Titanium alloy plate and preparation method thereof
By performing cover annealing and continuous annealing on the hot-rolled titanium alloy coil and combining flattening treatment, the problem of poor tissue performance and plate shape quality in the production of traditional titanium alloy sheets is solved, and a more efficient and environmentally friendly production process is achieved.
Patent Information
- Application Number
- CN202411241460.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-05
AI Technical Summary
The traditional titanium alloy sheet production process has problems such as small single batch production volume, many processes, low material yield, long production cycle and poor batch stability, resulting in poor tissue performance and plate flatness.
Titanium alloy hot rolled coil was used to perform hood annealing at a temperature of 700℃~850℃ for 8h~12h, then unrolled and continuously annealed for 5 minutes~15 minutes, and finally titanium alloy plates were prepared by leveling treatment to regulate tissue performance and plate shape.
提高了钛合金板材的组织性能和板形质量,实现了产品尺寸和性能的一致性,增强了批次稳定性,缩短了生产周期,降低了加工成本,且工艺更加环保。
Smart Images

Figure CN118751714B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of titanium alloy material preparation, and in particular to a titanium alloy plate and a preparation method thereof. Background Art
[0002] Titanium alloys have the advantages of high specific strength, corrosion resistance, and heat resistance, so they are widely used in aviation, aerospace, marine, petroleum, chemical, energy, automobile, medical, sports and leisure, etc. Due to the high strength and high elasticity of titanium alloys, it is difficult to optimize and control the roll plate shape.
[0003] The traditional sheet production process has problems such as small single batch production volume, multiple processes, low yield rate, long production cycle, and poor batch stability. The microstructure and flatness of traditional titanium alloy plates are poor, which affects the quality of titanium alloy plates. Compared with the traditional sheet process, the roll process significantly improves the consistency of product size and performance, batch stability, and has obvious advantages in batch capacity, production cycle and processing cost. The production process is more environmentally friendly. Therefore, it is of great significance to provide a method that can effectively improve the microstructure, performance and flatness of titanium alloy plates. Summary of the invention
[0004] Based on this, the present application provides a titanium alloy plate with excellent organizational properties and plate shape quality and a preparation method thereof.
[0005] The technical solution proposed in this application is as follows:
[0006] According to a first aspect of the present application, a method for preparing a titanium alloy plate is provided, comprising the following steps:
[0007] The titanium alloy hot-rolled coil is hood-annealed at 700°C to 850°C for 8 h to 12 h;
[0008] Uncoiling the titanium alloy hot-rolled coil after hood annealing, and continuously annealing at a temperature of 600° C. to 700° C. for 5 min to 15 min to obtain a titanium alloy strip;
[0009] The titanium alloy strip is flattened to prepare the titanium alloy plate.
[0010] The preparation method of the titanium alloy plate of the present application is to adjust the microstructure and properties of the titanium alloy hot-rolled coil under specific hood annealing conditions. Due to long-term heat preservation, the annealing is sufficient, and the grain structure is completely recrystallized and grows, so as to obtain the titanium alloy hot-rolled coil after hood annealing; then the completely recrystallized structure is continuously annealed to adjust the plate shape, and the titanium alloy hot-rolled coil after hood annealing is unrolled and heated and annealed. Through short-term heat preservation, the stress is further removed, and the tension is reasonably controlled to achieve the purpose of adjusting the plate shape, so as to obtain a titanium alloy strip; finally, the titanium alloy strip is flattened to prepare the titanium alloy plate, so as to obtain a titanium alloy plate with both excellent microstructure and properties and plate quality.
[0011] In one embodiment, the flattening process satisfies at least one of the conditions (1) to (4):
[0012] (1) The tension of the leveling treatment is 100kN~150kN;
[0013] (2) The rolling force of the flattening treatment is 6000 kN~12000 kN;
[0014] (3) The bending roller force of the leveling process is 500kN~1000kN;
[0015] (4) The leveling treatment is carried out on a multi-roller leveling machine.
[0016] In one embodiment, the heating temperature during the hood annealing process is 700° C. to 800° C., and the hood annealing treatment time is 8 h to 10 h.
