Defense-attack dual-mode intelligent antibacterial coating material inspired by poison frog and preparation method of defense-attack dual-mode intelligent antibacterial coating material
By forming a titanium nanotube structure on the surface of the implant and loading nanosilver and bone-promoting drugs, combined with the surface zwitterionic coating layer, dual defense and attack against bacteria are achieved, solving the problems of implant-related infection and biofilm formation. problem, significantly improving the anti-infective effect and implant prognosis.
Patent Information
- Application Number
- CN202410739597.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
AI Technical Summary
Existing antimicrobial coating technologies are difficult to effectively prevent and treat implant-related infections, especially the formation of bacterial biofilms, and conventional antibiotic use leads to drug resistance and low local drug concentrations.
Design a "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frogs. By forming a titanium nanotube structure on the surface of a titanium/titanium alloy matrix material, loading bone-promoting drugs and nanosilver, combined with surface zwitterionic packages The coating achieves the dual functions of bacterial adhesion and killing.
This material can effectively inhibit bacterial adhesion and biofilm formation, provide long-term sustained-release bone-promoting effects, significantly improve the anti-infection ability of the implant, and reduce the incidence of infection.
Smart Images

Figure CN118750650A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of antibacterial surface technology, and in particular to a "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frogs and a preparation method thereof. Background Art
[0002] With the rapid development of clinical level, the use of clinical implants is increasing. Bone-related implants are the most common clinical implants and are widely used in fracture fixation, defect repair, functional reconstruction and other aspects. Implant-associated infection (IAI) is a major problem faced in clinical practice. Although its incidence is low (0.3-3%), once infection occurs, the use of antibiotics is often ineffective, and a second operation is often required to remove the implant and thoroughly debride it. This process is expensive, the patient is extremely painful, and the prognosis is often poor. The main reason for the poor prognosis is the formation of bacterial biofilm. Bacterial biofilm originates from the adhesion of bacteria on the surface of the implant. After adhesion and colonization, the matrix is secreted to surround itself, forming a large number of bacterial aggregation membrane-like objects with extremely strong drug resistance and invasiveness. Modern internal and external surgical treatments are almost helpless against infections after biofilm formation. The conventional clinical method for preventing and treating implant-associated infection is the preventive use of systemic antibiotics, but due to the low local drug concentration, the effect is poor; local antibiotic flushing will lead to serious drug resistance problems, so it is generally not used. Therefore, it is urgent to design an implant that is highly antibacterial.
[0003] With the development of antibacterial coating technology, various antibacterial coating orthopedic implants have been gradually developed. Common antibacterial implants are simply coated with antibiotics, which have problems such as short action time and initial drug burst release; at the same time, this type of antibacterial implant is helpless against the formation of bacterial biofilms. To prevent and treat bacterial biofilms, we can only start from the root and prevent bacterial adhesion, thereby preventing the formation of biofilms. To this end, the present invention is inspired by the surface protective layer of the poison dart frog and designs a "defense-attack" dual-mode intelligent antibacterial coating material, in which the surface zwitterionic coating layer has a high-efficiency antibacterial adhesion effect. At the same time, for a small amount of invading bacteria, the AgNPs in the TNT tube at the bottom can play the role of "poison glands", releasing silver ions to kill bacteria, so as to solve the problem of biofilm-related infection. At the same time, the slender tubular structure and the osteogenic drugs loaded at the bottom of the tube can play a long-term sustained-release osteogenic effect, improving the patient's prognosis in all directions. Summary of the invention
[0004] The purpose of the present invention is to address the deficiencies in the prior art and provide a "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frogs and a preparation method thereof. The present invention successfully realizes the preparation of a dual-mode intelligent antibacterial coating material by carefully selecting and combining raw materials and production processes, and cleverly designing a multi-layer structure of a composite coating, using a combination of processes such as anodization, ultrasonic loading, in-situ self-polymerization, free radical tools, and surface grafting.
[0005] A "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frogs, wherein a titanium nanotube TNT structure is formed on the surface of a titanium / titanium alloy substrate material, wherein the nanotubes in the TNT structure are loaded with osteopromoting drugs and nanosilver AgNPs in sequence from bottom to top, and the surface of the TNT structure is also covered with a surface zwitterion coating layer; the material has an attack-defense dual mode similar to the surface protective layer of the poison dart frog, wherein the surface zwitterion coating layer is similar to the surface mucus layer of the poison dart frog and can resist bacterial adhesion and play a "defense" role; the AgNPs in the titanium nanotubes are similar to the poison gland structure of the poison dart frog and can kill invading bacteria and play an "attack" role.
