Multi-channel cell-loaded nerve repair conduit with double patterned structure and preparation method thereof

By designing a multi-channel cell-laden nerve repair catheter with a dual patterned structure, and using spinning solution and UV curing technology combined with electrical stimulation, the structural and functional deficiencies of the nerve repair catheter in the existing technology are solved, and the effective use of cells is achieved. Directional migration and differentiation provide an efficient solution for nerve damage repair.

CN118750644AActive Publication Date: 2024-10-11ZHEJIANG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410739629.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-07
Publication Date
2024-10-11
Estimated Expiration
2044-06-07

AI Technical Summary

Technical Problem

Existing nerve repair conduit materials have structural and functional deficiencies and are unable to comprehensively and comprehensively support the nerve repair process. In particular, there are challenges in defect repair of large gaps and cell orientation and differentiation.

Method used

A multi-channel cell-laden nerve repair catheter with a dual patterned structure was used to prepare conductive fibers through a chitosan/sodium alginate mixed spinning solution. Combined with UV curing polymers and electrical stimulation technology, the mold was designed to promote the directional migration of neural stem cells. and differentiation to form conduits with multiple channels and surface patterning.

Benefits of technology

It achieves effective cell adhesion, directional migration and neurogenic differentiation, provides an efficient nerve injury repair strategy, replaces autologous nerve transplantation, and solves the functional and structural deficiencies of traditional catheters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118750644A_ABST
    Figure CN118750644A_ABST
Patent Text Reader

Abstract

The invention discloses a multi-channel cell-carrying nerve repairing conduit with a double patterning structure and a preparation method thereof. The preparation method comprises the following steps: (1) preparing conductive fibers by adopting a wet spinning method and an in-situ surface polymerization method to form conductive fiber bundles; (2) designing a pouring mold; (3) coating the interior of a mold with a release agent, fixing the prepared fiber bundles in the mold, adding a UV-curable polymer solution to the mold, and curing into gel; (4) after the gel is aged, demolding; after removing the surface release agent, introducing a protein / polypeptide material capable of promoting cell adhesion to the surface of the nerve conduit by using an impregnation method, drying and sterilizing to obtain the multi-channel nerve repair conduit material with the double patterned structure. In combination with a co-culture technology of neural stem cells, after cells are adhered and directionally migrated in a tube, neural differentiation is realized in combination with a pulse direct current stimulation technology, and the material can be used for replacing an autologous nerve transplantation material. The catheter material can be used in the fields of nerve and spinal cord repair and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of nerve repair materials, and in particular to a multi-channel cell-carrying nerve repair conduit with a double patterning structure and a preparation method thereof. Background Art

[0002] Peripheral nerve injury (PNI) is a common clinical disease caused by traffic accidents, iatrogenic injuries, falls, etc. According to statistics, more than 5 million patients will suffer from peripheral nerve injury every year worldwide. At present, for defects smaller than a few millimeters, direct suture is generally used surgically, while for defects with large gaps, autologous transplantation has become the gold standard for clinical treatment. However, problems such as the source of donors and the risk of morbidity at the donor site have limited the further development of autologous transplantation.

[0003] In recent years, with the rapid development of tissue engineering, artificial nerve guide conduits (NGCs) have been developed to replace autologous nerve transplantation. The development of NGCs mainly focuses on three aspects: raw materials, structure and function. In terms of raw materials: the first generation of NGCs is made of non-degradable inert biomaterials such as silicone, but the defect of requiring secondary surgery to remove it has led to its gradual replacement by bioresorbable materials such as polylactide and type I collagen; in terms of structure: early NGCs were mainly single-channel structures, but comparative studies have found that multi-channel structures can promote nerve reinnervation; in terms of function: traditional nerve guides do not have various active functions, and are only used as a filling medium to connect damaged nerves. There are gaps in functions such as promoting cell adhesion, cell proliferation, and cell differentiation into neurons, and they have gradually developed this year. Although nerve repair catheter materials have been developing at a high speed, nerve repair is an extremely complex process, and the call for comprehensive and all-round development of nerve guides is also growing.

[0004] Based on the above problems, the present invention introduces a double patterned structure and combines technologies or structures such as fiber reinforcement, cell loading, cell adhesion promotion, and electrical stimulation to provide a highly integrated and efficient nerve repair strategy through the synergy of technology, structure, and function, targeting the actual physiological repair process of nerves. Summary of the invention

[0005] The purpose of the present invention is to provide a multi-channel cell-loaded nerve repair catheter with a double patterned structure and a preparation method thereof in view of the deficiencies of the prior art and by combining the advantages of various materials and processes.

[0006] The present invention is implemented by the following technical solutions:

[0007] A method for preparing a multi-channel cell-loaded nerve repair conduit with a double patterned structure comprises the following steps:

[0008] 1) preparing a chitosan / sodium alginate mixed spinning solution, preparing fiber filaments by a continuous multi-step wet spinning method, immersing the fiber filaments in an aniline / phytic acid solution for in-situ surface polymerization to prepare conductive fibers, and forming conductive fiber bundles by a twisting process;

[0009] 2) Designing a casting mold that can give the nerve repair conduit a double patterning and multi-channel structure that can promote the directional migration of neural stem cells; the mold can make the nerve repair conduit have multiple channels, and the surface of the nerve repair conduit and the surface of each channel are patterned;

[0010] 3) coating a release agent inside the mold, arranging the fiber bundles prepared in step 1) longitudinally and fixing them in the mold, adding a UV-curable polymer solution from an injection port on the mold, curing the solution to form a gel having a double network structure, and then curing the solution using UV;

[0011] 4) After the gel is solidified, a freeze-thaw cycle process is used to achieve demolding; after the surface release agent is removed by a rapid flushing-dialysis process, a protein / peptide material that can promote cell adhesion is introduced onto the surface of the nerve conduit by an immersion method, and a gel conduit is obtained by low-temperature airflow drying and irradiation sterilization, that is, a multi-channel nerve repair conduit material with a double patterned structure is obtained;

[0012] 5) Combined with the co-culture experiment of neural stem cells, after the cells adhere and migrate in a directional manner in the tube, pulsed direct current stimulation technology is used to achieve neurogenic differentiation, which can be used to replace autologous neural transplant materials.

