Heterogeneous ceramic cast-infiltration block as well as preparation method and application thereof
Through the porous grid composite of heterogeneous ceramic cast infiltration blocks, combined with powder metallurgy vacuum sintering and low-temperature paraffin pore-making technology, the problem of difficulty in smelting casting materials to have high wear resistance and high strength at the same time is solved, significantly extending the service life of the workpiece. service life and reduces energy consumption and environmental pollution.
Patent Information
- Application Number
- CN202410944741.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-11
AI Technical Summary
It is difficult for existing smelting and casting materials to achieve high wear resistance and high strength at the same time, resulting in short service life of workpieces with frequent impact and vibration, requiring frequent replacement, affecting production efficiency.
Heterogeneous ceramic cast infiltration blocks are used, with TiC as the hard phase, Mn, Ni, Mo, Cr, C, Fe as the bonding phase, coarse-grained cermets, and Al2O3, ZrO2, MgO, TiO2, and CaO as sintering aids. Fine-grained oxide ceramic powder is mixed, prepared through powder metallurgy vacuum sintering, and combined with low-temperature paraffin wax pore creation to form a porous grid composite.
It improves the toughness, rigidity and wear resistance of the base metal and extends the service life of the workpiece. For example, the service life of the impact crusher plate hammer is increased by 3.7 times, and the life of hitting limestone and cobblestone is extended by 2.6 times and 3.7 times respectively. Reduce energy consumption and environmental pollution.
Smart Images

Figure CN118751901A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cast-infiltration block smelting, and in particular to a heterogeneous ceramic cast-infiltration block and a preparation method and application thereof. Background Art
[0002] Materials obtained by smelting and casting methods usually cannot obtain high wear resistance and high strength at the same time, but in actual engineering applications, structural parts often require both properties. Therefore, technicians in this field often manufacture composite materials through processes such as inlay casting, inlaying, cast infiltration or inlay welding to achieve appropriate effects. For example, Southwest University and Xi'an Jiaotong University cooperated to inlay alumina porous ceramics on the working surface of the heat-resistant steel matrix. When the ceramic particles accounted for 39% of the volume fraction, the abrasive wear of the heat-resistant steel composite material at a high temperature of 900°C was 3.2 times that of pure heat-resistant steel. Central South University, Guangzhou Institute of Nonferrous Metals and Xi'an Jiaotong University cooperated to use self-made ZrO2 toughened alumina ceramic particles with a particle size of 2-3mm to strengthen the phase and prepare particle-reinforced high-chromium cast iron-based composite materials. When the volume fraction of ceramic particles was 47%-55%, the abrasive wear performance was 2.41 times that of high-chromium cast iron.
[0003] In the current application of technology, the resulting materials either have high strength or high hardness. For example, the tensile strength of high manganese steel ZG120Mn13Cr2 is ≥735MPa, and the impact toughness ak value is ≥118 joules. It is most suitable for making workpieces such as hammer heads and flanges of crushers with fast impact speed and high vibration frequency. However, the hardness of the matrix is very low, with a Brinell hardness of less than 300. Although it does not break during the impact hammering process, it has poor wear resistance, and frequent replacement of components has become inevitable. However, people have developed high-chromium cast iron with high hardness, high wear resistance and high corrosion resistance, such as multi-alloy cast iron Cr26 containing high carbon and high chromium. The matrix hardness is as high as HRC65. Although it has good wear resistance, it has poor toughness and an impact toughness ak value of only 3-5 joules. It is most suitable for rolling, sliding, rolling and low-impact workpieces dominated by shear force, such as steel balls in ball mills and grinding rollers in vertical mills. This is because high chromium cast iron is sensitive to shock and vibration, but it is difficult to meet the requirements of workpieces with concentrated loads and repeated impacts. For example, the service life of the plate hammer of the impact crusher is one week to one month, the impact plate is two months, and the side lining is only three months. As a result, these workpieces must be replaced frequently during the production process, which seriously affects production efficiency. Therefore, the present invention proposes a new type of ceramic cast infiltration block material and its preparation method and application to solve the above problems. Summary of the invention
[0004] In order to solve the above problems, the present invention proposes a heterogeneous ceramic cast-infiltration block and a preparation method and application thereof.