[0017] In one embodiment, the heating temperature during the continuous annealing process is 600° C. to 650° C., and the continuous annealing treatment time is 5 min to 10 min.
[0018] In one embodiment, the continuous annealing treatment is performed by heating in a continuous annealing furnace.
[0019] In one embodiment, after the bell annealing is completed, the titanium alloy hot-rolled coil is furnace-cooled to below 80° C. and then air-cooled after being taken out of the furnace.
[0020] In one embodiment, after the step of continuous annealing, before the step of flattening the titanium alloy strip, the step further includes sequentially performing surface treatment and edge trimming on the titanium alloy strip.
[0021] In one embodiment, the thickness of the titanium alloy hot-rolled coil is 4 mm to 10 mm.
[0022] In one embodiment, the titanium alloy hot-rolled coil includes any one of TA18 titanium alloy hot-rolled coil, TC4 titanium alloy hot-rolled coil, and Gr.38 titanium alloy hot-rolled coil.
[0023] A second aspect of the present application further provides a titanium alloy plate, which is prepared by the above-mentioned method for preparing the titanium alloy plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is the metallographic structure diagram of the TA18 titanium alloy hot-rolled coil after annealing in Example 1 of the present application;
[0025] Figure 2 This is the metallographic structure diagram of the TC4 titanium alloy hot-rolled coil after annealing in Example 2 of this application. DETAILED DESCRIPTION
[0026] The following is a further detailed description of a method for preparing a titanium alloy plate of the present application in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0028] The optional scope of the terms "and / or", "or / and", and "and / or" used in this article includes any one of two or more related listed items, and also includes any and all combinations of the related listed items, said any and all combinations include any combination of any two related listed items, any more related listed items, or all related listed items.
[0029] In the present application, when it comes to numerical intervals (i.e., numerical ranges), unless otherwise specified, the optional numerical distribution is considered continuous within the above numerical interval, and includes the two numerical endpoints (i.e., the minimum and maximum values) of the numerical range, and each numerical value between the two numerical endpoints. Unless otherwise specified, when the numerical interval only refers to the integers within the numerical interval, it includes the two endpoint integers of the numerical range, and each integer between the two endpoints. In this article, it is equivalent to directly listing each integer, such as t is an integer selected from 1-10, indicating that t is any integer selected from the integer group consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9 and 10. In addition, when multiple ranges are provided to describe features or characteristics, these ranges can be combined. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all sub-ranges included therein.
[0030] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0031] An embodiment of the present application provides a method for preparing a titanium alloy plate, and the preparation method includes the following steps S10 to S30.
[0032] Step S10: hood annealing the titanium alloy hot-rolled coil at a temperature of 700° C. to 850° C. for 8 h to 12 h.
[0033] It should be noted that the range of the heating temperature during the hood annealing treatment is "700°C to 850°C", which means that the minimum and maximum values in the range of 700°C to 850°C, as well as every value between the minimum and maximum values, can be taken. Specific examples include, but are not limited to, the point values in the embodiments and the following point values: 700°C, 705°C, 710°C, 715°C, 720°C, 725°C, 730°C, 735°C, 740°C, 745°C, 750°C, 755°C, 760°C, 765°C, 770°C, 775°C, 780°C, 785°C, 790°C, 795°C, 800°C, 805°C, 810°C, 815°C, 820°C, 825°C, 830°C, 835°C, 840°C, 845°C or 850°C; or a range consisting of any two of these values, including, by way of example, 700°C~800°C.
[0034] It is understandable that, depending on the target structure to be obtained in the finished titanium alloy plate, a corresponding specific heating temperature value can be adopted within the above range.
[0035] The range of the time for the hood annealing treatment is "8h~12h", that is, the minimum and maximum values of the range of 8h~12h, and each value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 8h, 8.5h, 9h, 9.5h, 10h, 10.5h, 11h, 11.5h or 12h; or a range consisting of any two of these values, as an example, including: 9h~12h.
