High-toughness metal powder cored wire and preparation method and application thereof

By adding Mo element to the titanium alloy welding wire, adjusting the alloy composition and particle size, and refining the grains, the problem of insufficient performance of titanium alloy welding materials under extreme conditions is solved, and high-strength, toughness and low-cost welding effects are achieved, which is suitable for Industrial application.

CN118752116APending Publication Date: 2024-10-11HEFEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410806912.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-18
Filing Date
2024-06-21
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing titanium alloy welding materials lack metal cored wires with high strength, toughness and high hardness. In particular, there are few studies on the effect of the addition of molybdenum on the high-temperature β phase transition temperature of titanium alloys, resulting in insufficient performance of welding materials under extreme conditions. .

Method used

Using a metal powder core containing Mo element, by adjusting the mass percentage and particle size of Mo, Al, V, Fe, C, O, N, 15-20% of the metal powder core is prepared and filled in the titanium belt to form a high strength and toughness Metal powder cored welding wire, and the deposited metal is prepared on the TC4 plate through MIG welding. The Mo element is used to expand the β phase transition temperature, promote lattice distortion and non-uniform nucleation, and refine the grains.

Benefits of technology

A high-strength, tough and low-cost welding wire has been achieved, with significantly improved microhardness, high welding efficiency, and excellent mechanical properties of the deposited metal, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118752116A_ABST
    Figure CN118752116A_ABST
Patent Text Reader

Abstract

The invention discloses a high-toughness metal powder core welding wire and a preparation method and application thereof, and belongs to the technical field of welding wires, the high-toughness metal powder core welding wire is particularly used for preparing deposited metal through TC4, the welding wire comprises a titanium belt and a metal powder core, the titanium belt is filled with the metal powder core, and the metal powder core comprises 0.5%-2.0% of Mo, 6.0%-6.5% of Al, 3.8%-4.5% of V, 0.14%-0.18% of Fe, 0.01%-0.03% of C, 0.12%-0.18% of O, 0.05%-0.08% of N and the balance Ti. The high-toughness metal powder core welding wire is stable in performance, high in welding efficiency and attractive in weld joint forming. When a proper amount of Mo is added into the powder core, deposited metal grains prepared on a TC4 plate in an MIG welding mode are refined, the solid solution strengthening and lattice distortion effects are improved, the mechanical property of deposited metal is excellent, and the hardness is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of welding in material processing engineering, and specifically relates to a high-strength and tough metal powder core welding wire and a preparation method and application thereof. Background Art

[0002] In actual engineering applications, the grains of metal materials are coarse, and microscopic defects such as pores and inclusions will cause insufficient strength and toughness of the material, which may lead to serious safety accidents in normal use or in extreme situations. Titanium alloy is an important strategic metal in the aerospace, marine engineering, medical and other industries, and its strength and toughness are also the focus and hotspot of research at home and abroad.

[0003] Microstructure research on titanium alloys shows that β-phase titanium alloys have smaller grain sizes than α-phase titanium alloys. The appropriate addition of Mo elements can effectively inhibit the formation and growth of phases, enhance the stability of the β-phase in TC4 titanium alloy materials, and maintain a relatively high content at various temperatures. At the same time, the atomic radius of Mo elements is very close to that of titanium, which is conducive to the formation of a stable solid solution, so that the solid solution strengthening and lattice distortion effects are improved, and the hardness of the weld layer is greatly improved.

[0004] At present, the research and development of titanium alloy welding materials at home and abroad is still in its infancy, and most of the related titanium alloy welding wire invention patents belong to the field of solid welding wire. For example, patent CN116329800A discloses a highly wear-resistant and impact-resistant carbon-titanium alloy welding wire and its preparation method; patent CN116460480A discloses a special welding wire suitable for titanium, tungsten, niobium and zirconium low-temperature titanium alloys; patent CN111745268A discloses a self-shielded flux-cored welding wire suitable for TC4 titanium alloy welding and its preparation method.