[0006] In the above scheme, the surface zwitterionic coating layer is a polydopamine PDA grafted with a GS copolymer, and the GS copolymer is prepared by copolymerization of SBMA and GMA.
[0007] The specific preparation method of the coating material comprises the following steps:
[0008] 1) The surface of the titanium / titanium alloy sample is polished, and after being polished and flattened, ultrasonic cleaning is performed in sequence using acetone, ethanol, and ultrapure water; after cleaning, anodizing is performed on the sample to form a uniform TNT structure on the surface, and then the sample is cleaned with ultrapure water for later use;
[0009] 2) placing the sample treated in step 1) in a bone promoting drug solution, ultrasonically loading, drying, and repeating the ultrasonic loading-drying step 3-5 times; placing it in a AgNO3 solution, ultrasonically loading; then combining the UV reduction method to reduce Ag + Reduction to obtain AgNPs; the cyclic ultrasonic loading-reduction step is repeated 5-10 times, and ultrapure water is used for washing after the loading is completed;
[0010] 3) placing the sample after the reaction in step 2) in a Tris-HCl solution (pH=8.5) containing DA, so that dopamine forms a PDA coating layer on the surface of the material through an in-situ self-polymerization process;
[0011] 4) dissolving the GS copolymer in ultrapure water to obtain a 2-8 wt % aqueous solution; immersing the sample treated in step 3) in the GS copolymer solution, and subjecting the sample to a self-rotation-oscillation reaction at 60-80° C. for 12-24 h, so as to achieve grafting of the GS copolymer on the sample surface through the ring-opening reaction of the epoxy group;
[0012] 5) The sample prepared in step 4) is cleaned, irradiated and sterilized, and packaged to obtain the desired "defense-attack" dual-mode intelligent antibacterial coating sample inspired by the poison dart frog.
[0013] Further, in step 1), the surface of the titanium / titanium alloy sample is polished smooth using 400, 800, and 1200 mesh sandpapers in sequence; the ultrasonic power during ultrasonic cleaning is 80-200 W, and the cleaning time is 10-20 min; anodizing parameters: the electrolyte is ammonium fluoride (1-2 wt%), calcium dihydrogen phosphate (0.5-1 wt%), and Sr(OH)2·8H2O (0.1-0.25 wt%) dissolved in 50 (v / v) % propylene glycol aqueous solution, the voltage is 10-30 V, the inter-electrode distance is 10-20 cm, and the electrolysis time is 2-4 h;
[0014] Further, in step 2), the ultrasonic load power is 80-120W, and the load time for each time is 15-30min; the osteogenic drug can be one or more of etidronate sodium, alendronate sodium, clodronate disodium, etc., with a concentration of 0.1-0.2wt%; the concentration of the AgNO3 solution is 0.05-0.2mol / L; the UV wavelength is 380-420nm, the power is 20-50w, and the reduction time is 30-60min;
[0015] Further, in step 3), the concentration of DA is 2-8 mg / ml, the self-polymerization condition is room temperature, and the time is 6-12 h;
[0016] Further, in step 4), the preparation method of the GS copolymer comprises: dissolving SBMA in ultrapure water under magnetic stirring to obtain an SBMA aqueous solution; taking a certain amount of GMA dissolved in a GMA methanol solution in methanol, mixing the GMA methanol solution with the above SBMA aqueous solution under magnetic stirring for 30-60 minutes to obtain a mixed solution; placing the reaction system in a constant temperature water bath at 40-60° C., stirring for 5-15 minutes to preheat the solution, then adding APS, stirring again for 5-15 minutes and then adding SBS, free radical copolymerizing for 5-10 hours, naturally cooling to room temperature, adding deionized water to remove unreacted monomers, initiators and other impurities to obtain a white crude product, then adding methanol to dissolve the crude product, and the above impurity removal process is repeated 5-10 times to completely remove impurities therein, followed by freeze drying to obtain a GS copolymer;
[0017] Furthermore, the concentration of the SBMA aqueous solution is 2-5wt%, the concentration of the GMA methanol solution is 5-10wt%, the volume ratio of the SBMA aqueous solution to the GMA methanol solution is 10:1-5:1; the amount of APS and SBS is 1-2% of the mass of SBMA;
[0018] Furthermore, the specific parameters of the rotation-oscillation in step 4) are as follows: the rotation rate is 5-10 rpm / min, the oscillation frequency is 30-60 Hz, and the oscillation amplitude is 0.2-0.5 cm.