[0005] The present invention first provides a non-homogeneous ceramic cast-infiltration block, which includes the following phase components: a coarse-grained metal ceramic with TiC as a hard phase and Mn, Ni, Mo, Cr, C, and Fe as bonding phases, with a content of 20-28wt%; a fine-grained oxide ceramic powder mixed with Al2O3 as a substrate, ZrO2, MgO, TiO2, and CaO as sintering aids, and one of Cu and Mn as an active metal additive, with a content of 80-72wt%.
[0006] Furthermore, the content of hard phase TiC in the coarse-grained cermet is 55-65wt%, and the content of bonding phase is 45-35wt%.
[0007] Furthermore, the Al2O3 content in the fine-grained oxide ceramic powder is 65-75wt%, the sintering aid content is 33.5-23.5wt%, and the active metal additive content is 1-2wt%.
[0008] The present invention provides a method for preparing the above-mentioned heterogeneous ceramic cast-infiltration block, and the preparation method comprises the following steps: Coarse particle preparation: After the coarse particle metal ceramic raw materials are mixed by powder metallurgy method, Sintering in vacuum at 1400-1500℃, cooling the sintered material to room temperature, and then mechanically crushing it to obtain irregular particles; Phase mixing: the prepared coarse-grained metal ceramic, fine-grained oxide ceramic powder and pore-increasing agent paraffin are mixed evenly, and the amount of paraffin added is 12-18% of the total mass; Green body molding: sodium butadiene rubber solution as a molding agent is added to the mixed powder, and then poured into a mold to form a cast infiltration block green body; Drying of green body: After the green body is air-dried for at least 16 hours, it is removed from the mold and placed in a steam drying furnace to recover the paraffin wax at 80-100℃; Green body sintering: The dried and dewaxed green body is placed in a vacuum furnace for vacuum sintering in three stages. The first stage is in the range of 20~950℃. When the vacuum degree rises to about 900℃, the vacuum pump is turned off and argon is introduced; the second stage is in the range of 950~1270℃, liquid phase is formed, and a micro-molten pool appears; the third stage is in the range of 1270~1400℃, the temperature is slowly increased, and after the sintering temperature is over, the vacuum pump is turned on to remove the gas in the furnace, and the cast infiltration block is obtained after accelerated cooling.
[0009] Furthermore, in the phase mixing step, the Al2O3 powder particle size ranges from 20 μm to 150 μm, and the powder particle size of the sintering aid and the active metal additive is 35-75 μm.
[0010] Furthermore, during the green body sintering step, argon is slowly introduced to 3-5 MPa.
[0011] The present invention also provides an application of the above-mentioned heterogeneous ceramic cast infiltration block. The cast infiltration block is inserted into a water glass sand mold, and molten steel is poured into the mold for inlay casting. The inlay casting temperature is controlled at 1370℃±10℃. After the pouring is completed, the casting box is surrounded by dry sand and slowly cooled. After cooling, the box is opened to remove the sand, and the surface of the workpiece is ground, polished and heat treated.
[0012] Furthermore, the components of the molten steel are: C: 3.0-3.35wt%, Si: 0.3-0.9wt%, Mn: 0.7-1.1wt%, Ni: 0.2-0.5wt%, Mo: 0.3-0.4wt%, V: 0.15-0.3wt%, Cu: 0.2-0.5wt%, Cr: 24.0-27.0wt%, and Fe is the balance. The components of the molten steel are smelted in a medium frequency induction furnace, and after deoxidation, slag removal and refining, they are poured out of the furnace.
[0013] Furthermore, the mold is shaped like a crusher hammer.
