparation process of the hydrotalcite nanosheet colloidal solution is to mix MgFe-LDH with deionized water, quantitatively dilute it to 1-2 mg / mL, preferably 2 mg / mL, to obtain a MgFe-LDH colloidal solution, and seal it for storage.

[0020] Furthermore, the concentration of the sodium selenite solution is 0.1-0.2 mol / L, more preferably 0.1 mol / L, and the concentration of the L-cysteine ​​solution is 0.1-0.3 mol / L, more preferably 0.2 mol / L.

[0021] Furthermore, after obtaining the hydrotalcite nanosheet colloidal solution, preferably the MgFe-LDH colloidal solution and the sodium selenite solution are mixed and then the L-cysteine ​​solution is added. The mixing is preferably carried out under stirring at room temperature, and the stirring speed is preferably 1000-1400 r / min, more preferably 1200 r / min.

[0022] Furthermore, the loading temperature is preferably room temperature, and the loading time is preferably 6 to 10 hours, more preferably 8 hours. After the loading is completed, the obtained product is preferably centrifuged to obtain MFL-Se.

[0023] Furthermore, after obtaining MFL-Se, BGS was ultrasonically impregnated and then dried, which was repeated three times to obtain BGS@LDH / Se.

[0024] Furthermore, the ultrasonic time is 3 to 6 minutes, more preferably 5 minutes; the drying temperature is 50 to 70°C, more preferably 60°C.

[0025] The beneficial effects of the present invention are:

[0026] 1. The present invention adopts a coprecipitation method to synthesize MgFe-LDH hydrotalcite nanosheets, and then uses the hydrotalcite nanosheets as a carrier to load selenium nanoparticles SeNPs on the MgFe-LDH hydrotalcite nanosheets, wherein the high-valent metal ions (Fe 3+ ) will be reduced to divalent form by the reducing substance glutathione (GSH) in the tumor microenvironment and participate in the Fenton reaction; under GSH and low pH conditions, it can efficiently produce reactive oxygen species and kill tumor cells, effectively preventing drug-resistant bacteria-related periprosthetic infection and subsequent osteomyelitis.

[0027] 2. The SeNPs loaded on the Mg-Fe-Hydrotalcite-based nanocomposite prepared by the present invention aggregate on the hydrotalcite layer, promoting the activation of SOD enzyme and O 2- The conversion to H2O2 can improve the chemodynamic therapeutic effect of Fenton catalyst, which has a significant killing ability on tumor cells, thus achieving the effect of targeted and specific treatment. At the same time, BGS@LDH / Se can completely prevent the recurrence of in situ tumors after osteosarcoma resection and avoid deaths related to recurrence. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The AFM image of MgFe-LDH prepared in Example 1; wherein a is an AFM image, and b is a schematic diagram of the thickness of each sheet structure in the AFM image;

[0029] Figure 2 TEM image of MFL-Se prepared in Example 2;

[0030] Figure 3 This is the ESR graph of MFL-Se prepared in Example 2;

[0031] Figure 4 This is the UV-vis graph of the MFL-Se prepared in Example 2 after the reaction with GSH;

[0032] Figure 5 The cell activity diagram of 4T1 cells treated with MFL-Se prepared in Example 2 under neutral and weakly acidic conditions after irradiation with light;

[0033] Figure 6 The staining diagrams are of the cell survival status of 4T1 cells treated with MFL-Se prepared in Example 2 under neutral conditions and weakly acidic conditions;

[0034] Figure 7 This is a Western blot detection image of hBMSCs cells treated with MFL-Se prepared in Example 2;

[0035] Figure 8 This is a colony photo of methicillin-resistant Staphylococcus aureus treated with BGS@LDH / Se prepared in Example 3;

[0036] Fig. 9 Alkaline phosphatase (ALP) staining and Alizarin Red S (ARS) staining images of hBMSCs cells treated with BGS@LDH / Se prepared in Example 3. DETAILED DESCRIPTION

[0037] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0038] Example 1

[0039] Synthesis of MgFe-LDH nanosheets:

[0040] Mg(NO3)2 6H2O (0.2564 g) and Fe(NO3)3 9H2O (0.202 g) were dissolved in deionized water (50 mL) to obtain a salt solution.

[0041] Sodium nitrate (0.0425 g) was dissolved in deionized water (50 mL) to obtain a sodium nitrate solution.

[0042] Sodium hydroxide (0.3 g) was dissolved in deionized water (50 mL) to obtain an alkaline solution.

[0043] The salt solution and the sodium hydroxide solution were simultaneously and uniformly added to the sodium nitrate solution at a dropping speed of 2 μL / s, the pH value of the obtained mixture was controlled to be 9, and the coprecipitation reaction was carried out for 15 minutes under stirring until the dropping was completed; the obtained system was naturally cooled to room temperature, the obtained product was collected by centrifugation, and then washed three times with deionized water to obtain magnesium iron hydrotalcite nanosheets, recorded as MgFe-LDH, and deionized water was added to prepare a magnesium iron hydrotalcite colloidal solution with a concentration of 2 mg / mL.