[0019] Compared with the prior art, the present invention has the following advantages:
[0020] 1. The present invention uses titanium / titanium alloy, osteogenic drugs, silver nitrate, zwitterions, dopamine, etc. as raw materials, and uses a combination of processes such as anodic oxidation, ultrasonic loading, in-situ self-polymerization, free radical copolymerization, and surface grafting to prepare a "defense-attack" dual-mode intelligent antibacterial coating material. This combination of process and material selection is the first of its kind in the present invention;
[0021] 2. The present invention focuses on all-round protection against implant infection. Inspired by the protective layer on the surface of poison dart frogs, a smart material with both anti-adhesion and bactericidal effects is designed: the coating has a bionic structure of the poison gland of poison dart frogs, and the interior is a TNT structure, which acts as the poison gland of poison dart frogs; and AgNPs are used as the "poison" of bacteria, which is stored inside the TNT (poison gland); and the surface is a coating structure of PDA and GS copolymers, which on the one hand coats the "poison gland" and on the other hand is similar to the mucus layer on the surface of the "poison gland", playing an anti-adhesion role. When the coating is working, the zwitterionic coating coated on the surface of the material forms a highly anti-adhesion surface, which plays a "defense" role, greatly inhibits the adhesion of bacteria, and fundamentally limits the possibility of bacterial biofilm formation; the TNT carrying AgNPs under the coating is similar to the poison gland under the mucus layer of poison dart frogs, which plays an "attack" role, and the internal AgNPs can effectively kill free bacteria that cannot form biofilms. Through the synergistic effect between the "defense-attack" dual modes of the above-mentioned coating, efficient prevention and treatment of implant surface infection is achieved; 3. The present invention realizes a new application of the old process, using anodizing to prepare TNT to simulate the "poison gland" structure of the poison dart frog, and cleverly uses a combination of ultrasonic impregnation and in-situ UV reduction to achieve efficient in-situ drug loading in the "poison gland". Through the combination of the above-mentioned processes, the internal structure of the poison gland of the "nuclear bomb" imitating the poison gland of the poison dart frog was successfully prepared. At the same time, a GS copolymer coating layer based on a PDA coating was innovatively designed to prepare the external structure of the poison gland of the poison dart frog. The anti-adhesion function of the zwitterions is similar to that of the poison gland mucus, which has an "anti-fouling" effect. The GS polymer is obtained by free radical copolymerization of GMA and SBMA under the action of an initiator. Its epoxy group undergoes a ring-opening reaction with the amino group (-NH2) on the PDA coating layer to achieve the preparation of the GS copolymer coating layer. No chemical crosslinking agent is used in the reaction process, which can maximize its biocompatibility and retain the activity of the drug loaded in the TNT tube. In addition, considering that it is difficult to evenly cover the coating on the surface of titanium alloy materials in conventional reaction systems, the surface grafting of the GS copolymer is innovatively performed using the self-rotation-oscillation method: the oscillation process can achieve uniform coating of the polymer on the surface, and the self-rotation process can play a "turning over" role, so that each surface of the material can be evenly covered with the polymer coating, thereby increasing the consistency of the finished product.
[0022] 3. Considering that the time span of bone defect repair is relatively long, the present invention sequentially loads osteogenic drugs and AgNPs in TNT to achieve full-cycle osteogenesis: the infection rate is relatively high in the early stage of implantation, and the AgNPs loaded later in the sequential loading process are located at the upper part of the TNT tube and can be released at an early stage, thus playing a good anti-infection role in the early stage; the start of the osteogenesis process is relatively slow, and the osteogenic drug is loaded before the AgNPs, so that it is located at the bottom of the TNT tube, which can form a time difference when the drug is released, which is adapted to physiological osteogenesis;
[0023] 4. The "attack" and "defense" integrated coating designed by the present invention is not only suitable for orthopedic implants, but can also be used for the prevention of various implant-related infections in orthopedics, dentistry, dermatology, etc. by changing the substrate and the loaded drug according to the specific use environment. Its integrated attack and defense function plays a good synergistic role, forming a double insurance against implant-related infections, reducing its incidence to the greatest extent, and has great clinical value. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 SEM image of TNT;
[0025] Figure 2 Surface SEM image of the "defense-attack" dual-mode smart antibacterial coating inspired by poison dart frogs;
[0026] Figure 3 Contact angle results of the poison dart frog-inspired “defense-attack” dual-mode smart antibacterial coating;
[0027] Figure 4 The silver ion release profile of the "defense-attack" dual-mode smart antibacterial coating inspired by the poison dart frog;
[0028] Figure 5 Comparison of biofilm formation on the surface of the poison dart frog-inspired "defense-attack" dual-mode intelligent antibacterial coating (the left picture is the pure TNT control group, and the right picture is the experimental group). DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further described in detail below with reference to the accompanying drawings and specific examples.