[0014] The beneficial effects of the present invention are as follows: The present invention is the first to prepare a cast infiltration block by mixing coarse-grained metal ceramics as a skeleton with fine-grained oxide ceramic powders through a vacuum sintering method in powder metallurgy. The particle size and shape of the coarse-grained metal ceramic powders in the cast infiltration block are quite different from those of traditional porous ceramic powders. The porous grid stacked by these particles has high porosity, good permeability after sintering, high strength and certain hardness. It can withstand the scouring of high-density high-temperature molten steel without loosening, collapse or breaking during the cast infiltration process. The qualified rate of the sintered finished product is above 98%, which is difficult to achieve with the existing 1600°C high-temperature sintering technology.
[0015] The cast infiltration block is composed of a variety of particles of different shapes, properties and qualities. It is a porous grid composite that combines reinforcement and multifunctional components. After being cast and infiltrated with the base metal, the base metal has higher strength, toughness, rigidity, corrosion resistance and wear resistance. The wear and abrasion performance of the high chromium alloy base after the cast infiltration block is 4.6 times that of the original one. The service life of the plate hammer of the impact crusher using the cast infiltration block is increased by 3.7 times when hitting limestone, and by 2.6 times when hitting pebbles.
[0016] The cast infiltration block uses low-temperature paraffin as a pore-forming agent during preparation. The paraffin can be recycled in the green body drying step. There is no need for the traditional pore-increasing foaming agent to be heated during mixing (usually up to 500°C), which reduces energy consumption while avoiding environmental pollution caused by the foaming gas. There is also no risk of pore closure and collapse caused by traditional foaming agents after foaming. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The unsintered cast infiltration block green body of the present invention; Figure 2 The cast infiltration block green body after vacuum sintering of the present invention; Figure 3 The distribution spacing of the cast infiltration block particles in the casting of the present invention; Figure 4 The wear morphology of the cast infiltration block of the present invention in the plate hammer. DETAILED DESCRIPTION
[0018] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. The following embodiments are only exemplary to illustrate and explain the present invention, and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0019] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.
[0020] The preparation of the heterogeneous ceramic cast-infiltration block of the present invention is carried out in the following steps.
[0021] Preparation of coarse particles: TiC is used as the hard phase, Mn, Ni, Mo, Cr, C, and Fe are used as the bonding phase. After mixing by powder metallurgy, they are vacuum sintered at a high temperature of 1450±50℃. The sintered material is cooled to room temperature with the furnace, and then mechanically crushed to obtain irregular particles with a particle size of 0.2mm-5.0mm. The particles are coarse particle cermets with a TiC content of 55-65wt% and a density of 6.0g / cm 3 , hardness is HRC70-73, the organizational characteristics are austenitic solid solution and it has temperature memory.
[0022] Phase mixing: 20-28wt% of coarse-grained metal ceramics are mixed with 80-72wt% of fine-grained oxide ceramic powders, and paraffin wax accounting for 12-18% of the total mass is added as a pore-increasing agent in the mixing process and mixed evenly in a V-type mixer. The ball-to-material ratio in the V-type mixer is 1:3, and dry mixing is performed for 40 minutes to 1.0 hours. Among them, the fine-grained oxide ceramic powder includes: Al2O3 with a content of 65-75wt%, ZrO2, MgO, TiO2, CaO sintering aids with a content of 33.5-23.5wt%, and active metal additives (Cu or Mn) with a content of 1.5wt%, the particle size of Al2O3 is 20μm-150μm, and the particle size of each additive is 35-75μm.
[0023] Green body forming: The mixed powder is sent into a spiral mixer and mixed with sodium butadiene rubber solution as a forming agent. After the slurry is stirred evenly, it is injected into an iron cast infiltration block mold and pins are inserted to form a cast infiltration block green body.
[0024] Drying of the blank: Use a fan to air-dry the cast infiltration block blank for at least 16 hours, remove the mold, take out the blank and send it into a steam drying furnace, recover the paraffin in the drying furnace at 80-100℃, and take it out after cooling.