[0013] Furthermore, in step 1), chitosan is dissolved in an acetic acid aqueous solution containing urea, glycerol and sodium ethoxide to obtain a chitosan solution, and then sodium alginate powder is slowly added and stirred to completely dissolve to obtain the desired chitosan / sodium alginate mixed spinning solution, wherein the concentration of chitosan is 2-5wt%, the molecular weight of chitosan is 1200000-2000000, the degree of deacetylation is 70-80%, and the concentration of the acetic acid aqueous solution is 2-4wt%; the viscosity of sodium alginate (10g / L, 20°C) is 0.02-0.1Pa·s, and the concentration is 0.1-0.5wt%; the amount of urea added is 2-3wt%, the amount of glycerol added is 2-5wt%, and the amount of sodium ethoxide added is 0.5-1wt%; the stirring rate during the preparation of the above spinning solution is 400-600rpm / min, and the stirring time is 2-4 hours.

[0014] Furthermore, in step 1), the spinneret parameters during the wet spinning process are: spinning flow rate 40-80mL / h, spinning temperature 30-45°C. The fiber-forming stage mainly passes through 7 solutions: including a single coagulation bath, a single cleaning solution, a double cleaning solution, a double coagulation bath, a triple cleaning solution, and a quadruple cleaning solution. The single coagulation bath is 3-5wt% NaOH or KOH, 0.2-0.5wt% Na2SO4 dissolved in ethanol / water solution (1:1v:v); the double coagulation bath is 5-10wt% calcium chloride aqueous solution; the cleaning solutions are all deionized water; the coagulation bath temperature is 20-50°C, and the cleaning solution temperature is 40-50°C.

[0015] Furthermore, in step 1), the conductive fiber preparation process is: immersing the prepared fiber filaments in an aniline / phytic acid solution, wherein the solution contains 0.01-0.03 g / ml of aniline, 0.06-0.12 g / ml of phytic acid, and 0.002-0.01 g / ml of initiator; wherein the initiator is one of potassium persulfate, sodium persulfate, and ammonium persulfate, and then in situ self-polymerizing for 2-4 hours under room temperature shaking conditions;

[0016] Furthermore, in step 2), the mold is a hollow columnar structure, composed of two halves, and has a removable bottom cover and upper cover, and the inner wall of the hollow column is provided with a plurality of axially parallel micron-level grooves; a plurality of columns are arranged on the bottom cover of the mold, and the outer surface of each column is also provided with a plurality of axially parallel micron-level grooves; the upper cover and the bottom cover are provided with corresponding small holes for the conductive fiber bundle to pass through, and the upper cover is provided with a liquid injection port. Preferably, the mold is made of a transparent material.

[0017] Furthermore, the mold is preferably made of PMMA material, cylindrical in shape, with a longitudinal groove structure on the inner surface, a groove width of 100-200 μm, a height of 80-150 μm, and a spacing of 100-200 μm between the grooves; the mold is arranged with fine cylindrical structures with a diameter of 400-500 μm, and the columns are evenly arranged with a spacing of 800-1000 μm, and the surface also has the same longitudinal groove structure as the inner surface of the mold; a liquid injection port is provided on the edge of the mold cover; at the same time, the mold cover has small holes with a diameter of 200-600 μm and a spacing of 800-1000 μm, and the mold bottom cover is provided with small holes of the same number and corresponding positions as the upper cover, and the conductive fiber bundle passes through the holes on the mold upper cover and the bottom cover, and the ends are exposed for fixed arrangement and subsequent application; a sealing gasket can be provided under the mold bottom cover to prevent leakage during solution casting;

[0018] Further, in step 3), the release agent may be one of glycerol and ethylene glycol; the polymer in the UV-curable polymer solution may be two of GelMA, Alg-MA, and Sil-MA, with a total concentration of 10-20wt% and a dosage ratio of 1:3-3:1; the photoinitiator may be one or more of LAP, I2959, and Irgacure, and the concentration of the photoinitiator may be 0.25-2.5wt%; the UV curing wavelength may be 405nm, the power may be 5-20W, and the curing time may be 3-5min;

[0019] Furthermore, in step 4), the freeze-thaw cycle process is: place the mold in a -80°C refrigerator, freeze for 5-10 minutes, then take it out and thaw naturally for 10-15 minutes; repeat the above freeze-thaw steps 3-5 times. Use a PBS solution precooled to 4°C as the rinse and dialyzate. After rinsing the gel 3-5 times, place it in a PBS solution, change the solution every 30-60 minutes, and repeat 5-8 times; the adhesion protein can be one or more of Fibronectin, Laminin, ColⅢ, etc., with a concentration of 0.1-0.5wt%, and the immersion time is 1-2h. After the immersion is completed, rinse with PBS;

[0020] Further, in step 5), the neural stem cells of P2-P4 and the gel conduit are placed in a low-adhesion plate and co-cultured for 2-3 days, and the cell density in the culture medium is 1-2*10 5 / ml, and then connected to the two ends of the conductive fiber bundle of the gel catheter with a wire, and pulsed direct current stimulation was applied to it, with a voltage of 1-3V, a positive and negative pulse direction, a pulse width of 100-300ms, and a pulse frequency of 3-10Hz; the stimulation lasted for 30-60min / day, and a total of 7-14 days.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] 1) The present invention uses UV-curable polymers, conductive polymers, adhesion-promoting proteins / peptides, etc. as raw materials, and a two-stage patterned mold as a tool. It combines casting method, template method, in-situ UV curing process, dipping method, cell loading, electrical stimulation and other combined processes to prepare a multi-channel cell-loaded nerve repair catheter material with a double patterned structure. This raw material selection and process combination to prepare the nerve repair catheter material is the first of its kind in the present invention.