[0036] Hood annealing treatment uses a hood furnace for heating (coil annealing). Its principle is to keep the strip at high temperature for a certain period of time through three stages of heating, insulation and cooling, and then slowly cool it to obtain the best organizational structure and performance. The above preparation method regulates the organizational properties of the titanium alloy hot-rolled coil under specific heating temperature and specific insulation treatment conditions. Due to the long insulation time, the annealing is sufficient, the grain structure is completely recrystallized and grown, and a titanium alloy hot-rolled coil with excellent organizational properties is obtained.
[0037] In some embodiments, the heating temperature during the hood annealing process is 700° C. to 800° C., and the hood annealing treatment time is 8 h to 10 h.
[0038] By further controlling the heating temperature during the hood annealing process and the time range of the hood annealing process, the microstructure, properties and plate shape quality of the titanium alloy plate are better.
[0039] In some embodiments, after the bell annealing is completed, the titanium alloy hot-rolled coil is furnace-cooled to below 80° C. and then air-cooled after being taken out of the furnace.
[0040] In some embodiments, the titanium alloy hot-rolled coil is a titanium alloy hot-rolled coil obtained by hot continuous rolling.
[0041] In some of the embodiments, the thickness of the titanium alloy hot-rolled coil is 4 mm to 10 mm. Specifically, the thickness of the titanium alloy hot-rolled coil includes but is not limited to 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, and 10 mm.
[0042] In some embodiments, the titanium alloy hot-rolled coil includes any one of TA18 titanium alloy hot-rolled coil, TC4 titanium alloy hot-rolled coil, and Gr.38 titanium alloy hot-rolled coil.
[0043] Step S20: unrolling the titanium alloy hot-rolled coil after hood annealing, and continuously annealing at a temperature of 600° C. to 700° C. for 5 min to 15 min to obtain a titanium alloy strip.
[0044] It should be noted that the range of the heating temperature during the continuous annealing process is "600°C~700°C", that is, the minimum and maximum values in the range of 600°C~700°C, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 600°C, 605°C, 610°C, 615°C, 620°C, 625°C, 630°C, 635°C, 640°C, 645°C, 650°C, 655°C, 660°C, 665°C, 670°C, 675°C, 680°C, 685°C, 690°C, 695°C or 700°C; or a range consisting of any two of these values, as an example, including: 600°C~650°C.
[0045] It is understandable that, depending on the target structure to be obtained in the finished titanium alloy plate, a corresponding specific heating temperature value can be adopted within the above range.
[0046] The range of the time for continuous annealing treatment is "5min~15min", that is, the minimum and maximum values in the range of 5min~15min, and each value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 5min, 6min, 7min, 8min, 9min, 10min, 11min, 12min, 13min, 14min or 15min; or a range consisting of any two of these values, as an example, including: 5min~10min.
[0047] It can be understood that continuous annealing is relative to hood annealing. Continuous annealing is a production method in which the strip continuously passes through the annealing furnace, the annealing furnace is not sealed, and the strip is directly coiled without stopping. The above-mentioned continuous annealing treatment of the completely recrystallized structure is used to adjust the plate shape. Since the titanium alloy hot-rolled coil after hood annealing is heated and annealed, the stress is further removed through a shorter period of heat preservation, and the tension is reasonably controlled to achieve the purpose of adjusting the plate shape.
[0048] In some embodiments, the continuous annealing process is performed by heating in an annealing furnace.
[0049] In some embodiments, the heating temperature during the continuous annealing process is 600° C. to 650° C., and the time of the continuous annealing process is 5 min to 10 min.
[0050] By further controlling the range of the heating temperature and the time of the continuous annealing treatment during the continuous annealing treatment, the microstructure, performance and plate shape quality of the titanium alloy plate are improved.
[0051] Step S30: flattening the titanium alloy strip to obtain the titanium alloy plate.
[0052] In some embodiments, after the step of continuous annealing, the titanium alloy strip is subjected to surface treatment and edge trimming in sequence before the step of flattening the titanium alloy strip.
[0053] In a specific example, the step S30 includes sequentially performing surface treatment, edge trimming treatment, flattening treatment and slitting treatment on the titanium alloy strip obtained in the step S20 to obtain a titanium alloy plate.