[0030] Comparative Example 1
[0031] 1) The surface of the titanium / titanium alloy sample (1*1*0.2cm square piece) was polished with 400, 800, and 1200 mesh sandpaper in sequence, and then ultrasonically cleaned with acetone, ethanol, and ultrapure water for 15 minutes respectively after polishing; after cleaning, it was anodized, and the electrolyte was ammonium fluoride (1.5wt%), calcium dihydrogen phosphate (0.5wt%), Sr(OH)2·8H2O (0.2wt%) dissolved in 50(v / v)% propylene glycol aqueous solution, the voltage was 20V, the inter-electrode distance was 120cm, and the electrolysis time was 2h, so that a uniform TNT structure was formed on the surface, and then it was cleaned with ultrapure water for use;
[0032] 2) placing the sample treated in step 1) in a 0.1wt% sodium alendronate solution, ultrasonically loading it for 30 minutes and drying it, repeating this process 5 times; placing it in a 0.1mol / L AgNO3 solution, ultrasonically loading it for 30 minutes, and then reducing it under a 365nm UV lamp for 30 minutes; repeating the above cyclic ultrasonic loading-reduction steps 5 times, and washing it with ultrapure water after the loading is completed;
[0033] 3) placing the sample after the reaction in step 2) in a Tris-HCl solution (pH=8.5) containing 4 mg / ml DA, and reacting at room temperature for 6 hours, so that dopamine forms a PDA coating layer on the surface of the material through an in-situ self-polymerization process;
[0034] 5) The sample prepared in step 3) is cleaned, irradiated and sterilized, and packaged to obtain an antibacterial coating sample.
[0035] The diameter of the TNT nanotubes on the titanium alloy surface obtained in this embodiment is 80-100nm ( Figure 1 ), the water contact angle was 65°; the sample was placed in 3ml PBS solution, and the silver ion release in 7 days was 6.02±0.65ug / ml; the sample extract was taken for CCK-8 experiment, which showed that the relative activity of the cells was 90% in 7 days, the bacterial adhesion experiment showed that bacterial biofilm was formed, and the inhibition zone experiment showed that the diameter of the inhibition zone was 4.2±0.7cm.
[0036] Example 1
[0037] 1) The surface of the titanium / titanium alloy sample (1*1*0.2cm square piece) was polished with 400, 800, and 1200 mesh sandpaper in sequence, and then ultrasonically cleaned with acetone, ethanol, and ultrapure water for 15 minutes respectively after polishing; after cleaning, it was anodized, and the electrolyte was ammonium fluoride (1.5wt%), calcium dihydrogen phosphate (0.5wt%), Sr(OH)2·8H2O (0.2wt%) dissolved in 50(v / v)% propylene glycol aqueous solution, the voltage was 20V, the inter-electrode distance was 120cm, and the electrolysis time was 2h, so that a uniform TNT structure was formed on the surface, and then it was cleaned with ultrapure water for use;
[0038] 2) placing the sample treated in step 1) in a 0.1wt% sodium alendronate solution, ultrasonically loading it for 30 minutes and drying it, repeating this process 5 times; placing it in a 0.1mol / L AgNO3 solution, ultrasonically loading it for 30 minutes, and then reducing it under a 365nm UV lamp for 30 minutes; repeating the cyclic ultrasonic loading-reduction steps 5 times, and washing it with ultrapure water after the loading is completed;
[0039] 3) placing the sample after the reaction in step 2) in a Tris-HCl solution (pH=8.5) containing 4 mg / ml DA, and reacting at room temperature for 6 hours, so that dopamine forms a PDA coating layer on the surface of the material through an in-situ self-polymerization process;
[0040] 4) Dissolve 2wt% SBMA in ultrapure water under stirring at 400rpm / min; Dissolve 5wt% GMA in methanol, and mix with the above SBMA aqueous solution for 30-60min under stirring at 400rpm / min to obtain a mixed solution; Place the reaction system in a constant temperature water bath at 40-60°C, stir at 400rpm / min for 5min to preheat the solution, then add APS, stir again at 400rpm / min for 5min and then add SBS, the mass of APS and SBS is 1% of SBMA; After 5 hours of free radical copolymerization, naturally cool to room temperature, add deionized water to remove unreacted monomers, initiators and other impurities to obtain a white crude product, then add methanol to dissolve the crude product, repeat the above impurity removal process 5 times, then freeze-dry, and the obtained product is recorded as GS copolymer. The above copolymer is dissolved in ultrapure water to obtain a 5wt% aqueous solution, and the sample treated in step 3) is immersed in the GS copolymer solution, and the reaction is carried out at 60°C for 12h by self-rotation-oscillation;
[0041] 5) The sample prepared in step 4) is cleaned, irradiated and sterilized, and packaged to obtain the desired "defense-attack" dual-mode intelligent antibacterial coating sample inspired by the poison dart frog.