[0044] Characterization and testing

[0045] 1) AFM test was performed on the MgFe-LDH prepared in Example 1. The results are shown in Figure 1 .Depend on Figure 1 It can be seen that MgFe-LDH presents a flake structure, is evenly distributed, and has a thickness of 10-12nm.

[0046] Example 2

[0047] Synthesis of MgFe-Hydrotalcite-based Nanocomposites (MFL-Se):

[0048] Na2SeO3 (0.0692 g) was dissolved in deionized water (4 mL) to obtain a sodium selenite solution. L-Cys (0.0969 g) was dissolved in deionized water (4 mL) to obtain an L-cysteine ​​solution.

[0049] 0.5 mL of sodium selenite solution was slowly added to 10 mL of MgFe-LDH suspension (2 mg / mL) prepared in Example 1 and stirred at room temperature for 8 h. Then, 1 mL of L-cysteine ​​solution was slowly added to the above suspension and stirred at room temperature for 30 min. The resulting system was naturally cooled to room temperature, the resulting product was collected by centrifugation, and then washed three times with deionized water to obtain a magnesium-iron hydrotalcite-based nanocomposite material loaded with SeNPs, denoted as MFL-Se, and deionized water was added to prepare a colloidal solution with a concentration of 2 mg / mL.

[0050] Characterization and testing

[0051] 2) The MFL-Se prepared in Example 2 was tested by TEM. The results are shown in Figure 2 ,Depend on Figure 2 It can be seen that the prepared MFL-Se has a hexagonal sheet structure, and SeNPs are loaded on MgFe-LDH.

[0052] 3) The MFL-Se prepared in Example 2 was subjected to ESR tests under different pH conditions (pH=7.4, pH=6.5). The results are as follows: Figure 3 As shown, from Figure 3 It can be seen that under neutral conditions, pH = 7.4, there is no ·OH signal, while under weakly acidic conditions, pH = 6.5, an obvious ·OH signal is generated, indicating that MFL-Se has good responsiveness to pH conditions.

[0053] 4) After mixing different concentrations of MFL-Se aqueous dispersions (0 μg / mL, 10 μg / mL, 20 μg / mL, 50 μg / mL and 100 μg / mL) with GSH (glutathione) aqueous solution (10 μmM), DTNB (5,5'-dithiobis(2-nitrobenzoic acid)) was added to test its ultraviolet absorption value at 420 nm. DTNB reagent reacts with GSH to generate a yellow substance, nitrothiobenzoic acid, which has ultraviolet visible absorption at 420 nm. The absorption value at 420 nm can be tested to reflect the change in the content of GSH in the system. The results are shown in Figure 4 , Figure 4 The UV-vis graph of GSH after the reaction of MFL-Se with different concentrations was characterized by 5,5'-dithiobis(2-nitrobenzoic acid) (DTNB). Figure 4 It can be seen that MFL-Se can consume GSH, resulting in a decrease in its content, which is due to the reaction between GSH and high-valent metal ions in the MFL-Se layer.

[0054] 5) After different concentrations (0.5 μg / mL, 1 μg / mL, 2 μg / mL, 5 μg / mL and 10 μg / mL) of MgFe-LDH prepared in Example 1 and MFL-Se prepared in Example 2 were incubated with 4T1 cells at pH = 6.5 for 12 hours, the cytotoxicity of different treatments was evaluated by MTT (thiazolyl blue) assay. The cell survival status was as follows: Figure 5 As shown, from Figure 5 It can be seen that when pH = 6.5, there is an obvious cell killing effect in the MFL-Se group, indicating that under the conditions of the tumor microenvironment, MFL-Se has a good tumor cell killing ability.

[0055] 6) The MFL-Se aqueous dispersion prepared in Example 2 was cultured under different pH conditions (pH = 7.4, pH = 6.5) for 12 h, then the cells were washed with PBS and stained with annexin (V-FITC) and propidium iodide (PI), and photographed under a fluorescence microscope. The results are shown in Figure 6 .Depend on Figure 6 From the live and dead cell staining of each treatment group, it can be seen that the MFL-Se group achieved a higher cell killing rate, indicating that MFL-Se has a good therapeutic effect on tumor cells.

[0056] Example 3

[0057] MFL-Se impregnated bioactive glass (BGS):

[0058] BGS was placed in the MFL-Se suspension (2 mg mL -1 ), ultrasonically treated for 5 min, and then thoroughly dried in an oven at 60 ° C. The whole process was repeated three times to obtain MFL-Se impregnated BGS, which was denoted as BGS@LDH / Se.