[0054] Traditional leveling processes are mostly used for plate shape control of low-strength cold-rolled thin coils. This application uses a four-roller leveling machine to adjust the plate shape and promotes the application of the leveling process to high-strength titanium alloy hot-rolled coils.
[0055] In some embodiments, the tension of the flattening process is 100 kN to 150 kN.
[0056] The tension of the leveling treatment ranges from "100kN to 150kN", that is, the minimum and maximum values of the range of 100kN to 150kN, and every value between the minimum and maximum values. Specific examples include, but are not limited to, the point values in the embodiments and the following point values: 100 kN, 105 kN, 110 kN, 115 kN, 120 kN, 125 kN, 130 kN, 135 kN, 140 kN, 145 kN, 150 kN; or a range consisting of any two of these values, including, as an example, 120 kN to 150kN.
[0057] It can be understood that adjustments should be made according to the coiling conditions of the titanium alloy strip. If there is obvious deviation, the tension setting can be appropriately increased within the specified range.
[0058] In some of the embodiments, the rolling force of the flattening process is 6000 kN to 12000 kN.
[0059] The rolling force of the flattening process has a value range of "6000kN ~ 12000kN", that is, the minimum value and the maximum value of the range of 6000kN ~ 12000kN, and every value between the minimum value and the maximum value. Specific examples include, but are not limited to, the point values in the embodiments and the following point values: 6000 kN, 6100 kN, 6200 kN, 6300 kN, 6400 kN, 6500 kN, 6600 kN, 6700 kN, 6800 kN, 6900 kN, 7000 kN, 7100 kN, 7200 kN, 7300 kN, 7400 kN, 7500 kN, 7600 kN, 7700 kN, 7800 kN, 7900 kN, 8000 kN, 8100 kN, 8200 kN, 8300 kN, 8400 kN, 8500 kN, 8600 kN, 8700 kN, 8800 kN, 8900 kN, 9000 kN, 9100 kN, 9200 kN kN, 9300 kN, 9400 kN, 9500 kN, 9600 kN, 9700 kN, 9800 kN, 9900 kN, 10000 kN, 10100 kN, 10200 kN, 10300 kN, 10400 kN, 10500 kN, 10600 kN, 10700 kN, 10800 kN, 10900 kN, 11000 kN, 11100 kN, 11200 kN, 11300 kN, 11400 kN, 11500 kN, 11600 kN, 11700 kN, 11800 kN, 11900 kN, 12000 kN, or a range consisting of any two of these values, including, by way of example, 6000 kN ~10000kN.
[0060] It can be understood that the adjustment is made according to the wave shape of the titanium alloy strip. If there is still a certain edge wave shape under the initial setting conditions, the rolling force setting can be appropriately increased within the specified range.
[0061] In some of the embodiments, the bending roller force of the above-mentioned leveling process is 500kN~1000kN.
[0062] The value range of the bending roll force for the leveling treatment is "500kN ~ 1000kN", that is, the minimum and maximum values in the range of 500kN ~ 1000kN, and every value between the minimum and maximum values. Specific examples include, but are not limited to, the point values in the embodiments and the following point values: 500 kN, 510 kN, 520 kN, 530 kN, 540 kN, 550 kN, 560 kN, 570 kN, 580 kN, 590 kN, 600 kN, 610 kN, 620 kN, 630 kN, 640 kN, 650 kN, 660 kN, 670 kN, 680 kN, 690 kN, 700 kN, 710 kN, 720 kN, 730 kN, 740 kN, 750 kN, 760 kN, 770 kN, 780 kN, 790 kN, 800 kN, 810 kN, 820 kN, 830 kN, 840 kN, 850 kN, 860 kN, 870 kN, 880 kN, kN, 890 kN, 900 kN, 910 kN, 920 kN, 930 kN, 940 kN, 950 kN, 960 kN, 970 kN, 980 kN, 990 kN, 1000 kN; or a range consisting of any two of these values, including, by way of example, 500 kN to 900 kN.
