Corrosion prevention method for pure water hydraulic support stand column and pure water hydraulic support stand column
Using laser cladding and arc surfacing technology to form a stainless steel protective layer on the hydraulic support column, combined with nitriding treatment, the corrosion and wear resistance problems of the pure water hydraulic support are solved, achieving higher corrosion resistance and wear resistance. properties, extending equipment life and reducing maintenance costs.
Patent Information
- Application Number
- CN202411024494.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-10-11
AI Technical Summary
The existing anti-corrosion technology cannot effectively resist the corrosion of pure water hydraulic supports, and it is difficult to meet the requirements of high wear resistance and high corrosion resistance in coal mines, especially under high stress and high friction working conditions.
Laser cladding technology and arc surfacing technology are used to treat key parts of the hydraulic support column with stainless steel, combined with nitriding protective treatment to form a protective layer of thickness and uniformity to enhance corrosion resistance and wear resistance.
It significantly improves the corrosion resistance and wear resistance of the hydraulic support column, extends the service life, reduces maintenance costs, and improves the stability and safety of the equipment, making it suitable for complex working conditions.
Smart Images

Figure CN118752184A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of pure water hydraulic supports, specifically to the technical field of pure water hydraulic support anti-corrosion, and in particular to an anti-corrosion method for a pure water hydraulic support column and a pure water hydraulic support column. Background Art
[0002] Hydraulic support is one of the most important production equipment in underground fully mechanized mining working faces. Its emulsion is the working medium of the traditional hydraulic system. Due to the problems of running, bubbling, dripping and leakage in the hydraulic pipeline of the working face, the emulsified oil is integrated into the groundwater, causing serious water pollution and soil oiliness. In order to solve the environmental pollution problem of the emulsion of the hydraulic system of the fully mechanized mining support, the research and development of pure water hydraulic support has become a research hotspot of fully mechanized mining equipment. As an innovative technology in the field of coal mining, pure water hydraulic support has received extensive attention and application for its significant advantages such as green environmental protection, clean and efficient, economical and reliable, and intelligent control. With the in-depth promotion of the transformation and development of the coal industry and the continuous improvement of environmental protection requirements, pure water hydraulic support is expected to be more widely used and promoted in the future.
[0003] In the complex environment of coal mining, hydraulic supports are key equipment to support and ensure the smooth progress of mining operations. Their stability and reliability are directly related to the safe production and economic benefits of coal mines. As the core components of hydraulic supports, columns and jacks are exposed to harsh working environments with dust, high humidity, and acid and alkali components for a long time. These environmental factors have a significant corrosive effect on the materials. Especially when pure water is used as the working medium, although pure water itself has the advantages of low electrolyte and no pollution, its potential corrosion to metal materials cannot be ignored, which further aggravates the corrosion risk of components such as columns and jacks. At present, the anti-corrosion treatment processes for columns and jack piston rods mainly include electroplating, chemical plating, thermal spraying, etc.; however, the above processes all have certain limitations. For example, electroplating technology is widely used in the anti-corrosion treatment of metal surfaces due to its low cost and mature process. However, the waste liquid and waste gas generated during the electroplating process cause serious pollution to the environment, which is contrary to the current concept of green mining and environmentally friendly production. In addition, the uniformity and density of the electroplating layer are difficult to ensure on certain complex structural parts, affecting the durability and reliability of the anti-corrosion effect; the chemical plating method has the advantages of no need for power supply and good coating uniformity, but its anti-corrosion performance is relatively single, and it is difficult to simultaneously meet the dual needs of wear resistance and corrosion resistance under complex and changeable working conditions in coal mines, especially under high stress and high friction working conditions. The wear resistance of the chemical plating layer is often insufficient, resulting in premature failure of the coating; thermal spraying technology can form a thicker coating, but the bonding strength between the coating and the substrate material and the uniformity of the coating are still the key factors restricting its application; defects such as pores and cracks generated during the spraying process will seriously affect the anti-corrosion performance of the coating, especially under the action of pure water medium, these defects may become the starting point of corrosion and accelerate the corrosion process.
