Flame-retardant chlorinated polyethylene waterproof coiled material and preparation method thereof

By adding lignin, paraffin, carbon black, barium stearate and flame retardants to the chlorinated polyethylene waterproofing membrane, and using vulcanizing agents and kaolin modifiers to synergistically optimize the coupling of nano-silica agents, the problem was solved The problem of difficulty in coordinating flame retardancy and mechanical properties in the existing technology has significantly improved the waterproof and heat-resistant stability of the product.

CN118852802AInactive Publication Date: 2024-10-29BEIJING EONZEAL WATERPROOF MATERIAL CO LTD

Patent Information

Application Number
CN202410808672.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

After adding flame retardants to existing chlorinated polyethylene waterproofing membranes, it is difficult to coordinate the flame retardant performance and mechanical properties, and the waterproof stability is poor, which affects the efficiency of the product.

Method used

It uses chlorinated polyethylene as the base material, adds lignin, paraffin, carbon black, barium stearate and flame retardants, and performs process vulcanization treatment through vulcanizing agents, combined with kaolin-modified conditioning agents and coupling nanoparticles. Silica agent coordinates and synergizes to optimize the flame retardant and mechanical properties of the product.

Benefits of technology

It achieves the coordinated improvement of the flame retardant and mechanical properties of the flame-retardant chlorinated polyethylene waterproofing membrane, and significantly improves the waterproof and heat-resistant stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of waterproof coiled materials, and particularly discloses a flame-retardant chlorinated polyethylene waterproof coiled material which comprises the following raw materials in parts by weight: 45-50 parts of chlorinated polyethylene, 8-12 parts of lignin, 6-9 parts of a flame retardant, 5-7 parts of paraffin, 3-5 parts of carbon black, 3-5 parts of barium stearate and 2-4 parts of a vulcanizing agent. According to the chlorinated polyethylene waterproof coiled material, chlorinated polyethylene is adopted as a base material, lignin, paraffin, carbon black and barium stearate are added to serve as functional auxiliaries, the flame retardant is added to optimize the flame retardance of a product, and meanwhile technological vulcanization mixing treatment is conducted through the vulcanizing agent; according to the flame-retardant and heat-resistant composite material disclosed by the invention, the flame-retardant and heat-resistant composite material, and the matched kaolin modification-based regulating agent and the coupled nano silicon dioxide agent are mutually coordinated and synergistically cooperated, so that the obtained product has the advantages of coordinated improvement of flame retardance and mechanical properties, and remarkable waterproof and heat-resistant stability effects of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyethylene waterproof coiled material, and in particular to a flame-retardant chlorinated polyethylene waterproof coiled material and a preparation method thereof. Background Art

[0002] Waterproofing roll refers to a waterproofing material product made by impregnating asphalt or polymer waterproofing materials on the base. It is provided in the form of a roll and is called waterproofing roll. Waterproofing roll is mainly used in building walls, roofs, tunnels, roads, landfills, etc. It is a kind of flexible building material product that can be rolled into a roll to prevent external rainwater and groundwater leakage.

[0003] In order to improve the flame retardant properties of existing chlorinated polyethylene waterproof membranes, inorganic flame retardant raw materials are added. The addition of flame retardants easily leads to agglomeration of the raw materials, which in turn affects the mechanical properties of the product, making it difficult to achieve coordinated improvements in the flame retardancy and mechanical properties of the product. The product also has poor waterproof stability, further limiting the use efficiency of the product. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a flame retardant chlorinated polyethylene waterproof membrane and a preparation method thereof, so as to solve the problems raised in the above background technology.

[0005] The present invention solves the technical problem by adopting the following technical solution: The present invention provides a flame-retardant chlorinated polyethylene waterproofing coiled material, comprising the following raw materials in parts by weight: 45-50 parts of chlorinated polyethylene, 8-12 parts of lignin, 6-9 parts of flame retardant, 5-7 parts of paraffin, 3-5 parts of carbon black, 3-5 parts of barium stearate, and 2-4 parts of vulcanizing agent.