[0042] Compared with the comparative example, the addition of GS copolymer coating layer ( Figure 2 ), the diameter of the TNT nanotubes on the titanium alloy surface obtained in this embodiment is 80-100nm, and the water contact angle is 21°; the sample is placed in 3ml PBS solution, and the silver ion release in 7 days is 5.16±0.37ug / ml ( Figure 4 ); The CCK-8 test of the sample extract showed that the relative activity of the cells was 93% after 7 days, and the bacterial adhesion test showed that compared with the control sample, the bacterial adhesion was significantly reduced, and no biofilm formation was observed ( Figure 5 Right), the inhibition zone experiment showed that the diameter of the inhibition zone was 3.8±0.3cm.
[0043] Example 2
[0044] 1) The surface of the titanium / titanium alloy sample (1*1*0.2cm square piece) was polished with 400, 800, and 1200 mesh sandpaper in sequence, and then ultrasonically cleaned with acetone, ethanol, and ultrapure water for 15 minutes respectively after polishing; after cleaning, it was anodized, and the electrolyte was ammonium fluoride (1.5wt%), calcium dihydrogen phosphate (0.5wt%), Sr(OH)2·8H2O (0.2wt%) dissolved in 50(v / v)% propylene glycol aqueous solution, the voltage was 20V, the inter-electrode distance was 120cm, and the electrolysis time was 2h, so that a uniform TNT structure was formed on the surface, and then it was cleaned with ultrapure water for use;
[0045] 2) placing the sample treated in step 1) in a 0.1wt% sodium alendronate solution, ultrasonically loading it for 30 minutes and drying it, repeating this process 5 times; placing it in a 0.1mol / L AgNO3 solution, ultrasonically loading it for 60 minutes, and then reducing it under a 365nm UV lamp for 30 minutes; repeating the cyclic ultrasonic loading-reduction steps 10 times, and washing it with ultrapure water after the loading is completed;
[0046] 3) placing the sample after the reaction in step 2) in a Tris-HCl solution (pH=8.5) containing 4 mg / ml DA, and reacting at room temperature for 6 hours, so that dopamine forms a PDA coating layer on the surface of the material through an in-situ self-polymerization process;
[0047] 4) Dissolve 2wt% SBMA in ultrapure water under stirring at 400rpm / min; Dissolve 5wt% GMA in methanol, and mix with the above SBMA aqueous solution for 30-60min under stirring at 400rpm / min to obtain a mixed solution; Place the reaction system in a constant temperature water bath at 40-60°C, stir at 400rpm / min for 5min to preheat the solution, then add APS, stir again at 400rpm / min for 5min and then add SBS, the mass of APS and SBS is 1% of SBMA; After 5 hours of free radical copolymerization, cool naturally to room temperature, add deionized water to remove unreacted monomers, initiators and other impurities to obtain a white crude product, then add methanol to dissolve the crude product, repeat the above impurity removal process 5 times, then freeze-dry, and the obtained product is recorded as GS copolymer. The above copolymer is dissolved in ultrapure water to obtain a 5wt% aqueous solution, and the sample treated in step 3) is immersed in the GS copolymer solution, and the reaction is carried out at 60°C for 12h by self-rotation-oscillation;
[0048] 5) The sample prepared in step 4) is cleaned, irradiated and sterilized, and packaged to obtain the desired "defense-attack" dual-mode intelligent antibacterial coating sample inspired by the poison dart frog.
