Wood size stabilizer as well as preparation method and application thereof

Through the combination of paraffin, polyethylene glycol and dimethyl silicone, it fills the internal pores of the wood and displaces water, solving the problem of moisture absorption in fast-growing forest wood, significantly improving the dimensional stability and water absorption resistance of the wood, and is suitable for process production.

CN118752571APending Publication Date: 2024-10-11TAN CARPENTER HANDICRAFT WANXIAN COUNTY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411141252.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Due to its short growth cycle, poor material quality, easy corrosion, low density, low strength, and easy cracking and deformation, fast-growing forest wood cannot meet the needs of use. In particular, it has moisture absorption problems in terms of dimensional stability, resulting in dimensional changes, which limits its scope of use.

Method used

Paraffin, polyethylene glycol and dimethyl silicone are used as wood dimensional stabilizers. Through heating and vacuum impregnation, the paraffin fills the internal pores of the wood to delay the entry of moisture, and replaces the moisture in the wood with a solubilizing agent to maintain the swelling state of the wood. , thereby improving dimensional stability.

Benefits of technology

It effectively blocks the internal pores of the wood, reduces the entry of moisture, and significantly improves the dimensional stability and water absorption resistance of the wood. At the same time, it uses environmentally friendly materials, is simple to operate, and is suitable for process production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005000864650000071
    Figure BDA0005000864650000071
  • Figure BDA0005000864650000081
    Figure BDA0005000864650000081
Patent Text Reader

Abstract

The invention discloses a wood size stabilizer which comprises the following raw materials in parts by mass: 50-70 parts of paraffin and 10-20 parts of a solubilizer, and the purpose of improving the dimensional stability of the wood is achieved by combining the dual synergistic effect of filling wood gaps and increasing the internal capacity of the wood. The molten paraffin flows into internal pores of the wood in a liquid form, the paraffin is fixed in the wood after being cooled, the effects of blocking part of the internal pores of the wood and delaying and reducing water entering the wood are achieved, the water in the wood is replaced through the compatibilizer, the wood is kept in a swelling state, and therefore the size stability of the wood is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of wood modification, and in particular to a wood dimensional stabilizer, a preparation method and application thereof. Background Art

[0002] Due to the short growth cycle, short rotation cycle, and high proportion of young wood, fast-growing wood in artificial forests inevitably has problems such as poor material quality, easy corrosion, low density, low strength, easy cracking and deformation. It is difficult to meet the use needs in terms of mechanical properties and dimensional stability, which greatly limits the scope of use of fast-growing wood. It is usually used as raw materials for artificial boards such as fiberboard, particleboard, plywood, etc., indirectly used in fields such as home furnishings, or as raw materials for papermaking and building templates. Therefore, the study of the dimensional stability of fast-growing forest wood is very important. Commonly used methods include high-temperature thermal modification, compression densification, chemical modification, impregnation modification, etc. Impregnation modification is to add the modifier to the inside of the wood by using vacuum, pressure and other impregnation methods, so that the modifier is physically adsorbed or filled inside the wood, closing the wood cell cavity or swelling the wood cell wall, increasing the bulk density of the wood, and thus improving the performance of the wood. The Chinese invention patent with publication number CN202011353095.7 discloses an integrated modification process and equipment for wood heat treatment, wax injection, and dewaxing. Through the combined treatment of heat treatment, wax injection, and dewaxing, the dimensional stability, corrosion resistance, and weather resistance of wood can be effectively improved, and the high-value utilization of low-quality wood can be achieved. Wax injection technology is now widely used to improve the dimensional stability of wood, but if wax is used alone, part of the wax will fill the gaps inside the wood during the treatment process, thereby slowing down the moisture absorption of the wood, but the hygroscopic groups inside the wood still exist, and long-term exposure to a humid environment will still slowly absorb moisture, causing dimensional changes.

[0003] Therefore, there is a need for a wood dimensional stabilizer that can fundamentally solve the moisture absorption problem of wood. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a wood dimensional stabilizer, a preparation method and application thereof, so as to fundamentally solve the moisture absorption problem of wood.

[0005] The wood dimensional stabilizer of the present invention comprises the following raw materials by mass: 50-70 parts of paraffin wax and 10-20 parts of a solubilizer;

[0006] Further, the solubilizing agent is polyethylene glycol;

[0007] Further, it also includes an auxiliary penetrant, 20-30 parts by mass of the auxiliary penetrant;

[0008] Further, the auxiliary penetrant is dimethyl silicone oil;

[0009] Furthermore, the raw materials include, by mass: 60 parts of paraffin, 15 parts of solubilizer, and 25 parts of auxiliary penetrant.

