Preparation method and application for rapidly generating all-intermetallic compound joint
By using electrodeposition method under micro-pressure and low-temperature conditions to form copper micro-nano structures, it promotes the diffusion connection between the substrate and the intermediate layer, solves the problem that traditional packaging technology cannot meet the working requirements of semiconductor devices under high-temperature conditions, and achieves fast and efficient full-scale packaging. The preparation of intermetallic compound joints improves the high temperature resistance and process simplicity of the joints.
Patent Information
- Application Number
- CN202410809463.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-21
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-21
AI Technical Summary
Traditional packaging technology cannot meet the working requirements of semiconductor devices under extreme high-temperature conditions, especially the high-temperature service requirements of third-generation semiconductor devices, and traditional soldering methods can cause high-temperature damage to chips and packaging systems.
Fully intermetallic compound joints are quickly prepared through transient liquid phase connection technology (TLP) under micro-pressure and low-temperature conditions. The copper micro-nano structure is formed on the surface of the substrate through electrodeposition to promote the diffusion connection between the substrate and the intermediate layer and reduce the cost of welding. consume energy and improve the high temperature resistance of the joint.
It realizes the rapid generation of all-metallic compound joints under micro-pressure and low temperature conditions, improves the welding efficiency and the high-temperature resistance of the joints, meets the high-temperature service requirements of third-generation semiconductor devices, while simplifying the process and reducing energy consumption.
Smart Images

Figure CN118752178A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electronic packaging, and in particular relates to a preparation method and application of a rapidly generated full intermetallic compound joint. Background Art
[0002] With the rapid development of semiconductor technology, the goal of highly integrated and miniaturized electronic devices has been achieved. The problem that power devices cannot quickly dissipate heat in a small space has emerged, resulting in long-term service at high temperatures. Especially in special environments such as nuclear energy and aerospace, the operating environment temperature of semiconductor devices exceeds 500°C. Traditional silicon devices will fail due to the junction temperature effect when the operating temperature exceeds 150°C, and cannot meet the requirements of scientific and technological development. This problem was not solved until the emergence of third-generation semiconductors. However, traditional packaging technology and interface connection materials still cannot meet the requirements of devices working under extreme high temperature conditions. If the traditional brazing method is used to solve the problem, a higher melting point brazing material and a higher process temperature are required. The high temperature generated will directly damage the chip and cause high residual stress, thereby damaging the packaging system. Therefore, it is of far-reaching significance to develop high-temperature service connection technology corresponding to the third-generation semiconductor.
[0003] At present, particle sintering, high-temperature brazing and transient liquid phase connection technology (TLP) are the mainstream packaging technologies for third-generation semiconductor devices. Au-based, Bi-based, Sn-based and high-Pb solders are currently commonly used high-temperature interconnect materials. Among them, Sn-based solders are widely used because of their moderate price, good electrical and thermal conductivity, and excellent wettability. However, its melting point is lower than the requirements of high-temperature interconnect packaging, and the problem of low shear strength also needs to be solved. The emergence of particle sintering technology is closely related to the properties of nanomaterials. The nanometer size of nanomaterials makes the materials have special surface effects, interface effects, dielectric effects and quantum size effects. Nanomaterials can be spontaneously connected at low temperatures, and when they are sintered into blocks, they still maintain their physical properties as metals. Therefore, the working environment requirements of the third-generation semiconductors are met within a certain range, but after the nanoparticles are sintered, the particles will agglomerate, there will be a large number of pores, and the cost is high. The essence of TLP is that after the high-melting point metal and the low-melting point metal are bonded at low temperature, the metal compound with a high melting point is produced. The metal compound is used as a connecting layer to allow the interconnect material to meet the high-temperature working environment. The solder joints prepared by TLP technology are sandwich structures, with low-melting-point metals sandwiched between high-melting-point metals. After welding, the middle layer is composed of metal compounds. However, when making connections, long-term continuous high-temperature heating is required, resulting in serious energy consumption. Summary of the invention
[0004] The purpose of the present invention is to solve the problems of long manufacturing time, high applied pressure and poor physical and mechanical properties of existing power chip high temperature resistant welding joints, and to provide a preparation method and application of rapidly generated full intermetallic compound joints.