[0063] In some of these embodiments, the leveling process is performed on a multi-roll leveling machine.
[0064] It can be understood that adjustments are made according to the export shape of the titanium alloy strip. If there is still a certain warping under the initial setting conditions, the bending roller force setting can be appropriately increased within the specified range; if the strip shape index after the first leveling still does not meet the requirements, a second leveling can be considered based on the actual shape of the strip after the first leveling.
[0065] The above-mentioned preparation method of titanium alloy plate achieves the requirements of finished plate by reasonably matching the tension, rolling force and bending roll force during the flattening process, and has both excellent organizational properties and plate quality.
[0066] The preparation method of the titanium alloy plate of the present application is to adjust the microstructure and properties of the titanium alloy hot-rolled coil under specific hood annealing conditions. Due to long-term heat preservation, the annealing is sufficient, and the grain structure is completely recrystallized and grows, so as to obtain the titanium alloy hot-rolled coil after hood annealing; then the completely recrystallized structure is continuously annealed to adjust the plate shape, and the titanium alloy hot-rolled coil after hood annealing is unrolled and heated and annealed. Through short-term heat preservation, the stress is further removed, and the tension is reasonably controlled to achieve the purpose of adjusting the plate shape, so as to obtain a titanium alloy strip; finally, the titanium alloy strip is flattened to prepare the titanium alloy plate, so as to obtain a titanium alloy plate with both excellent microstructure and properties and plate quality.
[0067] An embodiment of the present application further provides a titanium alloy plate, which is prepared by the above-mentioned method for preparing the titanium alloy plate.
[0068] The titanium alloy plate has both excellent organizational properties and plate quality.
[0069] In order to make the purpose, technical solutions and advantages of the present application more concise and clear, the present application is described with the following specific embodiments, but the present application is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present application and can be used to describe the present application, and cannot be understood as limiting the scope of the present application. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
[0070] The present application will be further described below in conjunction with specific embodiments and comparative examples, but they should not be construed as limiting the scope of protection of the present application.
[0071] Example 1
[0072] (1) Hood annealing treatment: The TA18 titanium alloy hot-rolled coil (thickness 7 mm, width 1050 mm) is heated for the first time (coil annealing) in a hood furnace. The vacuum degree in the furnace is controlled within 60 Pa by filling with high-purity argon gas. The coil is heated to the process temperature of 700 °C with the furnace. After the heat preservation time of 8 h, it is cooled to less than 80 °C with the furnace and then air-cooled.
[0073] (2) Continuous annealing treatment: The titanium alloy hot-rolled coil after hood annealing is heated for the second time (continuous annealing) in a continuous annealing furnace at a heating temperature of 600°C for a holding time of 5 min. After being taken out of the furnace, it is cooled by wind or air and the coiling temperature is 80°C to obtain a first titanium alloy strip.
[0074] (3) Surface treatment: The first titanium alloy strip is subjected to surface treatment to remove the oxide layer and the air absorption layer on the surface of the strip coil, thereby obtaining a second titanium alloy strip.
[0075] (4) Edge trimming: A titanium alloy strip edge preheating device is then used to preheat the edge of the strip, and then the two edges are trimmed to a fixed width of 1000 mm to obtain a third titanium alloy strip.
[0076] (5) Leveling treatment: The third titanium alloy strip obtained in the above step (4) is subjected to a four-roller leveling mill to adjust the shape of the strip. The front and rear tensions are controlled at 100 kN, the rolling force is controlled at 6000 kN, the bending roll force is controlled at 500 kN, and the unevenness is controlled within 10 mm / m. If the strip shape index after the first leveling still does not meet the requirements, a second leveling may be considered based on the actual shape of the strip after the first leveling to obtain a fourth titanium alloy strip.
[0077] (6) The flattened coil is cut into continuous lengths according to the finished product size requirements, with the length controlled at 6000 mm and the length tolerance controlled at (0, +10) mm to prepare titanium alloy plates.
[0078] The metallographic structure of the titanium alloy plate prepared in this embodiment is as follows: Figure 1 As shown. Figure 1 It can be seen that complete recrystallization has occurred, resulting in a relatively uniform grain structure with a grain size of ≤15μm.