[0006] Preferably, the waterproof coiled material comprises the following raw materials in parts by weight: 47.5 parts of chlorinated polyethylene, 10 parts of lignin, 7.5 parts of flame retardant, 6 parts of paraffin, 4 parts of carbon black, 4 parts of barium stearate, and 3 parts of vulcanizing agent.

[0007] Preferably, the Mooney viscosity of the chlorinated polyethylene is 85±5; the flame retardant is magnesium hydroxide; and the vulcanizing agent is dicumyl peroxide DCP.

[0008] Preferably, the waterproofing membrane further comprises 5 to 8 parts of a kaolin-modified conditioning agent and 2 to 5 parts of a coupled nano-silica agent; The preparation method of the conditioning agent based on kaolin modification is: S01: Preparation of modified kaolin: S11: calcining kaolin at 125-135°C for 5-10 min, then cooling naturally to 55°C and keeping warm; S12: adding 2-3 parts of stearic acid and 1-3 parts of urea to 4-7 parts of 10% by mass sodium lignin sulfonate solution and mixing them evenly to obtain a modified solution; adding 3-6 parts of heat-calcined kaolin to the modified solution and shaking the solution for modification treatment, filtering and drying after shaking to obtain modified kaolin; S02: The modified kaolin and chitosan conditioning liquid are uniformly mixed in a weight ratio of 2:5 to obtain a chitosan-conditioned kaolin agent; The preparation method of chitosan conditioning solution is as follows: Fully mix 2-5 parts of 5-7% chitosan solution, 1-2 parts of 4% yttrium nitrate solution and 2-3 parts of sodium dodecylbenzene sulfonate to obtain a chitosan conditioning solution; S03: Chitosan-modified kaolin agent and lanthanum oxide treatment agent are mixed and ball-milled in a weight ratio of 5:(2~3) at a ball-milling speed of 1000~1500r / min for 1~2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin-modified modifier.

[0009] Preferably, the oscillation power of the oscillation modification treatment in S12 is 350-400 W, and the oscillation time is 20-30 min.

[0010] Preferably, the preparation method of the lanthanum oxide treating agent is: The lanthanum oxide powder is calcined at 150-170°C for 10-15 minutes, then heated to 310-330°C at a rate of 2-5°C / min, kept warm for 5-10 minutes, then heated to 420°C at a rate of 1-3°C / min, kept warm for 2-5 minutes, and finally air-cooled to room temperature to obtain a lanthanum oxide treating agent.

[0011] Preferably, the preparation method of the coupled nano-silica agent is: S101: adding 1-2 parts of silane coupling agent KH560 to 4-7 parts of alcohol solution, and then adding 1-3 parts of sodium alginate solution and 3-5 parts of nano-silicon dioxide to mix well to obtain a coupling modified solution; S102: placing the glass fiber in a potassium permanganate solution of 3 to 5 times the total amount of the glass fiber for reaction treatment, washing with water and drying after the treatment, blending 1 to 3 parts of the dried glass fiber, 1 to 2 parts of tetrabutyl titanate and 4 to 7 parts of the coupling modification liquid for ultrasonic treatment, washing with water and drying after the treatment, to obtain a coupled nano-silica agent.

[0012] Preferably, the alcohol solution is prepared by mixing ethanol and water in a weight ratio of 10:1; the mass fraction of the sodium alginate solution is 10-15%; and the mass concentration of the potassium permanganate solution is 1-2 mol / L.

[0013] Preferably, the reaction temperature of the S102 reaction treatment is 52-55°C, the reaction speed is 450-500r / min, and the reaction time is 35-45min; the ultrasonic power of the blending ultrasonic treatment is 350-400W, and the ultrasonic time is 20-30min.

[0014] The present invention also provides a method for preparing a flame-retardant chlorinated polyethylene waterproofing coiled material, comprising the following steps: Chlorinated polyethylene, lignin, flame retardant, paraffin, carbon black, barium stearate, a conditioning agent based on kaolin modification, a coupled nano-silica agent and a vulcanizing agent are uniformly mixed; Then, the mixture was kneaded at 75°C for 5 minutes, and then kneaded at 120°C for 2 minutes. The kneading was completed to obtain a mixed material. The mixed material is calendered and formed, and finally compounded with the non-woven fabric to form the flame-retardant chlorinated polyethylene waterproof coiled material of the present invention; wherein the calendering pressure is 15 MPa and the calendering temperature is 135°C.