[0005] The invention provides a method for rapidly preparing a full intermetallic compound joint for power device packaging by transient liquid phase connection technology under micro-pressure and low temperature conditions.
[0006] A preparation method for rapidly generating a full intermetallic compound joint is specifically completed by the following steps:
[0007] 1. Preprocessing:
[0008] First, the surface of the pure copper plate is polished with sandpaper, then pickled, rinsed with deionized water, and dried to obtain a pretreated pure copper plate;
[0009] 2. Prepare the electrodeposition solution:
[0010] Copper sulfate pentahydrate, boric acid and Janus green are sequentially added into deionized water, heated and magnetically stirred to obtain an electrodeposition solution;
[0011] 3. Electrodeposition:
[0012] The pretreated pure copper plate is immersed in an electrodeposition solution, direct current electrodeposition is used, and then the electrodeposited sample is cleaned and dried to obtain a copper plate with a copper micro-nano structure;
[0013] Fourth, put the tin foil into anhydrous ethanol for ultrasonic cleaning, take it out and dry it to obtain the cleaned tin foil;
[0014] 5. Place the cleaned tin foil between two copper plates with copper micro-nano structures, and make the tin foil contact with the copper micro-nano structures on the upper and lower copper plates to form a copper-tin-copper "sandwich" structure, and then apply solder paste around the "sandwich" structure;
[0015] 6. Place the copper-tin-copper "sandwich" structure on the workbench of a hot press welding machine, control the heating temperature to 250°C, and perform brazing at 250°C for 1min to 7min. Continuously apply pressure during the brazing process to obtain a full intermetallic compound joint.
[0016] Principle of the present invention:
[0017] 1. The present invention micronizes the surface of the substrate, allowing the nano tips with special size effect to directly pierce the oxide film on the surface of the solder and reach the inside of the solder, making the surface of the copper substrate more prone to automatic diffusion and recrystallization, and the generated intermetallic compounds can still serve at high temperatures, improving the welding efficiency of the transient liquid phase connection technology (TLP), thereby reducing the high energy consumption problem in the TLP connection; In summary, in order to reduce the welding conditions in the TLP process and promote the diffusion connection between the substrate and the intermediate layer, it is very meaningful to prepare a micro-nano scale coating on the surface of the substrate, the intermediate layer cost of the transient liquid phase connection technology (TLP) is low, and the generated intermetallic compounds can meet the conditions for high temperature service;
[0018] 2. The present invention prepares a copper micro-nano surface structure with a (111) crystal orientation by a green electrodeposition method, and by forming a micro-nano structure-brazing material-micro-nano structure solder joint, the tip of the copper micro-nano structure with a special size effect directly pierces the oxide film on the surface of the brazing material and diffuses directly into the interior, thereby achieving the purpose of quickly generating a full metal compound joint under micro-pressure and low temperature conditions; the full metal compound joint prepared by the present invention has excellent high temperature resistance and can meet the high temperature service requirements of the third-generation semiconductor power devices.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. When sanding, use 400#, 800#, 1500#, 3000#, and 5000# sandpaper in turn to remove the oxide layer on the surface of the material. Polish the copper plate on a polishing machine equipped with 2000# water sandpaper, and build micro-nano grooves on the surface of the material by physical grinding, so that ions are attached to the original micro-nano protrusions and discharge, making the grains finer and the bonding force between the copper substrate and the deposition layer stronger;
[0021] 2. The electrodeposition solution mainly includes copper sulfate pentahydrate, boric acid and Janus green. The exchange time of the electrodeposition solution is between 4min and 16min, and the current density is 0.4A / dm 2 ~2.4A / dm 2 The temperature is between 20 and 60°C; the above components form a solution suitable for high current density electroplating copper layer; the current density filling will not cause problems such as voids and burns, and the surface is bright, which can effectively prevent the defects of uneven electrodeposition layer caused by voids and burns;