[0079] Embodiment 2:
[0080] Example 2 is basically the same as Example 1, except that: in step (1), the heating temperature of the TC4 titanium alloy hot-rolled coil during the hood annealing treatment is different. The specific steps are as follows:
[0081] (1) Hood annealing treatment: The TC4 titanium alloy hot-rolled coil (thickness 7 mm, width 1050 mm) is heated for the first time (coil annealing) in a hood furnace. The vacuum degree in the furnace is controlled within 60 Pa by filling with high-purity argon gas. The coil is heated to the process temperature of 750 ° C with the furnace. After the heat preservation time of 8 hours, it is cooled to less than 80 ° C with the furnace and then air-cooled.
[0082] (2) Continuous annealing treatment: The titanium alloy hot-rolled coil after hood annealing is heated for the second time (continuous annealing) in a continuous annealing furnace at a heating temperature of 600°C for a holding time of 5 min. After being taken out of the furnace, it is cooled by wind or air and the coiling temperature is 80°C to obtain a first titanium alloy strip.
[0083] (3) Surface treatment: The first titanium alloy strip is subjected to surface treatment to remove the oxide layer and the air absorption layer on the surface of the strip coil, thereby obtaining a second titanium alloy strip.
[0084] (4) Edge trimming: A titanium alloy strip edge preheating device is then used to preheat the edge of the strip, and then the two edges are trimmed to a fixed width of 1000 mm to obtain a third titanium alloy strip.
[0085] (5) Leveling treatment: The third titanium alloy strip obtained in the above step (4) is subjected to a four-roller leveling mill to adjust the shape of the strip. The front and rear tensions are controlled at 100 kN, the rolling force is controlled at 6000 kN, the bending roll force is controlled at 500 kN, and the unevenness is controlled within 10 mm / m. If the strip shape index after the first leveling still does not meet the requirements, a second leveling may be considered based on the actual shape of the strip after the first leveling to obtain a fourth titanium alloy strip.
[0086] (6) The flattened coil is cut into continuous lengths according to the finished product size requirements, with the length controlled at 6000 mm and the length tolerance controlled at (0, +10) mm to prepare titanium alloy plates.
[0087] The metallographic structure of the titanium alloy plate prepared in this embodiment is as follows: Figure 2 As shown. Figure 2 It can be seen that complete recrystallization has occurred, resulting in a relatively uniform grain structure with a grain size of ≤10μm.
[0088] Example 3
[0089] Example 3 is basically the same as Example 1, except that: the thickness of the titanium alloy hot-rolled coil in step (1) is different, and the heating temperature during the hood annealing treatment is different. The specific steps are as follows:
[0090] (1) Hood annealing treatment: The TA18 titanium alloy hot-rolled coil (thickness 4 mm, width 1050 mm) is heated for the first time (coil annealing) in a hood furnace. The vacuum degree in the furnace is controlled within 60 Pa by filling with high-purity argon gas. The coil is heated to the process temperature of 850 ° C with the furnace. After the heat preservation time of 8 hours, it is cooled to less than 80 ° C with the furnace and then air-cooled.
[0091] (2) Continuous annealing treatment: The titanium alloy hot-rolled coil after hood annealing is heated for the second time (continuous annealing) in a continuous annealing furnace at a heating temperature of 600°C for a holding time of 5 min. After being taken out of the furnace, it is cooled by wind or air and the coiling temperature is 80°C to obtain a first titanium alloy strip.
[0092] (3) Surface treatment: The first titanium alloy strip is subjected to surface treatment to remove the oxide layer and the air absorption layer on the surface of the strip coil, thereby obtaining a second titanium alloy strip.
[0093] (4) Edge trimming: A titanium alloy strip edge preheating device is then used to preheat the edge of the strip, and then the two edges are trimmed to a fixed width of 1000 mm to obtain a third titanium alloy strip.