[0005] Considering that molybdenum can expand the β phase transformation temperature in titanium alloys, more high-temperature β phases can be retained at room temperature or low temperature, and the grains can be refined to increase the hardness of the deposited layer metal. At present, there is little research on the effect of molybdenum addition on the high strength and toughness of titanium alloys, and there is no method for preparing high-strength and tough titanium alloys using titanium metal powder cored welding wires containing molybdenum elements. Summary of the invention

[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide a metal powder core containing Mo element which can be used to prepare high-strength and toughness weld metal.

[0007] The technical problem that the present invention also aims to solve is to provide a high-strength and tough metal powder core welding wire with stable performance and high welding efficiency.

[0008] The final technical problem to be solved by the present invention is to provide the application of metal powder core and metal powder core welding wire in the preparation of deposited metal with excellent mechanical properties and high hardness.

[0009] Technical solution: In order to solve the above technical problems, the present invention provides a metal powder core, which comprises the following components in mass percentage: Mo 0.5%~2.0%, Al 6.0%~6.5%, V 3.8%~4.5%, Fe0.14%~0.18%, C 0.01%~0.03%, O 0.12%~0.18%, N 0.05%~0.08%, and the balance is Ti.

[0010] The metal powder core comprises the following components by mass percentage: Mo 0.5%-2.0%, Al 6.0%-6.5%, V 3.8%-4.5%, Fe 0.14%-0.18%, C 0.01%-0.03%, O 0.12%-0.18%, N 0.05%-0.08%, and the balance is Ti.

[0011] Among them, the particle size of each component of Mo, Al, V, Fe, C, and Ti in the metal powder core is 200 mesh to 300 mesh. If the powder particle size is too large, it is difficult to draw the welding wire, and if the particle size is too small, the powder fluidity will deteriorate.

[0012] The present invention also provides a high-strength and toughness metal powder cored welding wire, which comprises a titanium strip and the metal powder core, wherein the metal powder core is filled in the titanium strip.

[0013] The metal powder core accounts for 15-20% of the total weight of the high-strength and tough metal powder core welding wire.

[0014] The titanium strip is TA1, and its specific components by mass percentage are N: ≤0.03%, H: 0.015%, and the balance is Ti.

[0015] Wherein, the thickness×width of the TA1 titanium strip is 0.8×12 mm.

[0016] Wherein, the diameter of the welding wire is one of 1.6 and 2.0 mm.

[0017] The present invention provides a method for preparing the high-strength and toughness metal powder cored welding wire, comprising the following steps:

[0018] (1) rolling the outer steel strip and bending it into a "U" shape to obtain a U-shaped steel strip;

[0019] (2) feeding the metal powder core into the U-shaped steel strip through a powder feeder at a weight of 15 to 20% of the total weight of the welding wire, and then rolling and sealing the upper opening of the U-shaped steel strip to form a tubular steel strip;

[0020] (3) The tubular steel strip is drawn and reduced in diameter until the diameter is 1.6 or 2.0 mm to obtain the high-strength and tough metal powder cored welding wire.

[0021] The present invention also provides the use of the metal powder core and the metal powder core welding wire in preparing deposited metal, specifically, it is used for preparing deposited metal by TC4. Specifically, when Mo is added, the deposited metal is prepared on the TC4 plate by MIG welding.

[0022] Mechanism of the present invention: The present invention adds molybdenum elements that improve the stability of β phase, which can expand the β phase transformation temperature, so that more high-temperature β phase is retained at room temperature or low temperature, and more β phase is obtained to refine the grains and improve the hardness of the deposited layer. In addition, the addition of molybdenum elements increases the supercooling degree of the alloy during solidification, promotes nucleation, and the solid solution behavior of molybdenum elements also causes lattice distortion in the crystal structure, hindering the growth of grains, all of which lead to the grain size becoming finer and the toughness can be improved. In addition, the molybdenum elements added in the present invention can promote the formation of basket structures at the top, middle and bottom of the welding wire deposited metal. The addition of molybdenum elements will introduce a large amount of lattice distortion, which limits the normal growth of grains during solidification; secondly, with the continuous increase in the amount of Mo added, the supercooling degree of the alloy during solidification will also increase. This change in temperature gradient promotes the occurrence of non-uniform nucleation, thereby leading to the appearance of more nuclei. These new nuclei grow rapidly along their respective orientations and eventually meet to form a basket structure, thereby achieving the refinement of the grain size.