[0022] 3. During welding, the copper micro-nanostructure prepared by electrodeposition greatly improves the wettability of liquid tin, eliminates interface voids, and reduces bonding time and temperature;
[0023] 4. The method provided by the present invention for rapidly generating all-metallic compound joints under micro-pressure and low-temperature conditions has the advantages of simple process, easy control of parameters, high process repeatability and stable system, which meets the requirements of energy conservation and emission reduction in current policy development and has better production and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 Surface morphology diagram, in which (a) is a copper plate with a copper micro-nano structure obtained in step 3 of Example 1, (b) is a copper plate with a copper micro-nano structure obtained in step 3 of Example 2, (c) is a copper plate with a copper micro-nano structure obtained in step 3 of Example 3, and (d) is an ordinary copper plate without any treatment;
[0025] Figure 2 XRD patterns of the copper micro-nanostructures with (111) crystal orientation on the surface of the copper plates prepared in Examples 1, 4, 5 and 6 and the ordinary copper plates without any treatment;
[0026] Figure 3 The cross-sectional views of the all-metallic compound joints prepared in Examples 1 and 7, wherein (a) is Example 1 and (b) is Example 7;
[0027] Figure 4 The fracture diagrams of the shear test of the all-metallic compound joints prepared in Examples 1 and 7;
[0028] Figure 5 is the shear strength of the weld point, (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Control Example 1. DETAILED DESCRIPTION
[0029] Specific implementation method 1: This implementation method is a preparation method for rapidly generating a full metal compound joint, which is specifically completed according to the following steps:
[0030] 1. Preprocessing:
[0031] First, the surface of the pure copper plate is polished with sandpaper, then pickled, rinsed with deionized water, and dried to obtain a pretreated pure copper plate;
[0032] 2. Prepare the electrodeposition solution:
[0033] Copper sulfate pentahydrate, boric acid and Janus green are sequentially added into deionized water, heated and magnetically stirred to obtain an electrodeposition solution;
[0034] 3. Electrodeposition:
[0035] The pretreated pure copper plate is immersed in an electrodeposition solution, direct current electrodeposition is used, and then the electrodeposited sample is cleaned and dried to obtain a copper plate with a copper micro-nano structure;
[0036] Fourth, put the tin foil into anhydrous ethanol for ultrasonic cleaning, take it out and dry it to obtain the cleaned tin foil;
[0037] 5. Place the cleaned tin foil between two copper plates with copper micro-nano structures, and make the tin foil contact with the copper micro-nano structures on the upper and lower copper plates to form a copper-tin-copper "sandwich" structure, and then apply solder paste around the "sandwich" structure;
[0038] 6. Place the copper-tin-copper "sandwich" structure on the workbench of a hot press welding machine, control the heating temperature to 250°C, and perform brazing at 250°C for 1min to 7min. Continuously apply pressure during the brazing process to obtain a full intermetallic compound joint.
[0039] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: in step 1, the surface of the pure copper plate is polished using 400#, 800#, 1500#, 3000#, and 5000# sandpapers in sequence, and then the copper plate is polished on a polishing machine equipped with 2000# water sandpaper for 1 minute. The other steps are the same as those of specific implementation method 1.
[0040] Specific implementation method 3: This implementation method is different from specific implementation method 1 or 2 in that: in step 1, the polished pure copper sheet is pickled with 10% sulfuric acid for 25s to 35s, and then rinsed with deionized water for 3 to 5 times. The other steps are the same as those of specific implementation method 1 or 2.
[0041] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that: the concentration of copper sulfate pentahydrate in the electrodeposition solution described in step 2 is 0.2 mol / L, the concentration of boric acid is 0.2 mol / L to 0.4 mol / L, and the concentration of Janus green is 0.1 g / L to 0.4 g / L; the concentration of boric acid in the preferred electrodeposition solution is 0.3 mol / L, and the concentration of Janus green is 0.2 g / L to 0.3 g / L. The other steps are the same as those in specific embodiments 1 to 3.