[0010] The present invention also discloses a method for preparing a wood dimensional stabilizer, comprising the following steps: slowly heating paraffin until it melts, then adding an auxiliary penetrant and stirring the mixture evenly, adding a solubilizer after heating the mixture and stirring the mixture evenly, and continuing to heat the prepared solution and stirring the mixture;

[0011] Further, after the temperature is raised to 85-95° C., a solubilizing agent is added and stirred evenly, and the prepared solution is further heated to above 100° C. and stirred.

[0012] The present invention also discloses an application of a wood dimensional stabilizer, comprising the following steps: vacuumizing the wood and immersing the wood in the melted wood dimensional stabilizer, and then heating the wood under atmospheric pressure;

[0013] Furthermore, during the treatment, the temperature of the wood dimensional stabilizer is maintained at 100 to 120°C.

[0014] Beneficial effects of the present invention: A wood dimensional stabilizer, a preparation method and its application of the present invention combine the dual synergistic effects of filling wood voids and increasing the internal volume of wood to achieve the purpose of improving the dimensional stability of wood. The melted paraffin flows into the internal pores of the wood in the form of liquid, and after the paraffin is cooled, it fixes inside the wood, thereby blocking part of the internal pores of the wood, delaying and reducing the entry of water into the wood, and replacing the water in the wood through the volume expander, and keeping the wood in a swollen state, thereby maintaining the dimensional stability of the wood; and the auxiliary penetrant has good lubricity and permeability, which helps the reagent to penetrate into the wood. The raw materials of the reagents used are all environmentally friendly materials, non-toxic and harmless, and the preparation process is simple to operate, and can be directly used in process production. DETAILED DESCRIPTION

[0015] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.

[0016] In the examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0017] The wood dimension stabilizer of this embodiment comprises, by mass, 50-70 parts of paraffin wax and 10-20 parts of solubilizer. The melted paraffin wax flows into the internal pores of the wood in the form of liquid, and after cooling, the paraffin wax is fixed inside the wood, thereby blocking part of the internal pores of the wood, delaying and reducing the entry of water into the wood. Then, the water in the wood is replaced by the volume expander, and the wood is kept in a swollen state, thereby maintaining the dimensional stability of the wood. The paraffin wax is one or more combinations of 60# to 80#.

[0018] Preferably, the solubilizer is polyethylene glycol (PEG), and PEG is selected from one or more combinations of PEG-100, PEG-200, PEG-300, PEG-400, PEG-600, PEG-800, and PEG-1000.

[0019] In order to facilitate the penetration of the reagent into the wood, an auxiliary penetrant may be added, 20-30 parts by mass of the auxiliary penetrant. Preferably, the auxiliary penetrant is dimethyl silicone oil, which may be one or more combinations of 350CS, 500CS, and 1000CS of dimethyl silicone oil.

[0020] A preferred embodiment is that the raw materials include, by mass, 60 parts of paraffin wax, 15 parts of solubilizer, and 25 parts of auxiliary penetrant. The wood dimensional stabilizer of this embodiment has the best effect.

[0021] This embodiment also discloses a method for preparing a wood dimensional stabilizer, comprising the following steps: slowly heating paraffin to 80°C to melt, then adding an auxiliary penetrant and stirring evenly, heating the temperature to 85-95°C, adding a solubilizer and stirring evenly, and further heating the prepared solution to above 100°C and stirring;

[0022] The present embodiment also discloses an application of a wood dimensional stabilizer, comprising the following steps: comprising the following steps: vacuumizing the wood to make the vacuum reach above 0.08MPa, and the vacuuming time is 60min. Injecting the melted modifying agent into the closed wood processing tank until the wood is completely submerged, the temperature of the agent in this process is 100-120°C, turning off the vacuum pump, opening the valve connected to the outside, restoring the wood processing tank to atmospheric pressure, turning on the heating system for heating the wood processing tank, keeping the temperature of the modifying agent at 100-120°C, and keeping this process for 24-72h, after the end, pumping the modifying agent back to the liquid storage tank, turning on the vacuum equipment, and under the premise of ensuring that the temperature in the processing tank is 100-120°C, vacuuming the processing tank to above 0.07MPa, and keeping it for 60min, after the excess modifying agent is discharged, turning off the vacuum and heating system, opening the valve connected to the outside, restoring the wood processing tank to atmospheric pressure, and taking out the wood after slowly cooling down to room temperature, completing the processing process.

[0023] Embodiment 1

[0024] The wood dimensional stabilizer of this embodiment includes, by mass, 60 parts of paraffin wax, 10 parts of solubilizer, and 30 parts of dimethyl silicone oil.

[0025] The preparation method comprises the following steps:

[0026] Slowly heat 76# paraffin to 80°C to melt it slowly, add 500CS dimethyl silicone oil, and stir well; heat to 90°C, add PEG1000, and stir well; heat the prepared solution to 100°C, stir well for 2 hours, and obtain the modified reagent (the mass ratio of the above reagents is 6:3:1).