[0004] It can be seen that for pure water hydraulic supports, the existing anti-corrosion technology cannot both effectively resist pure water corrosion and meet the requirements of high wear resistance and high corrosion resistance in coal mines. Summary of the invention
[0005] The purpose of the present invention is to provide a pure water hydraulic support column anti-corrosion method and a pure water hydraulic support column to solve the technical problem that the existing anti-corrosion process cannot effectively resist pure water corrosion and meet the requirements of high wear resistance and high corrosion resistance in coal mines.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] A method for anti-corrosion of pure water hydraulic support columns,
[0008] The anti-corrosion method comprises the following steps:
[0009] Laser cladding technology is used to perform stainless steel cladding treatment on the outer wall of the outer cylinder, the stroke section of the inner wall of the outer cylinder and the static sealing surface of the outer cylinder; arc cladding technology is used to perform stainless steel cladding treatment on the bottom of the outer cylinder;
[0010] Laser cladding technology is used to perform stainless steel cladding treatment on the stroke section of the outer wall of the middle cylinder, the stroke section of the inner wall of the middle cylinder and the static sealing surface of the middle cylinder barrel; arc cladding technology is used to perform stainless steel cladding treatment on the piston section at the bottom of the middle cylinder, the inner wall of the bottom of the middle cylinder, the outer wall of the bottom of the middle cylinder and the valve hole at the bottom of the middle cylinder;
[0011] Laser cladding technology is used to perform stainless steel cladding treatment on the stroke section of the piston outer wall; arc cladding technology is used to perform stainless steel cladding treatment on the piston bottom and piston section;
[0012] One end of the liquid passage pipe is welded in the piston, and the other end is sleeved with a plurality of O-rings to form a sealing fit with the piston;
[0013] The entire surfaces of the first guide sleeve and the second guide sleeve are treated with nitriding protection.
[0014] Furthermore, laser cladding technology is used to clad the outer wall of the outer cylinder with TY-2C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm; laser cladding technology is used to clad the stroke section of the inner wall of the outer cylinder and the static sealing surface of the outer cylinder with TY-4C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm.
[0015] Furthermore, arc surfacing technology is used to surfacing 309 austenitic stainless steel on the bottom surface of the outer cylinder, and the thickness of the surfacing layer is ≥1.5mm.
[0016] Furthermore, the pipe seat, liquid pipe and joint block connected to the outer cylinder are all made of 17-4 precipitation hardening martensitic stainless steel.
[0017] Furthermore, laser cladding technology is used to clad the stroke section of the outer wall of the center cylinder with TY-2C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm; laser cladding technology is used to clad the stroke section of the inner wall of the center cylinder and the static sealing surface of the center cylinder barrel with TY-4C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm.
[0018] Furthermore, arc surfacing technology is used to surfacing 17-4 precipitation hardened martensitic stainless steel on the piston section at the bottom of the middle cylinder, the inner wall of the bottom of the middle cylinder, the outer wall of the bottom of the middle cylinder and the surface of the valve hole at the bottom of the middle cylinder, and the thickness of the surfacing layer is ≥1.5mm; wherein, the bottom valve of the middle cylinder is made of stainless steel.
[0019] Furthermore, laser cladding technology is used to clad the stroke section of the outer wall of the plunger with TY-2C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm.
[0020] Furthermore, arc surfacing technology is used to surfacing 17-4 precipitation hardening martensitic stainless steel on the surface of the piston bottom and the piston segment, and the thickness of the surfacing layer is ≥1.5mm.
[0021] Furthermore, the entire surface of the first guide sleeve and the second guide sleeve is treated with nitriding protection, the depth of the nitriding layer is 0.4-0.6 mm, and the hardness of the nitriding layer is HV≥500.