[0023] 2) The present invention innovatively designs and prepares a two-stage patterned transparent casting mold for the preparation of the nerve repair catheter. First, the inner wall of the mold is provided with axially parallel grooves at the micron level, which serves as a mold for patterning the outer surface of the nerve catheter (single patterning); secondly, the interior of the mold is provided with columns arranged regularly according to the drawings, and the outer surface of the columns is also provided with axially parallel grooves at the micron level. The columns not only provide the possibility for the preparation of the nerve catheter channel, but also introduce a patterned structure (double patterning) into the nerve catheter channel. At the same time, when the mold is transparent and the side of the cover plate is provided with an injection port, the reason why the injection port is provided on the side of the cover plate is that the polymer solution can flow down along the mold wall when injected into the mold, reducing the generation of bubbles and defects (at the same time, the transparency of the mold can observe whether there are bubbles inside), ensuring the integrity of the material structure, and the transparent mold can ensure the feasibility of in-situ UV curing of the polymer solution in the mold.

[0024] 3) In the present invention, a multi-channel cell-carrying nerve repair catheter material with a double patterned structure is prepared by using the above-mentioned mold. The material has a multiple composite structure: wherein the nerve catheter is provided with a regularly arranged channel structure, which can provide space for the growth of cells in the catheter and also provide the possibility for the exchange of cell substances (oxygen, nutrition, waste, etc.). Moreover, the inner surface of the channel and the outer surface of the catheter are simultaneously provided with a longitudinally parallel micron-level groove structure, which has the function of inducing longitudinal migration of cells and can promote the migration and growth of cells on the inner and outer surfaces of the nerve catheter. At the same time, a conductive fiber bundle structure is provided inside, which can provide an enhancement effect on the matrix material of the nerve catheter on the one hand, and achieve a good physical combination between the fiber bundle and the matrix through the mechanical bite between the rough structure on the surface of the fiber bundle and the polymer matrix, and then achieve the enhancement of the matrix by the pulling effect of the fiber bundle; and the conductive effect of the fiber bundle can be used as a "transmission chain" for the later electrical stimulation effect. After applying electrical stimulation at both ends of the nerve catheter, it can act on the cells through the conductive fiber bundle to achieve the induction of cell neural differentiation. The above-mentioned structural designs are all obtained through organic and synergistic combinations based on the actual needs of nerve repair, realizing the innovative application and functional amplification of traditional structures.

[0025] 4) The multi-channel cell-loaded nerve repair conduit with a double patterned structure prepared in the present invention has the functions of promoting cell adhesion on the surface, inducing cell growth into the nerve conduit channel, promoting cell differentiation into nerves, and being biodegradable. First, the purpose of inducing neural stem cells to adhere to the nerve conduit is achieved by having proteins / peptides on the surface that promote cell adhesion; secondly, the adhered cells can be induced by the patterned structure on the surface or in the pores of the nerve conduit to grow longitudinally; then, the conductive polymer fiber bundle and electrical stimulation are used to induce the differentiation of neural stem cells into nerves; finally, the cell-loaded and fully differentiated nerve conduit material is connected to the broken and damaged nerves, and it is expected that the synergy of the above functions can achieve efficient repair of nerve damage.

[0026] 5) The present invention innovatively completes the in vitro construction of "human nerves" by introducing stem cells into nerve conduits, inducing stem cell migration, and using electrical stimulation to induce stem cell differentiation into neurons in vitro, providing an efficient "substitute" for autologous transplantation for nerve damage repair and addressing actual clinical needs. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 Conductive fiber SEM;

[0028] Figure 2 A 3D schematic diagram of an example structure of a mold for preparing a multi-channel cell-laden nerve repair conduit with a double patterning structure;

[0029] Figure 3 3D schematic diagram of a multi-channel cell-laden nerve repair conduit with a double patterning structure;

[0030] Figure 4 Schematic diagram of the operation of a multi-channel cell-loaded neural repair conduit with a double patterned structure combined with electrical stimulation technology to promote neural differentiation;

[0031] Figure 5 PCR data of multi-channel cell-loaded nerve repair conduits with double patterning structure combined with electrical stimulation to induce neural stem cell differentiation into neurons (day 7, Group C represents Comparative Example 1, Group E represents Example 1). DETAILED DESCRIPTION

[0032] The technical solutions and effects of the present invention are further described below with reference to the accompanying drawings and specific examples.

[0033] The preparation method of the multi-channel cell-carrying nerve repair conduit with a double patterned structure of the present invention is as follows: Figure 4As shown, the designed mold is a hollow columnar structure, which is composed of two halves, and has a detachable bottom cover and upper cover. The inner wall of the hollow column is provided with a number of axially parallel micron-level grooves; a number of columns are arranged on the bottom cover of the mold, and the outer surface of each column is also provided with a number of axially parallel micron-level grooves; the upper cover and the bottom cover are correspondingly provided with small holes for the conductive fiber bundle to pass through, and the upper cover is provided with a liquid injection port. The mold is preferably made of transparent material. Figure 2 This is a schematic diagram of a structural portion of a mold used in an embodiment of the present invention. In other embodiments, other mold structures that meet the above requirements may also be used.