[0025] Green body sintering: Place the dried and dewaxed green body into a vacuum furnace, set the control parameters of the vacuum furnace (such as heating time, insulation time, temperature control range, etc.), turn on the vacuum pump and perform heating and sintering: In the first stage, the temperature is slowly increased in the range of 20~950℃. When the temperature is increased to about 300℃, the vacuum degree begins to decrease, indicating that the binder in the cast infiltration block begins to decompose, and the ash and flying objects begin to escape. When the temperature rises to about 900℃, the vacuum degree in the furnace is relatively high, indicating that the binder has been decomposed and the flying objects have been removed. At this time, the vacuum pump is turned off and argon gas (3-5Mpa) is slowly introduced to control the metallization of the oxide ceramics. When it reaches 950℃, it is kept warm.
[0026] The second stage is in the range of 950~1270℃. The active metal melts in this stage and then enters liquid phase sintering. The appearance of liquid phase tends to induce Al2O3 recrystallization, but due to the small amount of active metal and the small amount of micro-molten pool formed, Al2O3 has no time to recrystallize. More liquid phase, under the action of electromagnetic force, causes some coarse-grained metal ceramics to adhere to alumina ceramic particles, which plays a role in improving the strength and hardness of the cast infiltration block.
[0027] The third stage is in the range of 1270~1400℃, and its heating rate is slower than the first two stages. Because low-temperature sintering is different from the traditional high-temperature sintering of 1600℃, the cast infiltration block must have sufficient time to undergo physical and chemical reactions in the furnace to allow the alumina ceramic to complete solid melting and recrystallization. When the sintering temperature reaches 1400℃, it enters the cooling stage, and the vacuum pump is turned on until the temperature in the furnace drops to about 150℃. The furnace door is opened to unload the cast infiltration block, and the cast infiltration block is checked for edge loss, corner loss, cracks, looseness, etc. The yield of the present invention is above 98%.
[0028] The application of the heterogeneous ceramic cast-infiltration block in the present invention is carried out according to the following method.
[0029] Make a water glass sand mold for the required workpiece, insert the obtained cast infiltration block into the mold and fix it, according to C: 3.0-3.35wt%, Si: 0.3-0.9wt%, Mn: 0.7-1.1wt%, Ni: 0.2-0.5wt%, Mo: 0.3-0.4wt%, V: 0.15-0.3wt%, Cu: 0.2-0.5wt%, Cr: 24.0-27.0wt%, Fe as the balance, and the impurity control P≤0.06wt %, S≤0.06wt%, and the weighed raw materials are put into a medium frequency induction furnace to be melted into molten steel. After deoxidation, slag removal and refining, the molten steel is poured into a sand mold at a pouring temperature of 1370℃±10℃ (the pouring temperature of large castings with a thickness of more than 100mm is controlled at about 1360℃). After pouring, dry sand is used to surround the casting box for slow cooling. After cooling, the box is opened for sand removal, and the surface of the casting is ground and polished. Then the casting is sent to the heat treatment workshop for heat treatment.
[0030] It should be further explained that the coarse-grained metal ceramic phase of the cast infiltration block of the present invention contains 55-65wt% TiC as a hard phase, so that the hardness reaches HRC70-73, which is HRC10 higher than the hardness HRC62 of the traditional steel-bonded alloy, and the high hardness characteristics are optimized, especially its temperature memory, so that the high hardness factor will not change with temperature, thereby improving the wear resistance of the cast workpiece.