[0023] Beneficial effects: Compared with the prior art, the present invention has the following advantages: the high-strength and toughness metal powder cored welding wire of the present invention only adds a small amount of low-cost molybdenum element, and exhibits excellent high strength and toughness. Therefore, the high-strength and toughness metal powder cored welding wire alloy of the present invention has the advantage of low cost. More importantly, the high-strength and toughness metal powder cored welding wire of the present invention is simple to prepare, easy to mass produce, and has good industrial application value. The molybdenum-containing high-strength and toughness titanium alloy of the present invention has an average microhardness of 462.4HV at the top, 433.6HV at the middle, and 442.3HV at the bottom under the addition of 1.50wt.%, and the hardness of each region is greatly improved compared with the hardness of each region without Mo addition. The high-strength and toughness metal powder cored welding wire of the present invention has stable performance, high welding efficiency, and beautiful weld formation. When the present invention adds a Mo content of 1.50wt.%, the deposited metal grains prepared by MIG welding on the TC4 plate are refined, and the solid solution strengthening and lattice distortion effects are improved, the mechanical properties of the deposited metal are excellent, and the hardness is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1This is the metallographic structure diagram of the deposited metal when the molybdenum content in comparative example 1 is 0.00% (mass percentage of the total weight of the welding wire).

[0025] Figure 2 This is the metallographic structure diagram of the deposited metal when the molybdenum content of Example 2 is 0.5% (mass percentage content of the total weight of the welding wire).

[0026] Figure 3 This is the metallographic structure diagram of the deposited metal when the molybdenum content of Example 1 is 1.5% (mass percentage content of the total weight of the welding wire). DETAILED DESCRIPTION

[0027] The present invention can be better understood according to the following examples. However, the specific drug core component ratios, process conditions and results described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.

[0028] The welding wire components used in the following embodiments are: Mo 0.5%-2.0%, Al 6.0%-6.5%, V 3.8%-4.5%, Fe 0.14%-0.18%, C 0.01%-0.03%, O 0.12%-0.18%, N 0.05%-0.08%, and the balance is Ti.

[0029] Example 1

[0030] A high-strength and tough metal powder core welding wire comprises a titanium strip TA1 and metal powders, wherein each metal powder in the powder core is filled in the titanium strip. The composition of the titanium strip TA1 is N: ≤0.03%, H: 0.015%, and the balance is Ti. The metal powders are prepared as follows according to the mass percentage content of the total weight of the welding wire: Mo 1.5%, Al 6.5%, V 3.8%, Fe 0.14%, C 0.01%, and the balance is Ti. The preparation method is as follows: all powders are sieved through 200 mesh and 300 mesh sieves respectively to ensure that the powder particle size is 200 mesh to 300 mesh. The various powders are placed in a powder mixer and mixed for 60 minutes, and then the mixed powder is added to a U-shaped 0.8mm×12mm titanium strip groove, with a filling rate of 18%. The U-shaped groove is then closed to wrap the powder therein. The tubular steel strip is drawn and reduced in diameter until the diameter is 2.0mm to obtain the high-strength and tough metal powder core welding wire.