[0015] Compared with the prior art, the present invention has the following beneficial effects: The chlorinated polyethylene waterproofing coiled material of the present invention adopts chlorinated polyethylene as a base material, adds lignin, paraffin, carbon black and barium stearate as functional additives, and then adds a flame retardant to optimize the flame retardancy of the product, and at the same time, performs process vulcanization and mixing treatment by a vulcanizing agent, and the coordinated kaolin-modified regulating agent and coupled nano-silica agent are coordinated with each other and work together to coordinate and synergize, so that the obtained product has coordinated improvement of flame retardancy and mechanical properties, and the product has remarkable waterproof and heat-resistant stability effects; In the preparation of the regulating effect agent based on kaolin modification, kaolin is used as the base material, and its activity is optimized by heat calcination at 125~135℃ for 5~10min, and then it is oscillated and modified with a modifying liquid prepared with stearic acid, urea and sodium lignin sulfonate solution. The raw materials in the modifying liquid cooperate with each other to enhance the activity and interface of kaolin, thereby optimizing the coordinated harmonization effect of kaolin and chitosan regulating effect liquid. The chitosan solution, yttrium nitrate solution and sodium dodecylbenzene sulfonate in the chitosan regulating effect liquid cooperate with each other and enhance each other, and then coordinate with the modified kaolin to form a chitosan-regulated kaolin agent, thereby establishing a kaolin-chitosan system, which can The lanthanum oxide treatment agent is optimized to enhance the synergistic effect of kaolin in the system. The lanthanum oxide treatment agent is calcined at 150-170°C for 10-15 minutes, then heated to 310-330°C at a rate of 2-5°C / min, kept warm for 5-10 minutes, and then heated to 420°C at a rate of 1-3°C / min, and kept warm for 2-5 minutes. The activity of lanthanum oxide is optimized by continuous heating. The lanthanum oxide treatment agent is used to coordinate with the kaolin-chitosan system, and the obtained kaolin-modified regulating agent is used in the product to optimize the mechanical properties and flame retardancy of the product, and optimize the waterproof and heat-resistant stability of the product. The coupled nano-silica agent adopts a coupling modified liquid formed by blending silane coupling agent KH560, alcohol solution, sodium alginate solution and nano-silica, with nano-silica as the interface structure, matched with silane coupling agent KH560 and sodium alginate solution, so that it can better cooperate and synergize with glass fiber and tetrabutyl titanate, enhance the coordination effect of glass fiber and nano-silica, thereby enhancing the interface of the system in the system, and filling and reinforcing the system structure, the synergistic effect of the coupled nano-silica agent and the regulating agent based on kaolin modification is further enhanced, so that the performance of the product is further improved. DETAILED DESCRIPTION

[0016] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0017] A flame-retardant chlorinated polyethylene waterproofing coiled material of this embodiment includes the following raw materials in parts by weight: 45-50 parts of chlorinated polyethylene, 8-12 parts of lignin, 6-9 parts of flame retardant, 5-7 parts of paraffin, 3-5 parts of carbon black, 3-5 parts of barium stearate, and 2-4 parts of vulcanizing agent.

[0018] The waterproof coiled material of this embodiment includes the following raw materials in parts by weight: 47.5 parts of chlorinated polyethylene, 10 parts of lignin, 7.5 parts of flame retardant, 6 parts of paraffin, 4 parts of carbon black, 4 parts of barium stearate, and 3 parts of vulcanizing agent.

[0019] The Mooney viscosity of the chlorinated polyethylene of this embodiment is 85±5; the flame retardant is magnesium hydroxide; and the vulcanizing agent is dicumyl peroxide DCP.