[0034] Comparative Example 1

[0035] 1) Designing a casting mold that can endow a nerve repair conduit with a double patterning and multi-channel structure that can promote the directional migration of neural stem cells, wherein the mold is a hollow cylinder made of PMMA (composed of two halves), the inner surface of which has a longitudinal groove structure, the groove width is 200 μm, the height is 150 μm, and the interval between the grooves is 200 μm; the inside of the mold is arranged with small cylindrical structures, the diameter of which is 500 μm, and the columns are evenly arranged with a spacing of 1000 μm, and the surface also has the same longitudinal groove structure as the inner surface of the mold; the mold has a detachable bottom cover and an upper cover, and the edge of the upper cover is provided with a liquid injection port;

[0036] 2) 0.1 ml of glycerol was coated inside the mold, and a mixed solution of GelMA and Sil-MA (w:w=1:1) containing 0.25% LAP was added from the injection port on the mold to a total concentration of 10 wt %, followed by curing with 405 nm 10 W UV for 5 min to form a gel with a double network structure;

[0037] 3) After the gel is solidified, the mold is placed in a -80°C refrigerator, quick-frozen for 10 minutes, and then taken out and thawed naturally for 10 minutes; the freeze-thaw steps are repeated 3 times, and then demolding is performed; the gel is then rinsed 3 times with a PBS solution precooled to 4°C, and then placed in a PBS solution, the solution is changed every 30 minutes, and repeated 8 times to remove excess release agent; the gel is then immersed in a 0.1wt% Fibronectin solution for 2 hours, a protein material that promotes cell adhesion is introduced on the surface, and a multi-channel nerve repair catheter material with a double patterned structure is obtained after low-temperature airflow drying and irradiation sterilization;

[0038] 4) Use P3 neural stem cells with a cell density of 2*10 5 / ml, and co-cultured with nerve conduit gel in low-adhesion well plates for 3 days. After the cells adhered and migrated in the tube, they differentiated for 14 days.

[0039] The conductivity of the composite nerve conduit hydrogel obtained in this comparative example was 0.09 S / m, and the degradation rate in vitro was 72% after 30 days. After co-culture with neural stem cells for 14 days, Confocal imaging of live and dead cell fluorescence staining showed that the proportion of live cells was 94%, and the cells could partially grow into the nerve conduit; due to the lack of the introduction of conductive fibers and pulsed direct current stimulation, the neural differentiation of neural stem cells was poor (the PCR data are shown in Figure 2). Figure 5 Confocal imaging of NF200 immunofluorescence staining showed a relative fluorescence area of ​​9%.

[0040] Comparative Example 2

[0041] 1) Dissolve 5wt% chitosan with a molecular weight of 1200000 and a deacetylation degree of 80% in a 3% acetic acid solution containing 3wt% urea, 3wt% glycerol and 1wt% sodium ethoxide to obtain a chitosan solution, then slowly add sodium alginate powder and stir to dissolve completely, wherein the viscosity of sodium alginate (10g / L, 20°C) is 0.1Pa·s, and the concentration is 0.5wt%, to obtain the desired chitosan / sodium alginate mixed spinning solution; then use a continuous multi-step wet spinning method and an in-situ surface polymerization method to prepare conductive fibers, wherein the parameters of the continuous multi-step wet spinning method are as follows: spinning flow rate 50mL / h, spinning temperature 40°C. The fiber-forming stage mainly passes through 7 solutions: including a single coagulation bath, a single cleaning solution, a double cleaning solution, a double coagulation bath, a triple cleaning solution, and a quadruple cleaning solution. The first coagulation bath is 5wt% NaOH, 0.5wt% Na2SO4 dissolved in ethanol / water solution (1:1v:v); the second coagulation bath is 5wt% calcium chloride aqueous solution; the cleaning solution is deionized water; the coagulation bath temperature is 40°C, and the cleaning solution temperature is 50°C; the prepared fiber filaments are immersed in aniline / phytic acid solution, aniline 0.02g / ml, phytic acid 0.1g / ml, initiator 0.01g / ml; the initiator is potassium persulfate, and then in situ self-polymerization is carried out under room temperature shaking for 4h; after cleaning and drying, the conductive fiber bundle is formed by twisting process;

[0042] 2) Designing a casting mold that can endow a nerve repair conduit with a double patterning and multi-channel structure that can promote the directional migration of neural stem cells, wherein the mold is a hollow cylinder made of PMMA (composed of two halves), the inner surface of which has a longitudinal groove structure, the groove width is 200 μm, the height is 150 μm, and the interval between the grooves is 200 μm; the mold has a detachable upper cover and a bottom cover, and a liquid injection port is provided at the edge of the upper cover; the corresponding positions of the upper cover and the bottom cover of the mold have small holes with a diameter of 500 μm and a spacing of 1000 μm, and the conductive fiber bundle passes through the small holes on the mold, axially arranged with both ends exposed;

[0043] 3) 0.1 ml of glycerol was coated inside the mold, and a mixed solution of GelMA and Sil-MA (w:w=1:1) containing 0.25% LAP was added from the injection port on the mold to a total concentration of 10 wt %, and then 405 nm 10 W UV was used for curing for 5 min to form a gel with a double network structure;