[0049] Compared with Example 1, the number of repetitions of the silver loading operation is increased. The diameter of the TNT nanotubes on the titanium alloy surface obtained in this example is 80-100 nm, and the water contact angle is 23°; the sample is placed in 3 ml PBS solution, and the silver ion release in 7 days is 7.42±0.91 ug / ml; the sample extract is taken for CCK-8 experiment, which shows that the relative activity of the cells in 7 days is 86%, and the bacterial adhesion experiment shows that compared with Example 1, there is no obvious difference in bacterial adhesion, and no biofilm is formed. The inhibition zone experiment shows that the diameter of the inhibition zone is 4.6±0.4 cm.
[0050] Example 3
[0051] 1) The surface of the titanium / titanium alloy sample (1*1*0.2cm square piece) was polished with 400, 800 and 1200 mesh sandpaper in turn, and then ultrasonically cleaned with acetone, ethanol and ultrapure water for 15 minutes respectively after polishing; after cleaning, it was anodized, and the electrolyte was ammonium fluoride (1.5wt%), calcium dihydrogen phosphate (0.5wt%), Sr(OH)2·8H2O (0.2wt%) dissolved in 50(v / v)% propylene glycol aqueous solution, the voltage was 30V, the inter-electrode distance was 120cm, and the electrolysis time was 4h, so that a uniform TNT structure was formed on its surface, and then it was cleaned with ultrapure water for use;
[0052] 2) placing the sample treated in step 1) in a 0.1wt% sodium alendronate solution, ultrasonically loading it for 30 minutes and drying it, repeating this process 5 times; placing it in a 0.1mol / L AgNO3 solution, ultrasonically loading it for 30 minutes, and then reducing it under a 365nm UV lamp for 30 minutes; repeating the cyclic ultrasonic loading-reduction steps 5 times, and washing it with ultrapure water after the loading is completed;
[0053] 3) placing the sample after the reaction in step 2) in a Tris-HCl solution (pH=8.5) containing 4 mg / ml DA, and reacting at room temperature for 6 hours, so that dopamine forms a polydopamine (PDA) coating layer on the surface of the material through an in-situ self-polymerization process;
[0054] 4) Dissolve 2wt% SBMA in ultrapure water under stirring at 400rpm / min; Dissolve 5wt% GMA in methanol, and mix with the above SBMA aqueous solution for 30-60min under stirring at 400rpm / min to obtain a mixed solution; Place the reaction system in a constant temperature water bath at 40-60°C, stir at 400rpm / min for 5min to preheat the solution, then add APS, stir again at 400rpm / min for 5min and then add SBS, the mass of APS and SBS is 1% of SBMA; After 5 hours of free radical copolymerization, cool naturally to room temperature, add deionized water to remove unreacted monomers, initiators and other impurities to obtain a white crude product, then add methanol to dissolve the crude product, repeat the above impurity removal process 5 times, then freeze-dry, and the obtained product is recorded as GS copolymer. The above copolymer is dissolved in ultrapure water to obtain a 5wt% aqueous solution, and the sample treated in step 3) is immersed in the GS copolymer solution, and the reaction is carried out at 60°C for 12h by self-rotation-oscillation;
[0055] 5) The sample prepared in step 4) is cleaned, irradiated and sterilized, and packaged to obtain the desired "defense-attack" dual-mode intelligent antibacterial coating sample inspired by the poison dart frog.
[0056] Compared with Example 1, the voltage and time of anodization were increased. The diameter of TNT nanotubes on the titanium alloy surface obtained in this example was 100-130 nm, and the water contact angle was 21°. The sample was placed in 3 ml PBS solution, and the silver ion release in 7 days was 8.02±1.04 ug / ml. The CCK-8 experiment on the sample extract showed that the cell survival rate was 81% in 7 days. The bacterial adhesion experiment showed that compared with Example 1, almost no bacterial adhesion was observed, and no biofilm was formed. The inhibition zone experiment showed that the diameter of the inhibition zone was 4.9±0.6 cm.