[0022] A pure water hydraulic support column, wherein the pure water hydraulic support column is treated by the above-mentioned anti-corrosion method.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention provides an anti-corrosion method for a pure water hydraulic support column. The method uses laser cladding technology to perform stainless steel cladding treatment on key parts such as the outer cylinder, the middle cylinder and the inner and outer walls of the column and the sealing surface, which not only enhances the hardness and wear resistance of these parts, but also effectively isolates the direct contact of the corrosive medium, thereby greatly delaying the corrosion process; for special areas such as the cylinder bottom and the sealing section, arc cladding technology is used to perform stainless steel cladding treatment, thereby enhancing its corrosion resistance; the liquid pipe is fixed to the column by welding, and is sealed with a plurality of O-rings, and the emulsion does not pass through the closed cavity formed by the inner wall of the column and the outer wall of the liquid pipe, so there is no need for anti-corrosion treatment, thereby reducing the pushing, boring and rolling process of the inner wall of the column; the full surface nitriding protection treatment of the guide sleeve further enhances the wear resistance and corrosion resistance of the guide system, thereby ensuring the stable operation of the column; the method uses laser cladding or arc cladding to clad the stainless steel material at the contact part between the column and the medium to improve the corrosion resistance. The use of this anti-corrosion method comprehensively improves the corrosion resistance and overall performance of the pure water hydraulic support column, reduces maintenance costs, and extends service life, which is of great significance for improving production efficiency and safety in working environments such as mines.
[0025] On the other hand, in this method, laser cladding stainless steel technology is applied for the first time to the anti-corrosion treatment of the outer wall of the column. After one treatment, there is no need to sandblast and remove rust on the surface during the subsequent remanufacturing of the column, which increases the life of the column and shortens the remanufacturing process and cycle.
[0026] On the other hand, the anti-corrosion method is highly versatile and can be applied not only to the outer wall of a column, but is also particularly suitable for anti-corrosion treatment of hydraulic cylinders serving in various highly corrosive working environments.
[0027] Preferably, in the present invention, the selection of TY-2C and TY-4C stainless steel powders is optimized for different areas of the outer cylinder, ensuring the corrosion resistance, hardness and wear resistance of the cladding layer, and further enhancing the anti-corrosion performance of the column.
[0028] Preferably, in the present invention, 309 austenitic stainless steel is used for surfacing, which enhances the corrosion resistance of the bottom of the outer cylinder, and can effectively prevent the bottom of the cylinder from rusting, especially in a highly corrosive environment.
[0029] Preferably, in the present invention, the pipe seat, liquid pipe and joint block on the outer cylinder are made of 17-4 precipitation hardened martensitic stainless steel, which improves the strength and corrosion resistance of these components and reduces the risk of leakage or damage caused by material problems.
[0030] Preferably, in the present invention, the laser cladding process related to the middle cylinder also uses TY-2C and TY-4C stainless steel powders, which ensures the corrosion resistance of key parts of the middle cylinder and improves the stability and durability of the overall structure.
[0031] Preferably, in the present invention, the application of 17-4 precipitation hardened martensitic stainless steel further enhances the strength and corrosion resistance of the cylinder bottom and its related components, while the selection of a stainless steel bottom valve also improves the sealing performance and durability.
[0032] Preferably, in the present invention, the cladding treatment of TY-2C stainless steel powder effectively improves the anti-collision and corrosion resistance of the outer wall of the piston, protects the key parts of the piston during movement, and reduces the performance degradation caused by collision or corrosion.
[0033] Preferably, in the present invention, the surfacing treatment of 17-4 precipitation-hardened martensitic stainless steel enhances the wear resistance and corrosion resistance of the piston bottom and the piston section, improves the sealing performance, and ensures the reliability and safety of the column.
[0034] Preferably, in the present invention, the nitriding treatment improves the surface hardness and wear resistance of the guide sleeve, and at the same time enhances its corrosion resistance. After treatment, the depth of the nitriding layer is 0.4 to 0.6 mm, and the hardness of the nitriding layer is HV ≥ 500. In this way, the wear and failure caused by friction and corrosion are reduced, and the service life of the guide sleeve is extended.