[0044] 4) After the gel is solidified, the mold is placed in a -80°C refrigerator, quick-frozen for 10 minutes, and then taken out and thawed naturally for 10 minutes; the freeze-thaw steps are repeated 3 times, and then demolding is performed; the gel is then rinsed 3 times with a PBS solution precooled to 4°C, and then placed in a PBS solution, the solution is changed every 30 minutes, and repeated 8 times to remove excess release agent; the gel is then immersed in a 0.1wt% Fibronectin solution for 2 hours, a protein material that promotes cell adhesion is introduced on the surface, and a multi-channel nerve repair catheter material with a double patterned structure is obtained after low-temperature airflow drying and irradiation sterilization;

[0045] 5) Use P3 neural stem cells with a cell density of 2*10 5 / ml, and co-cultured with nerve conduit gel in a low-adhesion well plate for 3 days. After the cells adhered and migrated in the tube, they were combined with pulsed direct current stimulation technology to achieve neural differentiation, with a voltage of 3V, positive and negative pulse directions, a pulse width of 200ms, and a pulse frequency of 10Hz; the stimulation lasted for 60min / day, and the total stimulation lasted for 14 days.

[0046] Compared with comparative example 1, conductive fibers were introduced and the multi-channel structure was cancelled. The conductivity of the hydrogel obtained in this comparative example was 0.72 S / m, the 30-day in vitro degradation rate was 65%, and after co-culture with neural stem cells for 14 days, Confocal imaging of live and dead cell fluorescence staining showed that the proportion of live cells was 92%. Due to the lack of a multi-channel microcatheter structure, the cells were all adhered to the surface, and the neural differentiation of neural stem cells was poor. Confocal imaging of NF200 immunofluorescence staining showed that the relative fluorescence area was 17%.

[0047] Example 1

[0048] 1) Dissolve 5wt% chitosan with a molecular weight of 1200000 and a deacetylation degree of 80% in a 3% acetic acid solution containing 3wt% urea, 3wt% glycerol and 1wt% sodium ethoxide to obtain a chitosan solution, then slowly add sodium alginate powder and stir to dissolve completely, wherein the viscosity of sodium alginate (10g / L, 20°C) is 0.1Pa·s, and the concentration is 0.5wt%, to obtain the desired chitosan / sodium alginate mixed spinning solution; then use a continuous multi-step wet spinning method and an in-situ surface polymerization method to prepare conductive fibers, wherein the parameters of the continuous multi-step wet spinning method are as follows: spinning flow rate 50mL / h, spinning temperature 40°C. The fiber-forming stage mainly passes through 7 solutions: including a single coagulation bath, a single cleaning solution, a double cleaning solution, a double coagulation bath, a triple cleaning solution, and a quadruple cleaning solution. The first coagulation bath is 5wt% NaOH, 0.5wt% Na2SO4 dissolved in ethanol / water solution (1:1v:v); the second coagulation bath is 5wt% calcium chloride aqueous solution; the cleaning solution is deionized water; the coagulation bath temperature is 40℃, and the cleaning solution temperature is 50℃; the prepared fiber filaments are immersed in aniline / phytic acid solution, aniline 0.02g / ml, phytic acid 0.1g / ml, initiator 0.01g / ml; the initiator is potassium persulfate, and then in situ self-polymerization is carried out under room temperature shaking for 4h; the conductive fiber obtained is as follows Figure 1 As shown, after cleaning and drying, a conductive fiber bundle is formed through a twisting process;

[0049] 2) Designing a casting mold that can endow a nerve repair conduit with a double patterning and multi-channel structure that can promote the directional migration of neural stem cells, wherein the mold is a hollow cylinder made of PMMA (composed of two halves), the inner surface of which has a longitudinal groove structure, the groove width is 200 μm, the height is 150 μm, and the spacing between the grooves is 200 μm; the inside of the mold is arranged with fine cylindrical structures, the diameter of which is 500 μm, and the columns are evenly arranged with a spacing of 1000 μm, and the surface also has the same longitudinal groove structure as the inner surface of the mold; the mold has a detachable bottom cover and an upper cover, and an injection port is provided at the edge of the upper cover; the upper cover and the bottom cover of the mold have corresponding small holes, the diameter of which is 500 μm, and the spacing of which is 1000 μm, and the small hole structure on the mold is used to fix the conductive fiber bundle to pass through the small holes and be arranged axially with both ends exposed from the mold;

[0050] 3) 0.1 ml of glycerol was coated inside the mold, and a mixed solution of GelMA and Sil-MA (w:w=1:1) containing 0.25% LAP was added from the injection port on the mold to a total concentration of 10 wt %, and then 405 nm 10 W UV was used for curing for 5 min to form a gel with a double network structure;

[0051] 4) After the gel is solidified, the mold is placed in a -80°C refrigerator, quick-frozen for 10 minutes, and then taken out and thawed naturally for 10 minutes; the freeze-thaw steps are repeated 3 times, and then demolding is performed; the gel is then rinsed 3 times with a PBS solution precooled to 4°C, and then placed in a PBS solution, the solution is changed every 30 minutes, and repeated 8 times to remove excess release agent; the gel is then immersed in a 0.1wt% Fibronectin solution for 2 hours, a protein material that promotes cell adhesion is introduced on the surface, and a multi-channel nerve repair catheter material with a double patterned structure is obtained after low-temperature airflow drying and irradiation sterilization;

[0052] 5) Use P3 neural stem cells with a cell density of 2*10 5 / ml, and co-cultured with nerve conduit gel in a low-adhesion well plate for 3 days. After the cells adhered and migrated in the tube, they were combined with pulsed direct current stimulation technology to achieve neural differentiation, with a voltage of 3V, positive and negative pulse directions, a pulse width of 200ms, and a pulse frequency of 10Hz; the stimulation lasted for 60min / day, and the total stimulation lasted for 14 days.