[0031] The sintering aid in the fine-particle oxide ceramic powder of the present invention is specially designed according to the low-temperature sintering technology used in the present invention, and is significantly different from the sintering aid used in the traditional 1600°C high-temperature sintering. Each element in the sintering aid can promote the low-temperature sintering by forming a solid solution with Al2O3. Among them, TiO2 and MgO can replace aluminum ions in Al2O3 through titanium ions and magnesium ions during the sintering process, thereby forming a substitutional solid solution; while MgO and CaO with lower density can expand in volume during the cooling process after sintering, making the structure of the cast-infiltrate block loose and increasing the porosity, thereby promoting the growth of grains. These pores generated during the sintering process are exactly the effects required by porous materials; ZrO2 will undergo phase change during the sintering process. When the temperature drops to 1000°C, its volume will expand by 3-5% with the occurrence of phase change, leaving the required pores in the cast-infiltrate block. The above pores can be filled in the cast-infiltrate process. At the same time, ZrO2 is also a functional factor left in the cast-infiltrate block. When the cast-infiltrate block is cast in a steel matrix, it will expand in volume with changes in the casting temperature and subsequent heat treatment temperature. The microcracks formed by this expansion can enable the steel matrix to obtain surface energy, thereby playing a role in strengthening and toughening.
[0032] The active metal powder used in the present invention is at least one of Cu and Mn. When they are added to Al2O3 as low-melting materials, the appearance of their molten liquid phase tends to induce recrystallization of Al2O3. However, due to their limited addition amount, only a micro-molten pool can be formed. Combined with the effect of electromagnetic force, Al2O3 will not have time to recrystallize and will adhere to some particles in the coarse-grained metal ceramic component, so that it can withstand the erosion of high-temperature and high-density molten steel during the casting and infiltration process without loosening, breaking or collapsing.
[0033] The above is the preparation, application process and specific design principle of the cast infiltration block of the present invention. The following is the application of several specific embodiments of the present invention.
[0034] According to the above method, several cast infiltration blocks with a size of 25×10×10mm and two identical sand molds were prepared. The cast infiltration block was inserted into one of the molds to pour the above molten steel, and the other mold was poured with traditional Cr26 molten steel. After the same subsequent treatment, two workpiece samples were obtained. The two samples were put into a ball mill. The steel balls in the mill were bearing steel balls. The ratio of balls to samples was 5:1. After 48 hours of wear and tear, the samples were taken out and weighed. The pure Cr26 sample lost 7.8 grams (original weight 485.2 grams, 477.4 grams after wear), and the sample with cast infiltration block lost 1.4 grams (original weight 480.2 grams, 478.8 grams after wear). The difference between the two was 6.4 grams. It can be obtained that the loss of the traditional Cr26 sample is 4.6 times that of the sample with cast infiltration block.
[0035] According to the above method, several cast infiltration blocks with a size of 100×40×40mm were prepared, and the cast infiltration blocks were inserted into the mold to pour the above molten steel. The pouring temperature was about 1370℃. After cooling, sand removal and subsequent treatment were performed to obtain a plate hammer workpiece. The plate hammer workpiece weighed about 60kg. After quality inspection, the plate hammer was used in limestone crushing operations. The service life can reach 66 days, which is at least 52 days longer than the 13-14 days of traditional Cr26 plate hammer, which is about 3.7 times higher.
[0036] According to the above method, several cast infiltration blocks with a size of 250×50×50mm were prepared, and the cast infiltration blocks were inserted into the mold to pour the above molten steel. The pouring temperature was about 1360℃. After cooling, sand removal and subsequent treatment were performed to obtain a plate hammer workpiece. The plate hammer workpiece weighed about 170kg. After quality inspection, the plate hammer was used in pebble crushing operations. The service life can reach 29 days, which is 21 days longer than the 8-day service life of the traditional Cr26 plate hammer, which is about 2.6 times higher.
[0037] From the above examples, it can be concluded that the heterogeneous ceramic infiltration block prepared by vacuum sintering the coarse-grained metal ceramic and fine-grained oxide ceramic powders in the present invention has the characteristics of high porosity, large pores and good permeability. The pore size is indirectly expressed by the gap between the particles in the matrix metal, and the average is about 256 μm (see Figure 3 ), so it can produce a good cast-infiltration bond with the base metal, improving the toughness, rigidity and wear resistance of the base metal, thereby enhancing the impact friction wear, plowing wear and corrosive wear resistance of the plate hammer and other castings (see working wear Figure 4 ), it can be seen that the cast infiltration block has good applicability while increasing the service life of the inlaid casting and reducing the equipment maintenance cost.