[0027] Embodiment 2

[0028] The raw materials for preparing the modification reagent include 50 parts of 76# paraffin, 30 parts of 500CS dimethyl silicone oil and 20 parts of PEG1000.

[0029] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0030] Embodiment 3

[0031] The raw materials for preparing the modification reagent include 60 parts of 80# paraffin, 30 parts of 500CS dimethyl silicone oil and 10 parts of PEG1000.

[0032] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:3:1).

[0033] Embodiment 4

[0034] The raw materials for preparing the modification reagent include 50 parts of 80# paraffin, 30 parts of 500CS dimethyl silicone oil and 20 parts of PEG1000.

[0035] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0036] Embodiment 6

[0037] The raw materials for preparing the modification reagent include 60 parts of 76# paraffin, 20 parts of 500CS dimethyl silicone oil and 20 parts of PEG1000.

[0038] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:2:2).

[0039] Embodiment 7

[0040] The raw materials for preparing the modification reagent include 50 parts of 80# paraffin, 30 parts of 500CS dimethyl silicone oil and 20 parts of PEG1000.

[0041] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0042] Embodiment 7

[0043] The raw materials for preparing the modification reagent include 50 parts of 80# paraffin, 30 parts of 300CS dimethyl silicone oil and 20 parts of PEG1000.

[0044] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0045] Embodiment 8

[0046] The raw materials for preparing the modification reagent include 50 parts of 80# paraffin, 30 parts of 300CS dimethyl silicone oil and 20 parts of PEG800.

[0047] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0048] Embodiment 9

[0049] The raw materials for preparing the modification reagent include 60 parts of 80# paraffin, 30 parts of 500CS dimethyl silicone oil and 10 parts of PEG800.

[0050] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:3:1).

[0051] Embodiment 10

[0052] The raw materials for preparing the modification reagent include 50 parts of 80# paraffin, 30 parts of 500CS dimethyl silicone oil and 20 parts of PEG600.

[0053] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0054] Embodiment 11

[0055] The raw materials for preparing the modification reagent include 60 parts of 80# paraffin, 30 parts of 500CS dimethyl silicone oil and 10 parts of PEG600.

[0056] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:3:1).

[0057] Embodiment 12

[0058] The raw materials for preparing the modification reagent include 50 parts of 80# paraffin, 30 parts of 500CS dimethyl silicone oil and 20 parts of PEG1000.

[0059] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0060] Embodiment 13

[0061] The raw materials for preparing the modification reagent include 50 parts of 76# paraffin, 30 parts of 300CS dimethyl silicone oil and 20 parts of PEG1000.

[0062] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0063] Embodiment 14

[0064] The raw materials for preparing the modification reagent include 50 parts of 76# paraffin, 30 parts of 500CS dimethyl silicone oil and 20 parts of PEG800.

[0065] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0066] Embodiment 15

[0067] The raw materials for preparing the modification reagent include 50 parts of 76# paraffin, 30 parts of 500CS dimethyl silicone oil and 20 parts of PEG600.

[0068] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 5:3:2).

[0069] Embodiment 16

[0070] The raw materials for preparing the modification reagent include 60 parts of 76# paraffin, 20 parts of 350CS dimethyl silicone oil and 20 parts of PEG800.

[0071] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:2:2).

[0072] Embodiment 17

[0073] The raw materials for preparing the modification reagent include 60 parts of 76# paraffin, 30 parts of 350CS dimethyl silicone oil and 10 parts of PEG800.

[0074] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:3:1).

[0075] Embodiment 18

[0076] The raw materials for preparing the modification reagent include 60 parts of 76# paraffin, 20 parts of 350CS dimethyl silicone oil and 20 parts of PEG600.

[0077] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:2:2).

[0078] Embodiment 19

[0079] The raw materials for preparing the modification reagent include 60 parts of 76# paraffin, 30 parts of 350CS dimethyl silicone oil and 10 parts of PEG600.

[0080] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:3:1).

[0081] Embodiment 20

[0082] The raw materials for preparing the modification reagent include 60 parts of 76# paraffin, 30 parts of 500CS dimethyl silicone oil and 10 parts of PEG800.

[0083] The preparation method of the modified reagent is the same as that of Example 1 (the mass ratio of the above reagents is 6:3:1).

[0084] Comparative Example

[0085] Wood not treated with the treatment agent of the present invention

[0086] The treatment experiments on solid wood were carried out using the treatment agents of Examples 1 to 6.