[0035] The present invention also provides a pure water hydraulic support column. After being treated with the above-mentioned anti-corrosion method, the overall performance of the column is significantly improved, including corrosion resistance, strength, wear resistance and sealing, thereby improving the service life and reliability of the equipment, reducing maintenance costs, and providing safer and more efficient protection for working environments such as mines. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 A schematic structural diagram of a pure water hydraulic support column provided in an embodiment of the present invention; wherein (a) is a front view, and (b) is a CC sectional view in (a);
[0037] Figure 2A schematic diagram of the structure of an outer cylinder of a pure water hydraulic support column provided in an embodiment of the present invention; wherein (a) is a front view, and (b) is a cross-sectional view taken along the AA line in (a);
[0038] Figure 3 A schematic structural diagram of a middle cylinder of a pure water hydraulic support column provided by an embodiment of the present invention;
[0039] Figure 4 A schematic structural diagram of a live column of a pure water hydraulic support column provided by an embodiment of the present invention;
[0040] Figure 5 A schematic diagram of the structure of the outer wall of the outer cylinder provided in an embodiment of the present invention;
[0041] Figure 6 A schematic diagram of the structure of the inner wall stroke section of the outer cylinder and the static sealing surface of the outer cylinder provided in an embodiment of the present invention;
[0042] Figure 7 A schematic diagram of the structure of the bottom of the outer cylinder provided by an embodiment of the present invention;
[0043] Figure 8 A schematic diagram of the structure of the piston section at the bottom of the middle cylinder provided in an embodiment of the present invention;
[0044] Fig. 9 A schematic diagram of the structure of the outer wall travel section of the middle cylinder provided in an embodiment of the present invention;
[0045] Fig.10 A schematic diagram of the structure of the inner wall travel section of the middle cylinder provided in an embodiment of the present invention;
[0046] Fig.11 A schematic diagram of the structure of the outer wall travel section of the plunger provided in an embodiment of the present invention;
[0047] Fig.12 A schematic diagram of the structure of the plunger bottom and the piston section provided in an embodiment of the present invention;
[0048] Fig.13 A schematic diagram of the structure of a liquid passage pipe provided in an embodiment of the present invention;
[0049] Fig.14 A schematic diagram of the structure of a guide sleeve provided in an embodiment of the present invention;
[0050] Fig.15 A flow chart of an anti-corrosion method for a pure water hydraulic support column provided in an embodiment of the present invention.
[0051] Reference numerals:
[0052] 1-outer cylinder, 2-middle cylinder, 3-live column, 4-first guide sleeve, 5-second guide sleeve, 6-liquid passage; 7-O-type sealing ring;
[0053] 1-1-outer wall of outer cylinder, 1-2-stroke section of inner wall of outer cylinder, 1-3-static sealing surface of outer cylinder, 1-4-bottom of outer cylinder;
[0054] 2-1- piston section at the bottom of the middle cylinder, 2-2- inner wall at the bottom of the middle cylinder, 2-3- outer wall at the bottom of the middle cylinder, 2-4- valve hole at the bottom of the middle cylinder, 2-5- stroke section at the outer wall of the middle cylinder, 2-6- stroke section at the inner wall of the middle cylinder;
[0055] 3-1- piston outer wall travel section, 3-2- piston bottom and piston section. DETAILED DESCRIPTION
[0056] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0057] It should be noted that when an element is referred to as being "disposed on" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only and are not intended to be the only embodiment.