[0053] The conductivity of the composite nerve conduit hydrogel obtained in this example is 0.78 S / m, and the degradation rate in vitro after 30 days is 68%. After co-culture with neural stem cells for 14 days, Confocal imaging of live and dead cell fluorescence staining shows that the proportion of live cells is 90%, and a large number of cells migrate into the nerve conduit and are arranged in a directional manner. The neural stem cells have good neurogenic differentiation (the PCR data are shown in Figure 2). Figure 5 Confocal imaging of NF200 immunofluorescence staining showed a relative fluorescence area of ​​49%.

[0054] Example 2

[0055] 1) Dissolve 5wt% chitosan with a molecular weight of 1200000 and a deacetylation degree of 80% in a 3% acetic acid solution containing 3wt% urea, 3wt% glycerol and 1wt% sodium ethoxide to obtain a chitosan solution, then slowly add sodium alginate powder and stir to dissolve completely, wherein the viscosity of sodium alginate (10g / L, 20°C) is 0.1Pa·s, and the concentration is 0.5wt%, to obtain the desired chitosan / sodium alginate mixed spinning solution; then use a continuous multi-step wet spinning method and an in-situ surface polymerization method to prepare conductive fibers, wherein the parameters of the continuous multi-step wet spinning method are as follows: spinning flow rate 50mL / h, spinning temperature 40°C. The fiber-forming stage mainly passes through 7 solutions: including a single coagulation bath, a single cleaning solution, a double cleaning solution, a double coagulation bath, a triple cleaning solution, and a quadruple cleaning solution. The first coagulation bath is 5wt% NaOH, 0.5wt% Na2SO4 dissolved in ethanol / water solution (1:1v:v); the second coagulation bath is 5wt% calcium chloride aqueous solution; the cleaning solution is deionized water; the coagulation bath temperature is 40℃, and the cleaning solution temperature is 50℃; the prepared fiber filaments are immersed in aniline / phytic acid solution, aniline 0.03g / ml, phytic acid 0.1g / ml, initiator 0.01g / ml; the initiator is potassium persulfate, and then in situ self-polymerization is carried out under room temperature shaking for 4h; after cleaning and drying, the conductive fiber bundle is formed by twisting process;

[0056] 2) Designing a casting mold that can endow a nerve repair conduit with a double patterning and multi-channel structure that can promote the directional migration of neural stem cells, wherein the mold is a hollow cylinder made of PMMA (composed of two halves), the inner surface of which has a longitudinal groove structure, the groove width is 200 μm, the height is 150 μm, and the spacing between the grooves is 200 μm; the inside of the mold is arranged with small cylindrical structures, the diameter of which is 500 μm, and the columns are evenly arranged with a spacing of 1000 μm, and the surface also has the same longitudinal groove structure as the inner surface of the mold; the mold has a detachable bottom cover and an upper cover, and an injection port is provided at the edge of the upper cover; the upper cover and the bottom cover of the mold have corresponding small holes, the diameter of which is 500 μm, and the spacing of which is 800 μm, and the small hole structure on the mold is used to pass the conductive fiber bundle, which is axially arranged and exposed at both ends;

[0057] 3) 0.1 ml of glycerol was coated inside the mold, and a mixed solution of GelMA and Sil-MA (w:w=1:1) containing 0.25% LAP was added from the injection port on the mold to a total concentration of 10 wt %, and then 405 nm 10 W UV was used for curing for 5 min to form a gel with a double network structure;

[0058] 4) After the gel is solidified, the mold is placed in a -80°C refrigerator, quick-frozen for 10 minutes, and then taken out and thawed naturally for 10 minutes; the freeze-thaw steps are repeated 3 times, and then demolding is performed; the gel is then rinsed 3 times with a PBS solution precooled to 4°C, and then placed in a PBS solution, the solution is changed every 30 minutes, and repeated 8 times to remove excess release agent; the gel is then immersed in a 0.1wt% Fibronectin solution for 2 hours, a protein material that promotes cell adhesion is introduced on the surface, and a multi-channel nerve repair catheter material with a double patterned structure is obtained after low-temperature airflow drying and irradiation sterilization;

[0059] 5) Use P3 neural stem cells with a cell density of 2*10 5 / ml, and co-cultured with nerve conduit gel in a low-adhesion well plate for 3 days. After the cells adhered and migrated in the tube, they were combined with pulsed direct current stimulation technology to achieve neural differentiation, with a voltage of 3V, positive and negative pulse directions, a pulse width of 200ms, and a pulse frequency of 10Hz; the stimulation lasted for 60min / day, and the total stimulation lasted for 14 days.

[0060] Compared with Example 1, the aniline concentration was increased, so that the thickness of the conductive coating increased, and the number of conductive fibers was increased. The conductivity of the composite nerve conduit hydrogel obtained in this example was 0.93S / m, and the in vitro degradation rate was 64% after 30 days of co-culture with neural stem cells. Confocal imaging of live and dead cell fluorescence staining showed that the proportion of live cells was 86%, a large number of cells migrated into the nerve conduit and were arranged in a direction, the neural stem cells were well differentiated into neurons, and Confocal imaging of NF200 immunofluorescence staining showed that the relative fluorescence area was 61%.