[0020] The waterproofing membrane of this embodiment also includes 5 to 8 parts of a conditioning agent based on kaolin modification and 2 to 5 parts of a coupled nano-silica agent; The preparation method of the conditioning agent based on kaolin modification is: S01: Preparation of modified kaolin: S11: calcining kaolin at 125-135°C for 5-10 min, then cooling naturally to 55°C and keeping warm; S12: adding 2-3 parts of stearic acid and 1-3 parts of urea to 4-7 parts of 10% by mass sodium lignin sulfonate solution and mixing them evenly to obtain a modified solution; adding 3-6 parts of heat-calcined kaolin to the modified solution and shaking the solution for modification treatment, filtering and drying after shaking to obtain modified kaolin; S02: The modified kaolin and chitosan conditioning liquid are uniformly mixed in a weight ratio of 2:5 to obtain a chitosan-conditioned kaolin agent; The preparation method of chitosan conditioning solution is as follows: Fully mix 2-5 parts of 5-7% chitosan solution, 1-2 parts of 4% yttrium nitrate solution and 2-3 parts of sodium dodecylbenzene sulfonate to obtain a chitosan conditioning solution; S03: Chitosan-modified kaolin agent and lanthanum oxide treatment agent are mixed and ball-milled in a weight ratio of 5:(2~3) at a ball-milling speed of 1000~1500r / min for 1~2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin-modified modifier.

[0021] In S12 of this embodiment, the oscillation power of the oscillation modification treatment is 350-400 W, and the oscillation time is 20-30 min.

[0022] The preparation method of the lanthanum oxide treating agent of this embodiment is: The lanthanum oxide powder is calcined at 150-170°C for 10-15 minutes, then heated to 310-330°C at a rate of 2-5°C / min, kept warm for 5-10 minutes, then heated to 420°C at a rate of 1-3°C / min, kept warm for 2-5 minutes, and finally air-cooled to room temperature to obtain a lanthanum oxide treating agent.

[0023] The preparation method of the coupled nano-silica agent of this embodiment is: S101: adding 1-2 parts of silane coupling agent KH560 to 4-7 parts of alcohol solution, and then adding 1-3 parts of sodium alginate solution and 3-5 parts of nano-silicon dioxide to mix well to obtain a coupling modified solution; S102: placing the glass fiber in a potassium permanganate solution of 3 to 5 times the total amount of the glass fiber for reaction treatment, washing with water and drying after the treatment, blending 1 to 3 parts of the dried glass fiber, 1 to 2 parts of tetrabutyl titanate and 4 to 7 parts of the coupling modification liquid for ultrasonic treatment, washing with water and drying after the treatment, to obtain a coupled nano-silica agent.

[0024] The alcohol solution of this embodiment is prepared by mixing ethanol and water in a weight ratio of 10:1; the mass fraction of the sodium alginate solution is 10-15%; and the mass concentration of the potassium permanganate solution is 1-2 mol / L.

[0025] The reaction temperature of the S102 reaction treatment in this embodiment is 52-55° C., the reaction speed is 450-500 r / min, and the reaction time is 35-45 min; the ultrasonic power of the blending ultrasonic treatment is 350-400 W, and the ultrasonic time is 20-30 min.

[0026] A method for preparing a flame-retardant chlorinated polyethylene waterproofing coiled material in this embodiment comprises the following steps: Chlorinated polyethylene, lignin, flame retardant, paraffin, carbon black, barium stearate, a conditioning agent based on kaolin modification, a coupled nano-silica agent and a vulcanizing agent are uniformly mixed; Then, the mixture was kneaded at 75°C for 5 minutes, and then kneaded at 120°C for 2 minutes. The kneading was completed to obtain a mixed material. The mixed material is calendered and formed, and finally compounded with non-woven fabric to form the flame-retardant chlorinated polyethylene waterproof coiled material of the present invention; wherein the calendering pressure is 15 MPa and the calendering temperature is 135°C.

[0027] Example 1. A flame-retardant chlorinated polyethylene waterproofing coiled material of this embodiment includes the following raw materials in parts by weight: 45 parts of chlorinated polyethylene, 8 parts of lignin, 6 parts of flame retardant, 5 parts of paraffin, 3 parts of carbon black, 3 parts of barium stearate, and 2 parts of vulcanizing agent.