[0058] Example 1
[0059] As mentioned in the background technology, for the anti-corrosion treatment of hydraulic support columns, current conventional processes all have certain limitations, for example: electroplating technology is widely used in the anti-corrosion treatment of metal surfaces due to its low cost and mature process. However, the waste liquid and waste gas generated during the electroplating process cause serious pollution to the environment, which is contrary to the current concept of green mining and environmentally friendly production. In addition, the uniformity and density of the electroplating layer are difficult to guarantee on some complex structural parts, affecting the durability and reliability of the anti-corrosion effect; chemical plating has the advantages of no need for power supply and good uniformity of the coating, but its anti-corrosion performance is relatively single, and it is difficult to simultaneously meet the dual needs of wear resistance and anti-corrosion under complex and changeable working conditions in coal mines, especially under high stress and high friction working conditions, the wear resistance of the chemical plating layer is often insufficient, resulting in premature failure of the coating; thermal spraying technology can form a thicker coating, but the bonding strength of the coating and the base material and the uniformity of the coating are still the key factors restricting its application; defects such as pores and cracks generated during the spraying process will seriously affect the anti-corrosion performance of the coating, especially under the action of pure water medium, these defects may become the starting point of corrosion and accelerate the corrosion process. Therefore, it is particularly important to develop a new anti-corrosion treatment technology that can effectively resist pure water corrosion and meet the high wear resistance and high corrosion resistance requirements of coal mines. The successful development of this anti-corrosion technology will provide a strong guarantee for the long-term reliable operation of pure water hydraulic supports and promote the green, efficient and sustainable development of the coal mining industry.
[0060] First, the structure of the application object in this embodiment, that is, the pure water hydraulic support column, is introduced:
[0061] In this embodiment, the pure water hydraulic support column includes an outer cylinder 1, a middle cylinder 2 and a piston 3; the piston 3 is inserted in the middle cylinder 2, and a second guide sleeve 5 is provided between the piston 3 and the middle cylinder 2; the middle cylinder 2 is inserted in the outer cylinder 1, and a first guide sleeve 4 is provided between the middle cylinder 2 and the outer cylinder 1; a liquid pipe 6 is inserted in the inner cavity of the piston 3;
[0062] like Figures 1 to 4 As shown, specifically Figure 1 (a), (b) and Figure 2 As shown in (a) and (b), the pure water hydraulic support column includes an outer cylinder 1, a middle cylinder 2 and a piston 3; the piston 3 is inserted in the middle cylinder 2, and a second guide sleeve 5 is arranged between the piston 3 and the middle cylinder 2; the middle cylinder 2 is inserted in the outer cylinder 1, and a first guide sleeve 4 is arranged between the middle cylinder 2 and the outer cylinder 1; a liquid pipe 6 is inserted in the inner cavity of the piston 3, and specifically, the first guide sleeve 4 and the second guide sleeve 5 are connected to the corresponding cylinder barrel through rectangular threads.
[0063] like Fig.15 As shown, in order to achieve the above purpose and solve the above problem, the present invention provides a method for anti-corrosion of a pure water hydraulic support column, comprising the following steps:
[0064] S1: The outer wall 1-1 of the outer cylinder, the stroke section 1-2 of the inner wall of the outer cylinder and the static sealing surface 1-3 of the outer cylinder are respectively clad with stainless steel by laser cladding technology; the outer cylinder bottom 1-4 is clad with stainless steel by arc cladding technology.
[0065] S2: The laser cladding technology is used to perform stainless steel cladding treatment on the stroke section 2-5 of the outer wall of the middle cylinder, the stroke section 2-6 of the inner wall of the middle cylinder and the static sealing surface of the middle cylinder barrel; the arc cladding technology is used to perform stainless steel cladding treatment on the piston section 2-1 at the bottom of the middle cylinder, the inner wall 2-2 at the bottom of the middle cylinder, the outer wall 2-3 at the bottom of the middle cylinder and the valve hole 2-4 at the bottom of the middle cylinder.
[0066] S3: The outer wall stroke section 3-1 of the piston is clad with stainless steel using laser cladding technology; the bottom of the piston and the piston section 3-2 are clad with stainless steel using arc cladding technology.
[0067] S4: One end of the liquid passage tube 6 is welded to the piston 3, and the other end is sleeved with a plurality of O-rings 7 to form a sealing fit with the piston 3.
[0068] S5: The entire surfaces of the first guide sleeve 4 and the second guide sleeve 5 are treated with nitriding protection.