[0031] Example 2

[0032] A high-strength and tough metal powder core welding wire comprises a titanium strip TA1 and metal powders, wherein each metal powder in the powder core is filled in the titanium strip. The composition of the titanium strip TA1 is N: ≤0.03%, H: 0.015%, and the balance is Ti. The metal powders are prepared as follows according to the mass percentage content of the total weight of the welding wire: Mo 0.5%, Al 6.3%, V 4.5%, Fe 0.18%, C 0.03%, and the balance is Ti. The preparation method is as follows: all powders are sieved through 200 mesh and 300 mesh sieves respectively to ensure that the powder particle size is 200 mesh to 300 mesh. The various powders are placed in a powder mixer and mixed for 60 minutes, and then the mixed powder is added to a U-shaped 0.8mm×12mm titanium strip groove, and the filling rate is 15%. The U-shaped groove is then closed to wrap the powder therein. The tubular steel strip is drawn and reduced in diameter until the diameter is 2.0mm to obtain the high-strength and tough metal powder core welding wire.

[0033] Example 3

[0034] A high-strength and tough metal powder core welding wire comprises a titanium strip TA1 and metal powders, wherein each metal powder in the powder core is filled in the titanium strip. The composition of the titanium strip TA1 is N: ≤0.03%, H: 0.015%, and the balance is Ti. The metal powders are prepared as follows according to the mass percentage content of the total weight of the welding wire: Mo 2.0%, Al 6.0%, V 4.0%, Fe 0.14%, C 0.01%, and the balance is Ti. The preparation method is as follows: all powders are sieved through 200 mesh and 300 mesh sieves respectively to ensure that the powder particle size is 200 mesh to 300 mesh. The various powders are placed in a powder mixer and mixed for 60 minutes, and then the mixed powder is added to a U-shaped 0.8mm×12mm titanium strip groove, with a filling rate of 20%. The U-shaped groove is then closed to wrap the powder therein. The tubular steel strip is drawn and reduced in diameter until the diameter is 2.0mm to obtain the high-strength and tough metal powder core welding wire.

[0035] Example 4

[0036] A high-strength and tough metal powder core welding wire comprises a titanium strip TA1 and metal powders, wherein each metal powder in the powder core is filled in the titanium strip. The composition of the titanium strip TA1 is N: ≤0.03%, H: 0.015%, and the balance is Ti. The metal powders are prepared as follows according to the mass percentage content of the total weight of the welding wire: Mo 1.0%, Al 6.5%, V 3.8%, Fe 0.16%, C 0.02%, and the balance is Ti. The preparation method is as follows: all powders are sieved through 200 mesh and 300 mesh sieves respectively to ensure that the powder particle size is 200 mesh to 300 mesh. The various powders are placed in a powder mixer and mixed for 60 minutes, and then the mixed powder is added to a U-shaped 0.8mm×12mm titanium strip groove, and the filling rate is 17%. The U-shaped groove is then closed to wrap the powder therein. The tubular steel strip is drawn and reduced in diameter until the diameter is 2.0mm to obtain the high-strength and tough metal powder core welding wire.

[0037] Comparative Example 1

[0038] A titanium alloy metal powder cored welding wire comprises a titanium strip TA1 and metal powders, wherein each metal powder in the powder core is filled in the titanium strip. The composition of the titanium strip TA1 is N: ≤0.03%, H: 0.015%, and the balance is Ti. The metal powders are prepared as follows according to the mass percentage content of the total weight of the welding wire: Al 6.5%, V 3.8%, Fe 0.14%, C 0.01%, and the balance is Ti. The preparation method is as follows: all powders are sieved through 200 mesh and 300 mesh sieves respectively to ensure that the powder particle size is 200 mesh to 300 mesh. The various powders are placed in a powder mixer and mixed for 60 minutes, and then the mixed powder is added to a U-shaped 0.8mm×12mm titanium strip groove, with a filling rate of 18%. The U-shaped groove is then closed to wrap the powder therein. The tubular steel strip is drawn and reduced in diameter until the diameter is 2.0mm to obtain the titanium alloy metal powder cored welding wire.