[0042] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the heating temperature in step 2 is 40°C to 45°C; the magnetic stirring speed in step 2 is 800r / min to 1200r / min; heating and magnetic stirring in step 2 are performed until copper sulfate pentahydrate, boric acid and Janus green are completely dissolved in deionized water. The other steps are the same as those in specific embodiments 1 to 4.
[0043] Specific embodiment 6: The difference between this embodiment and specific embodiments 1 to 5 is that in step 3, the pretreated pure copper plate is immersed in an electrodeposition solution at a temperature of 20°C to 60°C, and then at a current density of 0.4A / dm 2~2.4A / dm 2 Electrodeposition for 4 to 16 minutes under the conditions of 1.2 A / dm 2 ~2.4A / dm 2 The electrodeposition was carried out for 12 to 16 minutes under the conditions of . The other steps are the same as those in the first to fifth embodiments.
[0044] Specific embodiment 7: The difference between this embodiment and specific embodiments 1 to 6 is that the cleaning described in step 3 is: using anhydrous ethanol and deionized water to clean the electrodeposited sample 1 to 3 times respectively. The other steps are the same as specific embodiments 1 to 6.
[0045] Specific implementation eight: This implementation differs from specific implementations one to seven in that: the thickness of the tin foil in step four is 10 μm to 50 μm; the solder paste in step five is American AMTECH solder paste. The other steps are the same as specific implementations one to seven.
[0046] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: in step 6, brazing is performed at 250° C. for 5 to 7 minutes, and the pressure continuously applied during the brazing process is 0.07 MPa. The other steps are the same as those of specific embodiments 1 to 8.
[0047] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that the full intermetallic compound joint is used for power device packaging. The other steps are the same as those of specific embodiments 1 to 9.
[0048] The following examples are used to verify the beneficial effects of the present invention:
[0049] Example 1: A method for rapidly generating a full intermetallic compound joint is specifically completed by the following steps:
[0050] 1. Preprocessing:
[0051] Prepare two sizes of copper plates, the sizes are 38mm×25mm×1mm and 4mm×4mm×1mm respectively; polish the copper plates of the two sizes respectively, that is, first use 400#, 800#, 1500#, 3000#, 5000# sandpaper to polish the surface of the pure copper plate in sequence, then polish the copper plate on a polishing machine equipped with 2000# water sandpaper for 1 minute, then use 10% sulfuric acid to pickle the polished pure copper sheet for 30 seconds, and then rinse it with deionized water for 5 times; blow dry to obtain the pretreated pure copper plate;
[0052] 2. Prepare the electrodeposition solution:
[0053] Copper sulfate pentahydrate, boric acid and Janus green are added to deionized water in sequence, heated to 40° C., and magnetically stirred at 40° C. and a stirring speed of 1000 r / min until copper sulfate pentahydrate, boric acid and Janus green are completely dissolved in the deionized water to obtain an electrodeposition solution;
[0054] The concentration of copper sulfate pentahydrate in the electrodeposition solution in step 2 is 0.2 mol / L, the concentration of boric acid is 0.3 mol / L, and the concentration of Janus Green is 0.2 g / L;
[0055] 3. Electrodeposition:
[0056] The pretreated pure copper plate was immersed in an electrodeposition solution at a temperature of 40°C and then heated at a current density of 1.2 A / dm 2 The electrodeposition was carried out for 12 minutes under the conditions of , and then the electrodeposited sample was washed with anhydrous ethanol and deionized water respectively and dried, and a copper plate with a copper micro-nano structure was obtained;
[0057] Fourth, put the tin foil into anhydrous ethanol for ultrasonic cleaning for 1 minute, take it out and dry it to obtain the cleaned tin foil;
[0058] The thickness of the tin foil described in step 4 is 20 μm;
[0059] 5. Cut the cleaned tin foil into 4mm×4mm, place a 38mm×25mm×1mm copper plate with a copper micro-nano structure at the bottom, and place a 4mm×4mm×1mm copper plate with a copper micro-nano structure at the top, and place the cleaned tin foil between the two copper plates with copper micro-nano structures, so that the tin foil contacts the copper micro-nano structures on the surfaces of the upper and lower copper plates, respectively, to form a copper-tin-copper "sandwich" structure, and then apply solder paste around the "sandwich" structure;
[0060] The soldering paste described in step 5 is the American AMTECH soldering paste;
[0061] 6. Place the copper-tin-copper "sandwich" structure on the workbench of the hot press welding machine, control the heating temperature to 250°C, and braze for 7 minutes at 250°C. During the brazing process, continuously apply a pressure of 0.07MPa to obtain a full intermetallic compound joint;
[0062] The full intermetallic compound joint obtained in step six is used for power device packaging.