[0069] It can be seen that the anti-corrosion method for the pure water hydraulic support column provided in this embodiment and the overall idea of the key anti-corrosion technology of the column are to use austenitic stainless steel for protection only for the parts with high requirements for corrosion resistance, and to use martensitic stainless steel for protection for the parts with requirements for both corrosion resistance and wear resistance, to ensure that all places in contact with the liquid medium are effectively protected.
[0070] Compared with the traditional anti-corrosion process, the anti-corrosion method mentioned in this embodiment has the following characteristics:
[0071] In this embodiment, on the one hand, a layer of stainless steel is clad on the contact parts of the column with the medium by laser cladding or arc welding to improve the corrosion resistance; on the other hand, a stainless steel liquid tube is inserted into the inner cavity of the piston, one end of which is welded and the other end is equipped with an O-ring to prevent the liquid medium from entering the inner cavity of the piston; on the other hand, in this method, the laser cladding stainless steel technology is applied to the anti-corrosion treatment of the outer wall of the column for the first time. After a one-time treatment, there is no need to sandblast and remove rust on the surface when the column is remanufactured subsequently, thereby increasing the life of the column and shortening the remanufacturing process and cycle; on the other hand, the laser cladding stainless steel technology can be applied not only to the outer wall of the column, but also is particularly suitable for the anti-corrosion treatment of hydraulic cylinders serving in various highly corrosive working environments, such as salt mines.
[0072] Example 2
[0073] This embodiment also provides another anti-corrosion method for pure water hydraulic support columns. This method is the same as that of Example 1, and is improved and optimized on the basis of Example 1. The specific steps are as follows:
[0074] (1) The anti-corrosion treatment process of the outer cylinder is as follows:
[0075] like Figure 5 As shown, the outer wall 1-1 of the outer cylinder is clad with TY-2C stainless steel powder by laser cladding technology, and the thickness of the cladding layer is ≥0.5mm.
[0076] like Figure 6 As shown, the outer cylinder inner wall stroke section 1-2 and the outer cylinder static sealing surface 1-3 are clad with TY-4C stainless steel powder by laser cladding technology, and the cladding layer thickness is ≥0.5mm.
[0077] Among them, the accessories such as the pipe seat, liquid pipe and joint block on the outer cylinder are made of 17-4 precipitation-hardened martensitic stainless steel. This improves the strength and corrosion resistance of these components and reduces the risk of leakage or damage caused by material problems.
[0078] like Figure 7 As shown, the inner wall of the outer cylinder bottom 1-4 is welded with 309 austenitic stainless steel by arc welding technology, and the thickness of the welding layer is ≥1.5mm.
[0079] (2) The anti-corrosion treatment process of the middle cylinder is as follows:
[0080] like Fig. 9 As shown, the stroke section 2-5 of the outer wall of the middle cylinder is clad with TY-2C stainless steel powder using laser cladding technology, and the thickness of the cladding layer is ≥0.5mm.
[0081] like Fig.10 As shown, the stroke section 2-6 of the inner wall of the middle cylinder and the static sealing surface of the middle cylinder are clad with TY-4C stainless steel powder using laser cladding technology, and the thickness of the cladding layer is ≥0.5mm.
[0082] like Figure 8 As shown, the piston section 2-1 at the bottom of the middle cylinder adopts arc surfacing technology, and the surface is surfacing-welded with 17-4 precipitation-hardened martensitic stainless steel, and the thickness of the surfacing layer is ≥1.5mm.
[0083] The inner wall 2-2 of the middle cylinder bottom and the outer wall 2-3 of the middle cylinder bottom, the overall outer surface and the surface of the valve hole 2-4 at the middle cylinder bottom are all welded with arc welding technology, and the surface is welded with 17-4 precipitation hardening martensitic stainless steel, and the thickness of the welding layer is ≥1.5mm.
[0084] Among them, the bottom valve inserted in the bottom valve hole 2-4 of the middle cylinder is a bottom valve made of stainless steel.