[0087] 1. Experimental Materials

[0088] Maple, wood size is 1000*150*25 (length*width*thickness) mm, moisture content is less than 8-10%;

[0089] 2. Experimental steps:

[0090] Separate the maple wood of the above specifications with spacers, fix them on the material rack and put them into the closed wood processing tank. Evacuate until the vacuum reaches 0.09MPa or more, and the vacuum time is 60min. Inject the melted modification reagents of Examples 1 to 20 of the present invention into the closed wood processing tank until the wood is completely submerged. The temperature of the reagents in this process is 110°C. Turn off the vacuum pump, open the valve connected to the outside world, restore the wood processing tank to atmospheric pressure, turn on the heating system for heating the wood processing tank, and keep the temperature of the modification reagent at 110°C. This process is maintained for 48h. After the end, the modification reagent is withdrawn to the liquid storage tank, the vacuum equipment is turned on, and under the premise of ensuring that the temperature in the processing tank is 110°C, the vacuum in the processing tank is evacuated to 0.08MPa and maintained for 60min. After the excess modification reagent is discharged, turn off the vacuum and heating system, open the valve connected to the outside world, restore the wood processing tank to atmospheric pressure, and take out the wood after it is slowly cooled to room temperature to complete the processing process.

[0091] The treated maple wood boards were prepared into samples of 20*20*20 mm, and the volume swelling rate of the wood treated in Examples 1 to 6 of the present invention and the comparison sample 1 were tested in accordance with the requirements of GB / T1927.8-2021 Test method for physical and mechanical properties of small defect-free wood specimens Part 8: Determination of swelling.

[0092] According to the above test results, the dimensional stability anti-expansion rate (ASE) is calculated as follows:

[0093]

[0094] In the above formula: V C —Volume expansion rate of untreated material

[0095] V t —Volume expansion rate of treated material

[0096] The water absorption test formula is as follows:

[0097]

[0098] In the above formula: W 1 —Dry mass of the sample

[0099] W 2 —The mass of the sample after water absorption

[0100] The test results are shown in the following table:

[0101] Example ASE% Water absorption % Comparative Example — 87.4 Example 1 46.9 44.6 Example 2 50.9 52.8 Example 3 47.5 43.4 Example 4 50.4 54.7 Example 5 52.8 45.6 Example 6 55.9 51.8 Example 7 44.6 43.4 Example 8 48.1 50.2 Example 9 50.2 49.6 Example 10 53.8 42.6 Embodiment 11 48.7 43.1 Example 12 53.9 46.3 Example 13 54.6 53.6 Embodiment 14 53.3 55.8 Embodiment 15 56.9 54.2 Example 16 51.7 54.9 Embodiment 17 47.5 46.3 Embodiment 18 54.1 45.8 Embodiment 19 51.1 48.6 Embodiment 20 49.7 47.3

[0102] The above test results show that the dimensional stability and water absorption resistance of wood can be significantly improved by treating wood with the modified reagent of the present invention in the above treatment method. In addition, the reagent used in the present invention has good environmental performance, and the reagent can be recycled and reused in the process of treating wood without polluting the environment. The treatment process is simple and easy, and has broad application prospects.

[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A wood dimensional stabilizer, characterized in that: The raw materials include, by weight: 50-70 parts of paraffin wax and 10-20 parts of solubilizer.

2. The wood dimensional stabilizer according to claim 1, characterized in that: The solubilizing agent is polyethylene glycol.

3. The wood dimensional stabilizer according to claim 1, characterized in that: It also includes an auxiliary penetrant, 20-30 parts by mass of the auxiliary penetrant.

4. The wood dimensional stabilizer according to claim 3, characterized in that: The auxiliary penetrating agent is dimethyl silicone oil.

5. The wood dimensional stabilizer according to claim 3, characterized in that: The raw materials include, by mass: 60 parts of paraffin, 15 parts of solubilizer, and 25 parts of auxiliary penetrant.

6. The method for preparing a wood dimensional stabilizer according to claim 3, characterized in that: The following steps are involved: Slowly heat the paraffin until it melts, then add the auxiliary penetration agent and stir thoroughly, add the solubilizer after heating and stir thoroughly, and continue to heat and stir the prepared solution.

7. The method for preparing a wood dimensional stabilizer according to claim 6, characterized in that: After heating to 85-95°C, add a solubilizing agent and stir evenly, and continue to heat the prepared solution to above 100°C and stir.

8. The use of the wood dimensional stabilizer according to claim 1, characterized in that: The following steps are involved: The wood is evacuated and immersed in melted wood dimensional stabilizer, then heated at atmospheric pressure.

9. The use of the wood dimensional stabilizer according to claim 8, characterized in that: During the treatment process, the temperature of the wood dimensional stabilizer is maintained at 100-120°C.

Citation Information

Patent Citations

  • Method for treating birch bark

    CN104942939A

  • High-efficiency osmotic organosilicon waterproofing agent of timber and preparation method thereof

    CN105293992A

  • Compound mildew-proof treatment agent for wood crafts and preparation method thereof

    CN105563585A

  • Modifying agent for wood and bamboos

    CN105619561A