[0038] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A heterogeneous ceramic cast infiltration block, characterized in that: The cast infiltration block includes the following phases: coarse-grained metal ceramics with TiC as hard phase and Mn, Ni, Mo, Cr, C, and Fe as bonding phases, with a content of 20-28wt%; fine-grained oxide ceramic powder mixed with Al2O3 as substrate, ZrO2, MgO, TiO2, and CaO as sintering aids, and one of Cu and Mn as active metal additives, with a content of 80-72wt%.
2. A heterogeneous ceramic cast block according to claim 1, characterized in that: The coarse-grained cermet has a hard phase TiC content of 55-65 wt %, and a bonding phase content of 45-35 wt %.
3. The heterogeneous ceramic cast block according to claim 1, characterized in that: The fine-particle oxide ceramic powder has an Al2O3 content of 65-75wt%, a sintering aid content of 33.5-23.5wt%, and an active metal additive content of 1-2wt%.
4. The method for preparing a heterogeneous ceramic cast-infiltration block according to claim 1, characterized in that: The preparation method comprises the following steps: Coarse particle preparation: After the coarse particle metal ceramic raw materials are mixed by powder metallurgy method, Sintering in vacuum at 1400-1500℃, cooling the sintered material to room temperature, and then mechanically crushing it to obtain irregular particles; Phase mixing: the prepared coarse-grained metal ceramic, fine-grained oxide ceramic powder and pore-increasing agent paraffin are mixed evenly, and the amount of paraffin added is 12-18% of the total mass; Green body molding: sodium butadiene rubber solution as a molding agent is added to the mixed powder, and then poured into a mold to form a cast infiltration block green body; Drying of green body: After the green body is air-dried for at least 16 hours, it is removed from the mold and placed in a steam drying furnace to recover the paraffin wax at 80-100℃; Green body sintering: The dried and dewaxed green body is placed in a vacuum furnace for vacuum sintering in three stages. The first stage is in the range of 20~950℃. When the vacuum degree rises to about 900℃, the vacuum pump is turned off and argon gas is introduced. The second stage is in the range of 950~1270℃, when liquid phase is formed and a micro-molten pool appears. The third stage is slowly heated in the range of 1270~1400℃. After the sintering temperature is reached, the vacuum pump is turned on to exhaust the gas in the furnace, and the cast infiltration block is obtained after accelerated cooling.
5. The method for preparing a heterogeneous ceramic cast-infiltration block according to claim 4, characterized in that: The fine-grained oxide ceramic powder in the phase mixing step has an Al2O3 powder particle size range of 20 μm-150 μm, and a sintering aid and an active metal aid powder particle size range of 35-75 μm.
6. The method for preparing a heterogeneous ceramic cast-infiltration block according to claim 4, characterized in that: During the green body sintering step, argon is slowly introduced to 3-5 MPa.
7. The use of the heterogeneous ceramic cast-infiltration block according to claim 1, characterized in that: The cast block is inserted into a water glass sand mold, and molten steel is poured into the mold for inlay casting. The inlay casting temperature is controlled at 1370°C±10°C. After the pouring is completed, the casting box is surrounded by dry sand for slow cooling. After cooling, the box is opened to remove the sand, and the surface of the workpiece is ground, polished and heat treated.
8. The use of the heterogeneous ceramic cast-infiltration block according to claim 7, characterized in that: The components of the molten steel are: C: 3.0-3.35wt%, Si: 0.3-0.9wt%, Mn: 0.7-1.1wt%, Ni: 0.2-0.5wt%, Mo: 0.3-0.4wt%, V: 0.15-0.3wt%, Cu: 0.2-0.5wt%, Cr: 24.0-27.0wt%, and Fe is the balance. The components of the molten steel are smelted in a medium frequency induction furnace, and after deoxidation, slag removal and refining, they are poured out of the furnace.
9. The use of the heterogeneous ceramic cast-infiltration block according to claim 7, characterized in that: The shape of the mold is a crusher hammer.