[0061] Example 3

[0062] 1) Dissolve 5wt% chitosan with a molecular weight of 1200000 and a deacetylation degree of 80% in a 3% acetic acid solution containing 3wt% urea, 3wt% glycerol and 1wt% sodium ethoxide to obtain a chitosan solution, then slowly add sodium alginate powder and stir to dissolve completely, wherein the viscosity of sodium alginate (10g / L, 20°C) is 0.1Pa·s, and the concentration is 0.5wt%, to obtain the desired chitosan / sodium alginate mixed spinning solution; then use a continuous multi-step wet spinning method and an in-situ surface polymerization method to prepare conductive fibers, wherein the parameters of the continuous multi-step wet spinning method are as follows: spinning flow rate 50mL / h, spinning temperature 40°C. The fiber-forming stage mainly passes through 7 solutions: including a single coagulation bath, a single cleaning solution, a double cleaning solution, a double coagulation bath, a triple cleaning solution, and a quadruple cleaning solution. The first coagulation bath is 5wt% NaOH, 0.5wt% Na2SO4 dissolved in ethanol / water solution (1:1v:v); the second coagulation bath is 5-wt% calcium chloride aqueous solution; the cleaning solution is deionized water; the coagulation bath temperature is 40°C, and the cleaning solution temperature is 50°C; the prepared fiber filaments are immersed in aniline / phytic acid solution, aniline 0.02g / ml, phytic acid 0.1g / ml, initiator 0.01g / ml; the initiator is potassium persulfate, and then in situ self-polymerization is carried out under room temperature shaking for 4h; after cleaning and drying, the conductive fiber bundle is formed by twisting process;

[0063] 2) Designing a casting mold that can endow a nerve repair conduit with a double patterning and multi-channel structure that can promote the directional migration of neural stem cells, wherein the mold is a hollow cylinder made of PMMA (composed of two halves), the inner surface of which has a longitudinal groove structure, the groove width is 100 μm, the height is 100 μm, and the spacing between the grooves is 100 μm; the inside of the mold is arranged with small cylindrical structures, the diameter of which is 500 μm, and the columns are evenly arranged with a spacing of 1000 μm, and the surface also has the same longitudinal groove structure as the inner surface of the mold; the mold has a detachable upper cover and a bottom cover, and a liquid injection port is provided at the edge of the upper cover; the upper cover and the bottom cover of the mold have corresponding small holes, the diameter of which is 500 μm, and the spacing of which is 1000 μm, and the small hole structure on the mold is used to pass the conductive fiber bundle, which is axially arranged and exposed at both ends;

[0064] 3) 0.1 ml of glycerol was coated inside the mold, and a mixed solution of GelMA and Sil-MA (w:w=1:1) containing 0.25% LAP was added from the injection port on the mold to a total concentration of 10 wt %, and then 405 nm 10 W UV was used for curing for 5 min to form a gel with a double network structure;

[0065] 4) After the gel is solidified, the mold is placed in a -80°C refrigerator, quick-frozen for 10 minutes, and then taken out and thawed naturally for 10 minutes; the freeze-thaw steps are repeated 3 times, and then demolding is performed; the gel is then rinsed 3 times with a PBS solution precooled to 4°C, and then placed in a PBS solution, the solution is changed every 30 minutes, and repeated 8 times to remove excess release agent; the gel is then immersed in a 0.1wt% Fibronectin solution for 2 hours, a protein material that promotes cell adhesion is introduced on the surface, and a multi-channel nerve repair catheter material with a double patterned structure is obtained after low-temperature airflow drying and irradiation sterilization;

[0066] 5) Use P3 neural stem cells with a cell density of 2*10 5 / ml, and co-cultured with nerve conduit gel in a low-adhesion well plate for 3 days. After the cells adhered and migrated in the tube, they were combined with pulsed direct current stimulation technology to achieve neural differentiation, with a voltage of 3V, positive and negative pulse directions, a pulse width of 200ms, and a pulse frequency of 10Hz; the stimulation lasted for 60min / day, and the total stimulation lasted for 14 days.

[0067] Compared with Example 1, the surface morphology of the nerve conduit micropattern is changed to make the pattern more dense. The conductivity of the composite nerve conduit hydrogel obtained in this example is 0.76 S / m, and the 30-day in vitro degradation rate is 67%. After co-culture with neural stem cells for 14 days, Confocal imaging of live and dead cell fluorescence staining showed that the proportion of live cells was 92%, and a large number of cells migrated into the nerve conduit and arranged in a direction, and the cell arrangement was more orderly than that in Example 1, and the neural stem cells were well differentiated into neurons. Confocal imaging of NF200 immunofluorescence staining showed that the relative fluorescence area was 57%.

[0068] The above description is only part of the preferred embodiments of the present invention, which is only used to help understand the present invention and is not intended to limit the present invention. It should be pointed out that for those skilled in the art, several changes and improvements can be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

Claims

1. A method for preparing a multi-channel cell-carrying nerve repair catheter with a double patterned structure, characterized in that: The steps include: 1) preparing a chitosan / sodium alginate mixed spinning solution, preparing fiber filaments by a continuous multi-step wet spinning method, then immersing the mixed solution in an aniline / phytic acid solution for in-situ surface polymerization to prepare conductive fibers, and forming conductive fiber bundles by a twisting process; 2) Designing a casting mold, which needs to be able to give the nerve repair conduit a double patterning and multi-channel structure, that is, it can make the nerve repair conduit have multiple channels, and the surface of the nerve repair conduit and the surface of each channel are patterned; 3) coating a release agent inside the mold, arranging the conductive fiber bundles prepared in step 1) longitudinally and fixing them in the mold, adding a UV-curable polymer solution from an injection port on the mold, curing to form a gel having a double network structure, and then curing with UV; 4) After the gel is solidified, a freeze-thaw cycle process is used to achieve demolding; after the surface release agent is removed by a rapid washing-dialysis process, a protein / peptide material that can promote cell adhesion is introduced onto the sample surface by an immersion method, and a gel catheter is obtained by low-temperature airflow drying and irradiation sterilization, that is, a multi-channel nerve repair catheter material with a double-patterned structure is obtained; 5) Combined with the co-culture experiment of neural stem cells, after the cells adhered and migrated in a directional manner in the tube, pulsed direct current stimulation technology was used to achieve neurogenic differentiation, and a multi-channel cell-loaded neural repair conduit with a double-patterned structure was obtained.