[0085] (3) The anti-corrosion treatment process of the live column is as follows:
[0086] like Fig.11 As shown, the plunger outer wall travel section 3-1 is clad with TY-2C stainless steel powder using laser cladding technology, and the cladding layer thickness is ≥0.5mm.
[0087] like Fig.12 As shown, the outer surface of the piston bottom and the piston segment 3-2 is clad with 17-4 precipitation hardening martensitic stainless steel by arc cladding technology, and the thickness of the cladding layer is ≥1.5mm.
[0088] like Fig.13 As shown, the inner cavity of the piston 3 is inserted into a liquid tube 6, one end of the liquid tube 6 is welded to the tail of the piston 3, and the other end is inserted into the piston and equipped with two high-temperature resistant O-rings 7 to prevent the medium from entering the inner cavity of the piston.
[0089] (4) The anti-corrosion treatment process of the first guide sleeve 4 and the second guide sleeve 5 is as follows:
[0090] like Figure 4 As shown, the structures of the first guide sleeve 4 and the second guide sleeve 5 are basically the same, but the specifications are different. In this embodiment, the entire surface of the first guide sleeve 4 and the second guide sleeve 5 is subjected to nitriding protection treatment, wherein the nitriding layer is 0.4 to 0.6 mm deep and the nitriding layer hardness HV≥500.
[0091] The present invention also provides a pure water hydraulic support column. After being treated with the above-mentioned anti-corrosion method, the overall performance of the column is significantly improved, including corrosion resistance, strength, wear resistance and sealing, thereby improving the service life and reliability of the equipment, reducing maintenance costs, and providing safer and more efficient protection for working environments such as mines.
[0092] In summary, the present invention provides a pure water hydraulic support column anti-corrosion method and a pure water hydraulic support column, which have the following advantages compared with the existing anti-corrosion treatment process:
[0093] The present invention proposes a method for anti-corrosion of pure water hydraulic support columns. By comprehensively using laser cladding technology and arc surfacing technology, the key parts of the hydraulic support columns are treated with stainless steel, which significantly improves the corrosion resistance and wear resistance of the columns. Specifically, according to the characteristics and working environment of different parts, TY-2C and TY-4C stainless steel powders are used for laser cladding, and 309 austenitic stainless steel and 17-4 precipitation hardening martensitic stainless steel are used for arc surfacing, ensuring that each part can form a protective layer of sufficient thickness and uniformity. In addition, the entire surface of the guide sleeve is nitrided for protection, which further enhances its hardness, wear resistance and corrosion resistance. These measures not only extend the service life of the hydraulic support columns, but also improve their working stability and safety, which is of great significance for the long-term operation of the pure water hydraulic support system under harsh working conditions. Overall, this anti-corrosion method is advanced in technology, meticulous in operation, and has significant effects. It is an effective means to improve the anti-corrosion performance of the pure water hydraulic support columns.
[0094] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0095] The above are only preferred specific implementation modes of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and the disclosed concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0096] The further detailed description made in the disclosure cannot be used to determine that the specific implementation methods of the present invention are limited to these. For ordinary technicians in the technical field to which the present invention belongs, they can make several simple deductions or substitutions without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention determined by the submitted claims.
Claims
1. A method for anti-corrosion of pure water hydraulic support columns, characterized in that: The anti-corrosion method comprises the following steps: Laser cladding technology is used to perform stainless steel cladding treatment on the outer wall (1-1) of the outer cylinder, the stroke section (1-2) of the inner wall of the outer cylinder, and the static sealing surface (1-3) of the outer cylinder barrel; arc cladding technology is used to perform stainless steel cladding treatment on the bottom (1-4) of the outer cylinder; Laser cladding technology is used to perform stainless steel cladding treatment on the stroke section (2-5) of the outer wall of the middle cylinder, the stroke section (2-6) of the inner wall of the middle cylinder, and the static sealing surface of the middle cylinder barrel; arc cladding technology is used to perform stainless steel cladding treatment on the piston section (2-1) at the bottom of the middle cylinder, the inner wall (2-2) at the bottom of the middle cylinder, the outer wall (2-3) at the bottom of the middle cylinder, and the valve hole (2-4) at the bottom of the middle cylinder; The laser cladding technology is used to perform stainless steel cladding treatment on the piston outer wall stroke section (3-1); the arc cladding technology is used to perform stainless steel cladding treatment on the piston bottom and the piston section (3-2); One end of the liquid passage tube (6) is welded to the piston (3), and the other end is sleeved with a plurality of O-rings (7) to form a sealing fit with the piston (3); The entire surfaces of the first guide sleeve (4) and the second guide sleeve (5) are treated with nitriding protection.