[0039] Comparative Example 2

[0040] A titanium alloy metal powder cored welding wire comprises a titanium strip TA1 and metal powders, wherein each metal powder in the powder core is filled in the titanium strip. The composition of the titanium strip TA1 is N: ≤0.03%, H: 0.015%, and the balance is Ti. The metal powders are prepared as follows according to the mass percentage content of the total weight of the welding wire: Mo 2.3%, Al 6.5%, V 3.8%, Fe 0.14%, C 0.01%, and the balance is Ti. The preparation method is as follows: all powders are sieved through 200 mesh and 300 mesh sieves respectively to ensure that the powder particle size is 200 mesh to 300 mesh. The various powders are placed in a powder mixer and mixed for 60 minutes, and then the mixed powder is added to a U-shaped 0.8mm×12mm titanium strip groove, with a filling rate of 18%. The U-shaped groove is then closed to wrap the powder therein. The tubular steel strip is drawn and reduced in diameter until the diameter is 2.0mm to obtain the titanium alloy metal powder cored welding wire.

[0041] Comparative Example 3

[0042] A titanium alloy metal powder cored welding wire comprises a titanium strip TA1 and metal powders, wherein each metal powder in the powder core is filled in the titanium strip. The composition of the titanium strip TA1 is N: ≤0.03%, H: 0.015%, and the balance is Ti. The metal powders are prepared as follows according to the mass percentage content of the total weight of the welding wire: Mo 0.2%, Al 6.5%, V 3.8%, Fe 0.14%, C 0.01%, and the balance is Ti. The preparation method is as follows: all powders are sieved through 200 mesh and 300 mesh sieves respectively to ensure that the powder particle size is 200 mesh to 300 mesh. The various powders are placed in a powder mixer and mixed for 60 minutes, and then the mixed powder is added to a U-shaped 0.8mm×12mm titanium strip groove, with a filling rate of 18%. The U-shaped groove is then closed to wrap the powder therein. The tubular steel strip is drawn and reduced in diameter until the diameter is 2.0mm to obtain the titanium alloy metal powder cored welding wire.

[0043] The welding machine used was a MIG-500P fully digital pulse gas shielded welding machine. The base material substrate was TC4 plate with a size of 120mm×50mm×10mm. The base material substrate was polished with sandpaper before the test, and the surface was wiped with alcohol and acetone solution to reduce pollution such as oxide film and oil stains. The welding test adopted the form of DC reverse connection to prepare TC4 deposited metal by surfacing.

[0044] The welding wires obtained in each embodiment and comparative example were subjected to hardness test and tensile test. The hardness test was carried out using HVS100A-XYT automatic image processing fiber Vickers hardness tester, with the load set to 0.3 kgf and the loading time set to 15 s; the speed of the tensile test was 0.1 mm / min.

[0045] As shown in Table 1 and Table 2.

[0046] Table 1 Hardness of deposited metal

[0047] Top average hardness / HV Average hardness of the middle part / HV Bottom average hardness / HV Example 1 462.4 433.6 442.3 Example 2 432.1 402.9 421.2 Example 3 442.1 420.6 432.5 Example 4 460.7 429.8 438.6 Comparative Example 1 382.5 360.9 372.7 Comparative Example 2 430.5 410.5 413.4 Comparative Example 3 411.6 393.8 398.6

[0048] Table 2 Tensile strength and elongation of deposited metal

[0049] Tensile strength / MPa Elongation after break / % Example 1 1145 8.5 Example 2 1075 8.8 Example 3 1139 6.3 Example 4 1109 7.9 Comparative Example 1 1001 9.1 Comparative Example 2 1130 5.9 Comparative Example 3 1028 6.2

[0050] From the results in Table 1 and Table 2, it can be seen that the average hardness of the top, middle and bottom of the deposited metal prepared on the TC4 plate by the welding wire prepared when the Mo content is 1.5% is optimal compared with other embodiments; through the data obtained from the hardness and tensile tests, it can be concluded that the tensile strength of the deposited metal prepared on the TC4 plate by the welding wire prepared when the Mo content is 1.5% is the highest, and the elongation after fracture is appropriate.