[0094] (5) Leveling treatment: The third titanium alloy strip obtained in the above step (4) is subjected to a four-roller leveling mill to adjust the shape of the strip. The front and rear tensions are controlled at 100 kN, the rolling force is controlled at 6000 kN, the bending roll force is controlled at 500 kN, and the unevenness is controlled within 10 mm / m. If the strip shape index after the first leveling still does not meet the requirements, a second leveling may be considered based on the actual shape of the strip after the first leveling to obtain a fourth titanium alloy strip.
[0095] (6) The flattened coil is cut into continuous lengths according to the finished product size requirements, with the length controlled at 6000 mm and the length tolerance controlled at (0, +10) mm to prepare titanium alloy plates.
[0096] Example 4
[0097] Example 4 is basically the same as Example 1, except that the time of the hood annealing treatment during the hood annealing treatment in step (1) is different.
[0098] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0099] Example 5
[0100] Example 5 is basically the same as Example 1, except that the time of the hood annealing treatment during the hood annealing treatment in step (1) is different.
[0101] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0102] Embodiment 6-7
[0103] Examples 6 to 7 are substantially the same as Example 1, except that the heating temperature during the continuous annealing treatment in step (2) is different.
[0104] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0105] Example 8
[0106] Example 8 is basically the same as Example 1, except that the time of continuous annealing treatment in step (2) is different.
[0107] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0108] Embodiment 9-10
[0109] Examples 9 to 10 are substantially the same as Example 1, except that the time of continuous annealing treatment in step (2) is different, and the tension, rolling force and bending roll force of the leveling treatment in step (5) are different.
[0110] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0111] Embodiment 11
[0112] Example 11 is basically the same as Example 1, except that the tension, rolling force and bending roll force in the flattening process in step (6) are different.
[0113] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0114] Comparative Example 1
[0115] (1) Hood annealing treatment: The TA18 titanium alloy hot-rolled coil (thickness 7 mm, width 1050 mm) is heated for the first time (coil annealing) in a hood furnace. By filling with high-purity argon gas, the vacuum degree in the furnace is controlled within 60 Pa. The coil is heated to the process temperature of 700 °C with the furnace. After the heat preservation time of 8 h, it is cooled to within 80 °C with the furnace and air-cooled to obtain the first titanium alloy strip.
[0116] (2) Surface treatment: The first titanium alloy strip is subjected to surface treatment to remove the oxide layer and the air absorption layer on the surface of the strip coil, thereby obtaining a second titanium alloy strip.
[0117] (3) Edge trimming: A titanium alloy strip edge preheating device is then used to preheat the edge of the strip, and then the two edges are trimmed to a fixed width of 1000 mm to obtain a third titanium alloy strip.
[0118] (4) Leveling treatment: The third titanium alloy strip obtained in the above step (3) is subjected to a four-roller leveling mill to adjust the shape of the strip. The front and rear tensions are controlled at 100 kN, the rolling force is controlled at 6000 kN, the bending roll force is controlled at 500 kN, and the unevenness is controlled within 10 mm / m. If the strip shape index after the first leveling still does not meet the requirements, a second leveling may be considered based on the actual shape of the strip after the first leveling to obtain a fourth titanium alloy strip.
[0119] (5) The flattened coil is cut into continuous lengths according to the finished product size requirements, with the length controlled at 6000 mm and the length tolerance controlled at (0, +10) mm to prepare titanium alloy plates.
[0120] Comparative Examples 2~3
[0121] Comparative Examples 2-3 are substantially the same as Example 1, except that the heating temperatures during the hood annealing treatment in step (1) are different.
[0122] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0123] Comparative Examples 4-5
[0124] Comparative Examples 4 to 5 are substantially the same as Example 1, except that the duration of the hood annealing treatment during the hood annealing treatment in step (1) is different.
[0125] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0126] Comparative Examples 6-7
[0127] Comparative Examples 6-7 are substantially the same as Example 1, except that the heating temperatures during the continuous annealing treatment in step (2) are different.
[0128] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0129] Comparative Examples 8-9
[0130] Comparative Examples 8 to 9 are substantially the same as Example 1, except that the time of the continuous annealing treatment in the continuous annealing treatment process in step (2) is different.