[0057] Example 4
[0058] 1) The surface of the titanium / titanium alloy sample (1*1*0.2cm square piece) was polished with 400, 800, and 1200 mesh sandpaper in sequence, and then ultrasonically cleaned with acetone, ethanol, and ultrapure water for 15 minutes respectively after polishing; after cleaning, it was anodized, and the electrolyte was ammonium fluoride (1.5wt%), calcium dihydrogen phosphate (0.5wt%), Sr(OH)2·8H2O (0.2wt%) dissolved in 50(v / v)% propylene glycol aqueous solution, the voltage was 20V, the inter-electrode distance was 120cm, and the electrolysis time was 2h, so that a uniform TNT structure was formed on the surface, and then it was cleaned with ultrapure water for use;
[0059] 2) placing the sample treated in step 1) in a 0.1wt% sodium alendronate solution, ultrasonically loading it for 30 minutes and drying it, repeating this process 5 times; placing it in a 0.1mol / L AgNO3 solution, ultrasonically loading it for 30 minutes, and then reducing it under a 365nm UV lamp for 30 minutes; repeating the cyclic ultrasonic loading-reduction steps 5 times, and washing it with ultrapure water after the loading is completed;
[0060] 3) placing the sample after the reaction in step 2) in a Tris-HCl solution (pH=8.5) containing 4 mg / ml DA, and reacting at room temperature for 6 hours, so that dopamine forms a polydopamine (PDA) coating layer on the surface of the material through an in-situ self-polymerization process;
[0061] 4) Dissolve 2wt% SBMA in ultrapure water under stirring at 400rpm / min; Dissolve 5wt% GMA in methanol, and mix with the above SBMA aqueous solution for 30-60min under stirring at 400rpm / min to obtain a mixed solution; Place the reaction system in a constant temperature water bath at 40-60°C, stir at 400rpm / min for 5min to preheat the solution, then add APS, stir at 400rpm / min for 5min again and add SBS, the mass of APS and SBS is 1% of SBMA; After 5 hours of free radical copolymerization, cool naturally to room temperature, add deionized water to remove unreacted monomers, initiators and other impurities to obtain a white crude product, then add methanol to dissolve the crude product, repeat the above impurity removal process 5 times, then freeze-dry, and the obtained product is recorded as GS copolymer. The above copolymer is dissolved in ultrapure water to obtain a 10wt% aqueous solution, and the sample treated in step 3) is immersed in the GS copolymer solution, and the reaction is carried out at 60°C for 24h under self-rotation-oscillation conditions;
[0062] 5) The sample prepared in step 4) is cleaned, irradiated and sterilized, and packaged to obtain the desired "defense-attack" dual-mode intelligent antibacterial coating sample inspired by the poison dart frog.
[0063] Compared with Example 1, the concentration of GS copolymer and coating time were increased. The diameter of TNT nanotubes on the titanium alloy surface obtained in this example was 80-100 nm, and the water contact angle was 12° ( Figure 3 ); the sample was placed in 3 ml PBS solution, and the silver ion release in 7 days was 3.77 ± 0.43 ug / ml; the CCK-8 experiment of the sample extract showed that the relative activity of the cells in 7 days was 95%, and the bacterial adhesion experiment showed that compared with Example 1, almost no bacterial adhesion was observed, and no biofilm was formed. The inhibition zone experiment showed that the diameter of the inhibition zone was 3.5 ± 0.2 cm.
[0064] The above description is only part of the preferred embodiments of the present invention, which is only used to help understand the present invention and is not intended to limit the present invention. It should be pointed out that for those skilled in the art, several changes and improvements can be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
Claims
1. A "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frogs, characterized by: The intelligent antibacterial coating material is a titanium nanotube TNT structure formed on the surface of a titanium / titanium alloy substrate material, wherein the nanotubes in the TNT structure are loaded with osteogenic drugs and nanosilver AgNPs in sequence from bottom to top, and the surface of the TNT structure is also covered with a surface zwitterion coating layer; the material has an attack-defense dual mode similar to the surface protective layer of a poison dart frog, wherein the surface zwitterion coating layer is similar to the mucus layer on the surface of the poison dart frog and can resist bacterial adhesion and play a "defense" role; the AgNPs in the titanium nanotubes are similar to the poison gland structure of the poison dart frog and can kill invading bacteria and play an "attack" role.
2. The "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frog according to claim 1, characterized in that: The surface zwitterionic coating layer is polydopamine (PDA) grafted with a GS copolymer, and the GS copolymer is prepared by copolymerization of zwitterionic sulfobetaine methacrylate (SBMA) and glycidyl acrylate (GMA).