[0051] Figure 1 , Figure 2 , Figure 3The following are the microstructure scans of the XY direction of the three kinds of deposited metals of the comparative example 1, the example 2 and the example 1. It can be seen from the figure that the microstructures of the deposited metals of the three kinds of welding wires are all basket structures, and the organization includes a large number of gray-black needle-shaped organizations, a small amount of short rod-shaped organizations and a gray-white organization between the two. There are great differences in the internal structure of the organization. Figure 1 When the Mo addition amount is 0.00wt.%, the gray-black needle-like structure is more and the short rod-like structure is less; when the Mo addition amount is 0.50wt.%, Figure 2 The internal structure is similar to that of the case with 0.00wt.% Mo element addition, with more gray-black needle-like structures and fewer short rod-like structures; when the Mo element addition amount is 1.50wt.%, such as Figure 3 The internal organizational structure of the deposited metal is obviously different from the previous two, showing a fine mesh basket structure. This structure can achieve the refinement of the deposited metal grains and improve the solid solution strengthening and lattice distortion effects. The prepared deposited metal has excellent mechanical properties and greatly improved hardness.

Claims

1. A metal powder core, It is characterized in that The metal powder core comprises the following components by mass percentage: Mo 0.5%-2.0%, Al 6.0%-6.5%, V 3.8%-4.5%, Fe 0.14%-0.18%, C 0.01%-0.03%, O 0.12%-0.18%, N 0.05%-0.08%, and the balance is Ti.

2. The metal powder core according to claim 1, It is characterized in that The metal powder core comprises the following components by mass percentage: Mo 0.5%-2.0%, Al 6.0%-6.5%, V 3.8%-4.5%, Fe 0.14%-0.18%, C 0.01%-0.03%, O 0.12%-0.18%, N 0.05%-0.08%, and the balance is Ti.

3. The metal powder core according to claim 1, It is characterized in that The particle size of each component of Mo, Al, V, Fe, C and Ti in the metal powder core is 200-300 meshes.

4. A high-strength and tough metal powder cored welding wire, It is characterized in that The high-strength and toughness metal powder cored welding wire comprises a titanium strip and the metal powder core according to any one of claims 1 to 3, wherein the metal powder core is filled in the titanium strip.

5. The high-strength and tough metal powder cored welding wire according to claim 4, It is characterized in that The metal powder core accounts for 15-20% of the total weight of the high-strength and tough metal powder core welding wire.

6. The high-strength and tough metal powder cored welding wire according to claim 4, It is characterized in that The titanium strip is TA1, and its specific components by mass percentage are N: ≤0.03%, H: 0.015%, and the balance is Ti.

7. The high-strength and tough metal powder cored welding wire according to claim 6, It is characterized in that The thickness×width of the TA1 titanium strip is 0.8×12 mm.

8. The high-strength and tough metal powder cored welding wire according to claim 4, It is characterized in that The diameter of the welding wire is one of 1.6 mm and 2.0 mm.

9. The method for preparing the high-strength and tough metal powder cored welding wire according to any one of claims 4 to 8, It is characterized in that The steps include: (1) Rolling the outer steel strip and bending it into a "U" shape to obtain a U-shaped steel strip; (2) The metal powder core according to any one of claims 1 to 3 is fed into a U-shaped steel strip through a powder feeder at a weight of 15 to 20% of the total weight of the welding wire, and then the upper opening of the U-shaped steel strip is rolled and sealed to form a tubular steel strip; (3) The tubular steel strip is drawn and reduced in diameter until the diameter is 1.6 or 2.0 mm to obtain the high-strength and tough metal powder cored welding wire.

10. Use of the metal powder core according to any one of claims 1 to 3 and the metal powder core welding wire according to any one of claims 4 to 8 in preparing deposited metal.