[0063] Example 2: The difference between this example and Example 1 is that in step 3, the pretreated pure copper plate is immersed in an electrodeposition solution at a temperature of 40°C, and then at a current density of 0.4A / dm 2 The other steps and parameters are the same as those in Example 1.
[0064] Example 3: The difference between this example and Example 1 is that the concentration of copper sulfate pentahydrate in the electrodeposition solution described in step 2 is 0.2 mol / L, the concentration of boric acid is 0.3 mol / L, and the concentration of Janus Green is 0.1 g / L. The other steps and parameters are the same as those in Example 1.
[0065] Example 4: The difference between this example and example 1 is that the pretreated pure copper plate is immersed in an electrodeposition solution at a temperature of 40°C and then at a current density of 1.2 A / dm 2 The other steps and parameters are the same as those in Example 1.
[0066] Example 5: The difference between this example and example 1 is that the pretreated pure copper plate is immersed in an electrodeposition solution at a temperature of 40°C and then at a current density of 1.2 A / dm 2 The other steps and parameters are the same as those in Example 1.
[0067] Example 6: The difference between this example and example 1 is that the pretreated pure copper plate is immersed in an electrodeposition solution at a temperature of 40°C and then at a current density of 1.2 A / dm 2 The other steps and parameters are the same as those in Example 1.
[0068] Embodiment 7: The difference between this embodiment and embodiment 1 is that in step 6, brazing is performed at 250° C. for 5 min. The other steps and parameters are the same as those in embodiment 1.
[0069] Comparative Example 1:
[0070] 1. Put the tin foil into anhydrous ethanol for ultrasonic cleaning for 1 minute, take it out and dry it to obtain the cleaned tin foil;
[0071] The thickness of the tin foil described in step 1 is 20 μm;
[0072] 2. Cut the cleaned tin foil into 4mm×4mm, put a copper plate of 38mm×25mm×1mm without any process treatment at the bottom, put a copper plate of 4mm×4mm×1mm without any process treatment at the top, put the cleaned tin foil between the two copper plates, and make the tin foil contact with the upper and lower surfaces of the two pure copper plates respectively to form a copper-tin-copper "sandwich" structure, and then apply solder paste around the "sandwich" structure;
[0073] The soldering paste described in step 2 is American AMTECH soldering paste;
[0074] 3. Place the copper-tin-copper "sandwich" structure on the workbench of the hot press welding machine, control the heating temperature to 250°C, and braze at 250°C for 7 minutes. During the brazing process, continuously apply a pressure of 0.07MPa to obtain a full intermetallic compound joint.
[0075] Figure 1 Surface morphology diagram, in which (a) is a copper plate with a copper micro-nano structure obtained in step 3 of Example 1, (b) is a copper plate with a copper micro-nano structure obtained in step 3 of Example 2, (c) is a copper plate with a copper micro-nano structure obtained in step 3 of Example 3, and (d) is an ordinary copper plate without any treatment;
[0076] from Figure 1 It can be seen that the surface of the micro-nano structure prepared in Example 1 has a unique structure, uniform and dense conical morphology. Figure 1 (a), compared with the current density of less than 0.8A / dm during electrodeposition 2 The fine granular structure prepared is shown in Figure 1 (b) The nodular structure prepared by adding no or less than 0.1 g / L of Janus Green to the electrodeposition solution is shown in FIG. Figure 1 (c) and the smooth and flat surface of ordinary copper plate without any treatment Figure 1 (d).