2. The preparation method according to claim 1, characterized in that: In step 1), chitosan is dissolved in an acetic acid aqueous solution containing urea, glycerol and sodium ethoxide to obtain a chitosan solution, and then sodium alginate powder is slowly added and stirred to completely dissolve to obtain the chitosan / sodium alginate mixed spinning solution, wherein the concentration of chitosan is 2-5wt%, the molecular weight of chitosan is 1200000-2000000, the degree of deacetylation is 70-80%, and the concentration of the acetic acid aqueous solution is 2-4wt%; the viscosity of sodium alginate (10g / L, 20°C) is 0.02-0.1Pa·s, and the concentration is 0.1-0.5wt%; the amount of urea added is 2-3wt%, the amount of glycerol added is 2-5wt%, and the amount of sodium ethoxide added is 0.5-1wt%; the stirring rate during the preparation of the above spinning solution is 400-600rpm / min, and the stirring time is 2-4 hours.

3. The preparation method according to claim 1, characterized in that: In step 1), the spinneret parameters during the wet spinning process are: spinning flow rate 40-80mL / h, spinning temperature 30-45°C; the fiber forming stage mainly passes through 7 solutions: including a heavy coagulation bath, a heavy cleaning solution, a double cleaning solution, a double coagulation bath, a triple cleaning solution, and a quadruple cleaning solution. The heavy coagulation bath is 3-5wt% NaOH or KOH, 0.2-0.5wt% Na2SO4 dissolved in ethanol / water solution (1:1v:v); the double coagulation bath is 5-10wt% calcium chloride aqueous solution; the cleaning solutions are all deionized water; the coagulation bath temperature is 20-50°C, and the cleaning solution temperature is 40-50°C.

4. The preparation method according to claim 1, characterized in that: In step 1), the conductive fiber preparation process is: immersing the fiber filaments in an aniline / phytic acid solution, the solution containing 0.01-0.03 g / ml aniline, 0.06-0.12 g / ml phytic acid, and 0.002-0.01 g / ml initiator; wherein the initiator is one of potassium persulfate, sodium persulfate, and ammonium persulfate, and then self-polymerizing in situ under room temperature shaking conditions for 2-4 hours.

5. The preparation method according to claim 1, characterized in that: The mold is a hollow cylindrical structure, composed of two halves, and has a removable bottom cover and upper cover. The inner wall of the hollow column is provided with a plurality of axially parallel grooves of the micron level; a plurality of axially parallel columns are arranged on the bottom cover of the mold, and a plurality of axially parallel grooves of the micron level are also arranged on the outer surface of each column; small holes are correspondingly distributed on the upper cover and the bottom surface for the conductive fiber bundle to pass through, and a liquid injection port is opened on the upper cover.

6. The preparation method according to claim 5, characterized in that: The mold is made of PMMA and is cylindrical in shape. The groove width is 100-200 μm, the height is 80-150 μm, and the spacing between the grooves is 100-200 μm. The diameter of the columns is 400-500 μm, and the columns are evenly arranged with a spacing of 800-1000 μm.

7. The preparation method according to claim 1, characterized in that: In step 3), the release agent is one of glycerol and ethylene glycol; the polymer in the UV-curable polymer solution is two of GelMA, Alg-MA, and Sil-MA, with a total concentration of 10-20wt%, and the mass ratio of the two polymers is 1:3-3:1; the photoinitiator in the solution is one or more of LAP, I2959, and Irgacure, and the concentration of the photoinitiator is 0.25-2.5wt%; The UV curing wavelength is 405nm, the power is 5-20W, and the curing time is 3-5min.

8. The preparation method according to claim 1, characterized in that: In step 4), the freeze-thaw cycle process is as follows: the mold is placed in a -80°C refrigerator, quick-frozen for 5-10 minutes, and then taken out and thawed naturally for 10-15 minutes; The above freeze-thaw steps are repeated 3-5 times; the flushing and dialysis fluid uses a PBS solution precooled to 4°C, the gel is rinsed 3-5 times, and then placed in a PBS solution, the solution is changed every 30-60 minutes, and repeated 5-8 times; the adhesion protein is one or more of Fibronectin, Laminin, and ColⅢ, the concentration is 0.1-0.5wt%, the immersion time is 1-2h, and it is rinsed with PBS after the immersion is completed.

9. The preparation method according to claim 1, characterized in that: In step 5), the neural stem cells of P2-P4 and the gel conduit are placed in a low-adhesion plate and co-cultured for 2-3 days. The cell density in the culture medium is 1-2*10 5 / ml, and then connected to the two ends of the conductive fiber bundle of the gel catheter with a wire, and pulsed direct current stimulation was applied to it, with a voltage of 1-3V, a positive and negative pulse direction, a pulse width of 100-300ms, and a pulse frequency of 3-10Hz; the stimulation lasted for 30-60min / day, and a total of 7-14 days.

10. A multi-channel cell-loaded nerve repair catheter with a double patterned structure, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Composite conductive hydrogel material with simulated neural network structure and preparation method of composite conductive hydrogel material

    CN116173306A

  • Preparation method of bionic multichannel nerve conduit and bionic multichannel nerve conduit

    CN116808294A

  • Golf putter with adjustable lie angle, loft angle and weight

    KR102170188B1

  • Nerve conduit, preparation method therefor, and use thereof

    WO2024098490A1