[0059] Characterization and testing

[0060] 7) After the BGS@LDH / Se prepared in Example 3 was co-cultured with hBMSCs cells for 17 days, BGS and BGS@LDH were set as control groups, and the activity of SOD enzyme was detected by Western blotting. The results were as follows: Figure 7 As shown, from Figure 7 It can be seen that BGS@LDH / Se can significantly induce the upregulation of superoxide dismutase 1 (SOD-1) protein expression and downregulation of phosphorylated signal transducer and activator of transcription 3 (p-STAT3) protein expression, indicating that LDH / Se-induced oxidative damage in Saos-2 cells is aggravated.

[0061] 8) The BGS@LDH / Se prepared in Example 3 was immersed in MRSA suspension and then implanted into the upper tibia bone defect to simulate postoperative periprosthetic infection. Muscle tissue bacteria around the scaffold were collected and cultured with LB agar. BGS and BGS@LDH were set as control groups. The results are shown in Figure 8. Figure 8 As shown, from Figure 8 It can be seen that a large number of colonies were formed in the BGS and BGS@LDH groups, while no colonies were formed in the BGS@LDH / Se group, indicating that BGS@LDH / Se has the ability to prevent periprosthetic infection.

[0062] 9) The BGS@LDH / Se prepared in Example 3 was co-cultured with hBMSCs for 14 days, and the osteogenic properties were studied by ALP staining and ARS detection. BGS and BGS@LDH were set as control groups. The results are shown in Figure 1. Fig. 9 As shown, from Fig. 9 It can be seen that compared with the control group and the BGS group, the calcium deposition activity of the BGS@LDH / Se group was significantly enhanced and the ALP activity was significantly increased, indicating that SeNPs and LDH act synergistically to enhance osteogenic performance.

[0063] The performance test of BGS@LDH / Se prepared in Example 3 showed that BGS@LDH / Se prepared in the present invention has a good therapeutic effect on tumor cells, can effectively prevent bacterial infection around the prosthesis, and has a strong osteogenic induction ability.

[0064] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

Claims

1. A method for preparing a magnesium-iron hydrotalcite-based nanocomposite material, characterized in that: The following steps are involved: A mixed metal salt solution including magnesium salt and iron salt, an alkaline solution and a sodium nitrate solution are mixed to perform a coprecipitation reaction to obtain magnesium-iron hydrotalcite nanosheets; The magnesium-iron hydrotalcite nanosheets and sodium selenite solution are stirred and mixed, and then mixed with an L-cysteine ​​aqueous solution to obtain a magnesium-iron hydrotalcite-based nanocomposite material.

2. The preparation method according to claim 1, characterized in that The iron salt includes iron nitrate, iron chloride or iron sulfate; the total concentration of magnesium salt and iron salt in the mixed metal salt solution is 20-40 mmol / L; the molar ratio of magnesium ion to iron ion in the mixed metal salt solution is 2-4.

3. The preparation method according to claim 1, characterized in that The concentration of the sodium nitrate is 9-12 mmol / L; the molar ratio of the sodium nitrate to the total molar amount of the magnesium salt and the iron salt in the mixed metal salt solution is 1:(2-4).

4. The preparation method according to claim 1, characterized in that The coprecipitation reaction time is 15 to 30 minutes; the pH value of the coprecipitation reaction is 9 to 10.

5. The preparation method according to claim 1, characterized in that The concentration of the sodium selenite solution is 0.1-0.2 mol / L, the concentration of the L-cysteine ​​solution is 0.1-0.3 mol / L, and the molar ratio of the sodium selenite solution, the L-cysteine ​​solution and the hydrotalcite nanosheets is (0.05-0.1): (0.1-0.3): (0.03-0.05).

6. The preparation method according to claim 1, characterized in that The method further includes ultrasonically treating the magnesium-iron hydrotalcite-based nanocomposite material with 3D-printed bioactive glass, drying the material, and repeating the process multiple times to obtain the magnesium-iron hydrotalcite-based nanocomposite material combined with the bioactive glass.

7. The preparation method according to claim 6, characterized in that The concentration of the magnesium-iron hydrotalcite-based nanocomposite material is 1-3 mg / mL; the ultrasonic time is 4-6 minutes; and the drying temperature is 50-70°C.

8. A composite material obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The magnesium-iron hydrotalcite-based nanocomposite material has a flaky morphology and a thickness of 10 to 12 nm.

9. Use of the magnesium-iron hydrotalcite-based nanocomposite material combined with bioactive glass according to any one of claims 6 to 7 in preparing products for treating osteosarcoma and periprosthetic infection and inducing bone regeneration.

10. Use of the magnesium-iron hydrotalcite-based nanocomposite material according to claim 8 in the preparation of a specific tumor treatment preparation.

Citation Information

Cited By

  • Composite bone repair material as well as preparation method and application thereof

    CN121313958A

  • Modified LDH composite material and application thereof in bone regeneration and bone tumor treatment

    CN121371209A

  • Modified ldh composites and their use in bone regeneration and treatment of bone tumors

    CN121371209B