[0131] Other conditions and parameters are the same as those in Example 1. Please see Table 1 for specific test results.
[0132] test:
[0133] 1. The titanium alloy plates prepared in the embodiments and comparative examples were subjected to tissue tests, specifically in accordance with the requirements of GB / T 5168-2020;
[0134] 2. The tensile strength and non-proportional elongation strength (R p0.2 ), elongation after fracture (A) test, specifically implement the requirements of GB / T 228.1-2021 standard;
[0135] 3. The titanium alloy plates prepared in the embodiments and comparative examples were tested for plate flatness, specifically complying with the requirements of GB / T3621-2022.
[0136] The preparation process parameters of the titanium alloy plates prepared in the above embodiments and comparative examples, as well as the test results of the microstructure and properties of the titanium alloy plates are shown in Table 1.
[0137] Table 1
[0138]
[0139] It can be seen from Table 1 that the unevenness of the titanium alloy sheet prepared by TA18 titanium alloy hot-rolled coil is ≤10mm / m, the tensile strength is ≥620 MPa, and the non-proportional elongation strength (R p0.2 )≥480 MPa, elongation after fracture (A)≥15.0%; the unevenness of titanium alloy sheets prepared from TC4 titanium alloy hot-rolled coils is ≤10mm / m, the tensile strength is ≥895 MPa, and the non-proportional elongation strength (R p0.2 )≥830MPa, elongation after fracture (A)≥10.0%. In summary, the titanium alloy sheet prepared in the embodiment of the present application has both excellent organizational performance and plate quality compared with the comparative example. Under the condition that the overall plate quality is controlled at 10mm / m, the mechanical properties such as strength and plasticity also meet the requirements of GB / T 3621-2022 standard.
[0140] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0141] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the patent application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent application shall be subject to the attached claims.
Claims
1. A method for preparing a titanium alloy sheet, characterized in that: The following steps are involved: The titanium alloy hot-rolled coil is hood-annealed at 700°C to 850°C for 8 h to 12 h; Uncoiling the titanium alloy hot-rolled coil after hood annealing, and continuously annealing at a temperature of 600° C. to 700° C. for 5 min to 15 min to obtain a titanium alloy strip; The titanium alloy strip is flattened to prepare the titanium alloy plate; The thickness of the titanium alloy hot-rolled coil is 7 mm to 10 mm.
2. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The leveling process satisfies at least one of the following conditions: (1) The tension of the leveling treatment is 100kN~150kN; (2) The rolling force of the flattening treatment is 6000 kN ~ 12000 kN; (3) The bending roller force of the leveling process is 500kN~1000kN; (4) The leveling treatment is carried out on a multi-roller leveling machine.
3. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The heating temperature during the hood annealing process is 700° C. to 800° C., and the hood annealing treatment time is 8 h to 10 h.
4. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The heating temperature during the continuous annealing process is 600° C. to 650° C., and the continuous annealing treatment time is 5 min to 10 min.
5. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The continuous annealing treatment is performed by heating in a continuous annealing furnace.
6. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: After the bell annealing is completed, the titanium alloy hot-rolled coil is furnace-cooled to below 80° C. and then air-cooled out of the furnace.
7. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: After the step of continuous annealing, before the step of flattening the titanium alloy strip, the method further includes sequentially performing surface treatment and edge trimming on the titanium alloy strip.
8. The method for preparing a titanium alloy sheet according to claim 1, characterized in that: The titanium alloy hot-rolled coil includes any one of TA18 titanium alloy hot-rolled coil, TC4 titanium alloy hot-rolled coil and Gr.38 titanium alloy hot-rolled coil.
9. A titanium alloy plate, characterized in that: The titanium alloy sheet is prepared by the method for preparing the titanium alloy sheet as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Method for producing thin TA4 titanium material by roll type cold rolling method
CN106011714A
Preparation method of TA2 cold-rolled titanium strip for low-strength and easily-formed welded pipe
CN108165822A
Micro-medium wave plate shape finishing method for thin-gauge high-strength strip steel
CN115582433A