[0077] Figure 2 XRD patterns of the copper micro-nanostructures with (111) crystal orientation on the surface of the copper plates prepared in Examples 1, 4, 5 and 6 and the ordinary copper plates without any treatment;
[0078] from Figure 2 It can be seen that there is a significant difference in the diffraction peak of the (111) crystal phase between the pure copper plate without electrodeposition and the copper plate with surface micro-nano structure after electrodeposition for 4-16 minutes. With the increase of electrodeposition time, the diffraction peak of the (111) crystal phase gradually increases, indicating that the degree of crystallization of the (111) crystal phase gradually increases.
[0079] Figure 3 The cross-sectional views of the all-metallic compound joints prepared in Examples 1 and 7, wherein (a) is Example 1 and (b) is Example 7;
[0080] The cross-sectional view of the all-metallic compound joint prepared in Example 1 is shown in Figure 3 (a), it can be seen that the joint has been completely formed, and it can be observed that the Cu6Sn5 at both ends have been completely contacted and fused, and the entire interface is completely filled with IMC compounds and no residual tin islands can be observed. The cross-sectional view of the full intermetallic compound joint prepared in Example 7 is shown in Figure 3 (b) The heads of the scallop-shaped Cu6Sn5 at the upper and lower ends began to contact and fuse with each other, generating independent tin islands in the non-contacting intermetallic compound layer.
[0081] Figure 4 The fracture diagrams of the shear test of the all-metallic compound joints prepared in Examples 1 and 7;
[0082] The shear test fracture diagram of the all-metallic compound joint prepared in Example 1 is shown in Figure 4 (a), it can be seen that the fracture is relatively flat, without elongated dimples, and no exposed Cu substrate is found on the fracture surface, so the cracks all occur inside Cu6Sn5, which is a transgranular fracture of Cu6Sn5. There is no plastic deformation in this area, which is a brittle fracture.
[0083] The shear test fracture diagram of the all-metallic compound joint prepared in Example 7 is shown in Figure 4 (b) It can be seen that the Cu6Sn5 with Sn on the surface is distributed on the fracture interface, resulting in an uneven interface. It can be seen that the fracture mainly occurs inside Cu6Sn5, Cu6Sn5 / Cu3Sn, and Cu3Sn, and the fracture mechanism is brittle fracture.
[0084] The pointed cone with unique morphology can greatly improve the bonding force between the substrate surface and the solder, further enhancing the mechanical properties of the solder joint. The shear strength of the solder joint prepared by the surface micro-nano structure prepared by different electrodeposition processes is shown in Figure 5 ;
[0085] Figure 5 is the shear strength of the weld, (a) is Example 1, (b) is Example 2, (c) is Example 3, and (d) is Control Example 1;
[0086] from Figure 5 It can be seen that compared with the shear strength of the solder joint prepared in Example 1, the fine granular structure has no obvious sharp cone on the surface, which will slow down the formation of intermetallic compounds between the solder and the substrate and reduce the connection strength; the nodular structure, due to its uneven cluster morphology and large gaps, further slows down the reaction with the solder, and the shear strength is further reduced; the untreated ordinary copper plate has the slowest reaction with the solder and the lowest shear strength because it does not have a micro-nano structure with special surface energy.