2. The anti-corrosion method for a pure water hydraulic support column according to claim 1, characterized in that: The outer wall (1-1) of the outer cylinder is clad with TY-2C stainless steel powder by laser cladding technology, and the thickness of the cladding layer is ≥0.5mm; the inner wall stroke section (1-2) of the outer cylinder and the static sealing surface (1-3) of the outer cylinder are clad with TY-4C stainless steel powder by laser cladding technology, and the thickness of the cladding layer is ≥0.5mm.
3. The anti-corrosion method for a pure water hydraulic support column according to claim 1, characterized in that: The outer cylinder bottom (1-4) is welded with 309 austenitic stainless steel by arc welding technology, and the thickness of the welding layer is ≥1.5mm.
4. A method for anti-corrosion of a pure water hydraulic support column according to any one of claims 1 to 3, characterized in that: The pipe seat, liquid-passing pipe and joint block connected to the outer cylinder (1) are all made of 17-4 precipitation-hardened martensitic stainless steel.
5. The anti-corrosion method for a pure water hydraulic support column according to claim 1, characterized in that: Laser cladding technology is used to clad the stroke section (2-5) of the outer wall of the center cylinder with TY-2C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm; laser cladding technology is used to clad the stroke section (2-6) of the inner wall of the center cylinder and the static sealing surface of the center cylinder with TY-4C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm.
6. The anti-corrosion method for a pure water hydraulic support column according to claim 1, characterized in that: Arc cladding technology is used to clad the piston section (2-1) at the bottom of the middle cylinder, the inner wall (2-2) at the bottom of the middle cylinder, the outer wall (2-3) at the bottom of the middle cylinder, and the valve hole (2-4) at the bottom of the middle cylinder with 17-4 precipitation hardened martensitic stainless steel, and the thickness of the cladding layer is ≥1.5 mm; wherein the bottom valve of the middle cylinder (2) is made of stainless steel.
7. The anti-corrosion method for a pure water hydraulic support column according to claim 1, characterized in that: The laser cladding technology is used to clad the stroke section (3-1) of the outer wall of the plunger with TY-2C stainless steel powder, and the thickness of the cladding layer is ≥0.5mm.
8. The anti-corrosion method for pure water hydraulic support columns according to claim 1, characterized in that: The surface of the piston bottom and the piston section (3-2) is welded with 17-4 precipitation hardening martensitic stainless steel by using arc welding technology, and the thickness of the welding layer is ≥1.5mm.
9. A method for anti-corrosion of a pure water hydraulic support column according to any one of claims 1 to 8, characterized in that: The entire surface of the first guide sleeve (4) and the second guide sleeve (5) are treated with nitriding protection, the depth of the nitriding layer is 0.4-0.6 mm, and the hardness of the nitriding layer is HV≥500.
10. A pure water hydraulic support column, characterized in that: The pure water hydraulic support column is treated by the anti-corrosion method described in any one of claims 1-9.
Citation Information
Patent Citations
Wear resistant piston rod component for hydraulic cylinder
CN105257622A
Reinforcing treatment method for pure water hydraulic cylinder stand column and pure water hydraulic cylinder stand column
CN113118622A
Manufacturing method of full-protection hydraulic support stand column suitable for various media
CN114160776A
Stand column movable column capable of reducing use amount of anti-freezing solution
CN117646641A
Corrosion-resistant and wear-resistant cladding process for whole series of stand columns and jacks of hydraulic support
CN118127504A