3. The method for preparing the "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frogs as claimed in claim 1 or 2, characterized in that: The steps include: 1) The surface of the titanium / titanium alloy sample is polished, and after being polished and flattened, ultrasonic cleaning is performed in sequence using acetone, ethanol, and ultrapure water; after cleaning, anodizing is performed on the sample to form a uniform TNT structure on the surface, and then the sample is cleaned with ultrapure water for later use; 2) placing the sample treated in step 1) in a bone promoting drug solution, ultrasonically loading, drying, and repeating the ultrasonic loading-drying step 3-5 times; placing it in a AgNO3 solution, ultrasonically loading; then combining the UV reduction method to reduce Ag + AgNPs were obtained by reduction, and the cyclic ultrasonic loading-reduction steps were repeated 5-10 times, and ultrapure water was used for washing after the loading; 3) placing the sample after the reaction in step 2) in a Tris-HCl solution containing dopamine (DA), the pH of the solution being 8.5, and in situ self-polymerizing the surface to form a PDA coating layer; 4) dissolving the GS copolymer in ultrapure water to prepare a 2-8 wt % aqueous solution; immersing the sample treated in step 3) in the GS copolymer solution, and subjecting the sample to a self-rotation-oscillation reaction at 60-80° C. for 12-24 h, so as to achieve grafting of the GS copolymer on the sample surface through the ring-opening reaction of the epoxy group; 5) The sample prepared in step 4) is cleaned, irradiated and sterilized, and packaged to obtain the desired "defense-attack" dual-mode intelligent antibacterial coating material inspired by the poison dart frog.
4. The method for preparing the "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frog according to claim 3, characterized in that: In step 1), the surface of the titanium / titanium alloy sample is polished smooth using 400, 800, and 1200 mesh sandpapers in sequence; the ultrasonic power during ultrasonic cleaning is 80-200 W, and the cleaning time is 10-20 min; the anodizing parameters are as follows: the electrolyte is a glycerol aqueous solution containing 1-2 wt% ammonium fluoride, 0.5-1 wt% calcium dihydrogen phosphate, and 0.1-0.25 wt% Sr(OH)2·8H2O, the volume ratio of glycerol to water is 1:1, the voltage is 10-30 V, the inter-electrode distance is 10-20 cm, and the electrolysis time is 2-4 h.
5. The method for preparing the "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frog according to claim 3, characterized in that: In step 2), the ultrasonic load power is 80-120W, and the load time for each time is 15-30min; the osteogenic drug is one or more of etidronate sodium, alendronate sodium, and clodronate disodium, with a concentration of 0.1-0.2wt%; the concentration of the AgNO3 solution is 0.05-0.2mol / L; the UV wavelength is 380-420nm, the power is 20-50w, and the reduction time is 30-60min.
6. The method for preparing the "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frog according to claim 3, characterized in that: In step 3), the concentration of DA is 2-8 mg / ml, the self-polymerization condition is room temperature, and the time is 6-12 h.
7. The method for preparing the "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frog according to claim 3, characterized in that: The preparation method of the GS copolymer in step 4) is as follows: dissolving SBMA in ultrapure water under magnetic stirring to obtain an SBMA aqueous solution; dissolving GMA in methanol, and mixing it with the SBMA aqueous solution under magnetic stirring to obtain a mixed solution; The mixture was placed in a constant temperature water bath at 40-60°C, stirred for 5-15 minutes to preheat the solution, and ammonium persulfate (APS) was added. After stirring for another 5-15 minutes, sodium bisulfite (SBS) was added. After free radical copolymerization for 5-10 hours, the mixture was naturally cooled to room temperature, and deionized water was added to remove impurities to obtain a white crude product. Methanol was then added to dissolve the crude product, and the impurity removal-dissolution process was repeated 5-10 times, followed by freeze-drying to obtain a GS copolymer.
8. The method for preparing the poison dart frog-inspired "defense-attack" dual-mode intelligent antibacterial coating material according to claim 7, characterized in that: The concentration of the SBMA aqueous solution is 2-5wt%, the concentration of the GMA methanol solution is 5-10wt%, the volume ratio of the SBMA aqueous solution to the GMA methanol solution is 10:1-5:1; the mass of APS and SBS is 1-2% of SBMA.
9. The method for preparing the "defense-attack" dual-mode intelligent antibacterial coating material inspired by poison dart frog according to claim 3, characterized in that: The specific parameters of the rotation-oscillation in step 4) are as follows: the rotation rate is 5-10 rpm / min, the oscillation frequency is 30-60 Hz, and the oscillation amplitude is 0.2-0.5 cm.
Citation Information
Cited By
Preparation method of glass fiber reinforced epoxy pipeline with antifouling and antibacterial functions
CN119931123A