Claims
1. A method for rapidly generating a full metal compound joint, characterized in that The preparation method is specifically completed according to the following steps:
1. Preprocessing: First, the surface of the pure copper plate is polished with sandpaper, then pickled, rinsed with deionized water, and dried to obtain a pretreated pure copper plate; 2. Prepare the electrodeposition solution: Copper sulfate pentahydrate, boric acid and Janus green are sequentially added into deionized water, heated and magnetically stirred to obtain an electrodeposition solution; 3. Electrodeposition: The pretreated pure copper plate is immersed in an electrodeposition solution, direct current electrodeposition is used, and then the electrodeposited sample is cleaned and dried to obtain a copper plate with a copper micro-nano structure; Fourth, put the tin foil into anhydrous ethanol for ultrasonic cleaning, take it out and dry it to obtain the cleaned tin foil; 5. Place the cleaned tin foil between two copper plates with copper micro-nano structures, and place the tin foil in contact with the copper micro-nano structures on the upper and lower copper plates to form a copper-tin-copper "sandwich" structure. Then apply solder paste around the "sandwich" structure.
6. Place the copper-tin-copper "sandwich" structure on the workbench of a hot press welding machine, control the heating temperature to 250°C, and braze at 250°C for 1min to 7min. Apply pressure continuously during the brazing process to obtain a full intermetallic compound joint.
2. A method for preparing a fast-generated all-metallic compound joint according to claim 1, characterized in that In step 1, use 400#, 800#, 1500#, 3000#, and 5000# sandpaper to polish the surface of the pure copper plate in sequence, and then polish the copper plate on a polishing machine equipped with 2000# water sandpaper for 1 minute.
3. A method for rapidly generating a full metal compound joint according to claim 1, characterized in that In step 1, the polished pure copper sheet is pickled with 10% sulfuric acid for 25s to 35s, and then rinsed with deionized water for 3 to 5 times.
4. A method for rapidly generating a full intermetallic compound joint according to claim 1, characterized in that The concentration of copper sulfate pentahydrate in the electrodeposition solution in step 2 is 0.2 mol / L, the concentration of boric acid is 0.2 mol / L to 0.4 mol / L, and the concentration of Janus Green is 0.1 g / L to 0.4 g / L.
5. A method for rapidly generating a full intermetallic compound joint according to claim 1, characterized in that The heating temperature in step 2 is 40° C. to 45° C.; the magnetic stirring speed in step 2 is 800 r / min to 1200 r / min; heating and magnetic stirring in step 2 are performed until copper sulfate pentahydrate, boric acid and Janus green are completely dissolved in deionized water.
6. A method for rapidly generating a full metal compound joint according to claim 1, characterized in that In step 3, the pretreated pure copper plate is immersed in an electrodeposition solution at a temperature of 20°C to 60°C, and then the electrodeposition solution is heated at a current density of 0.4A / dm 2 ~2.4A / dm 2 The electrodeposition was carried out for 4 min to 16 min under the conditions of .
7. A method for rapidly generating a full metal compound joint according to claim 1, characterized in that The cleaning described in step three is: using anhydrous ethanol and deionized water to clean the electrodeposited sample 1 to 3 times respectively.
8. A method for rapidly generating a full metal compound joint according to claim 1, characterized in that The thickness of the tin foil described in step 4 is 10 μm to 50 μm; the soldering paste described in step 5 is American AMTECH soldering paste.
9. A method for rapidly generating a full metal compound joint according to claim 1, characterized in that In step six, brazing is performed at 250° C. for 5 to 7 minutes, and the pressure continuously applied during the brazing process is 0.07 MPa.
10. Application of the all-metallic compound joint prepared by the preparation method according to claim 1, characterized in that Full intermetallic compound joints are used in power device packaging.
Citation Information
Patent Citations
Method for rapidly preparing electronic packaging material Cu3Sn intermetallic compound
CN107096988A
Low-temperature chip surface-mounted method free of organic matters and chip surface-mounted structure
CN108305838A
Preparation method of hydrophobic corrosion-resistant copper coating with surface micro-nano structure
CN117089902A
Method for realizing aluminum alloy reaction diffusion bonding by depositing copper nano layer on interface
CN118081054A
Enhanced Adhesion by Nanoparticle Layer Having Randomly Configured Voids
US20180138110A1