[0028] The Mooney viscosity of the chlorinated polyethylene of this embodiment is 85±5; the flame retardant is magnesium hydroxide; and the vulcanizing agent is dicumyl peroxide DCP.

[0029] The waterproofing membrane of this embodiment also includes 5 parts of a conditioning agent based on kaolin modification and 2 parts of a coupled nano-silica agent; The preparation method of the conditioning agent based on kaolin modification is: S01: Preparation of modified kaolin: S11: calcining kaolin at 125°C for 5 min, then cooling naturally to 55°C and keeping warm; S12: adding 2 parts of stearic acid and 1 part of urea to 4 parts of 10% by mass sodium lignin sulfonate solution and mixing them evenly to obtain a modified solution; adding 3 parts of heat-calcined kaolin to the modified solution and performing oscillation modification treatment, filtering and drying after the oscillation is completed to obtain modified kaolin; S02: The modified kaolin and chitosan conditioning liquid are uniformly mixed in a weight ratio of 2:5 to obtain a chitosan-conditioned kaolin agent; The preparation method of chitosan conditioning solution is as follows: Fully mix 2 parts of 5% by mass chitosan solution, 1 part of 4% by mass yttrium nitrate solution and 2 parts of sodium dodecylbenzene sulfonate to obtain a chitosan conditioning solution; S03: The chitosan-modified kaolin agent and lanthanum oxide treatment agent are mixed and ball-milled in a weight ratio of 5:2. The ball-milling speed is 1000r / min and the ball-milling is performed for 1h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin-modified modifier.

[0030] The oscillation power of the oscillation modification treatment in S12 of this embodiment is 350 W, and the oscillation time is 20 min.

[0031] The preparation method of the lanthanum oxide treating agent of this embodiment is: The lanthanum oxide powder was calcined at 150°C for 10 min, then heated to 310°C at a rate of 2°C / min, kept warm for 5 min, then heated to 420°C at a rate of 1°C / min, kept warm for 2 min, and finally air-cooled to room temperature to obtain a lanthanum oxide treating agent.

[0032] The preparation method of the coupled nano-silica agent of this embodiment is: S101: adding 1 part of silane coupling agent KH560 to 4 parts of alcohol solution, and then adding 1 part of sodium alginate solution and 3 parts of nano-silicon dioxide to mix well to obtain a coupling modified solution; S102: placing the glass fiber in a potassium permanganate solution of 3 times the total amount of the glass fiber for reaction treatment, washing with water and drying after the treatment, blending 1 part of the dry glass fiber, 1 part of tetrabutyl titanate and 4 parts of the coupling modification liquid for ultrasonic treatment, washing with water and drying after the treatment, to obtain a coupled nano-silica agent.

[0033] The alcohol solution of this embodiment is prepared by mixing ethanol and water in a weight ratio of 10:1; the mass fraction of the sodium alginate solution is 10%; and the mass concentration of the potassium permanganate solution is 1 mol / L.

[0034] The reaction temperature of the S102 reaction treatment in this embodiment is 52° C., the reaction speed is 450 r / min, and the reaction time is 35 min; the ultrasonic power of the blending ultrasonic treatment is 350 W, and the ultrasonic time is 20 min.

[0035] A method for preparing a flame-retardant chlorinated polyethylene waterproofing coiled material in this embodiment comprises the following steps: Chlorinated polyethylene, lignin, flame retardant, paraffin, carbon black, barium stearate, a conditioning agent based on kaolin modification, a coupled nano-silica agent and a vulcanizing agent are uniformly mixed; Then, the mixture was kneaded at 75°C for 5 minutes, and then kneaded at 120°C for 2 minutes. The kneading was completed to obtain a mixed material. The mixed material is calendered and formed, and finally compounded with the non-woven fabric to form the flame-retardant chlorinated polyethylene waterproof coiled material of the present invention; wherein the calendering pressure is 15 MPa and the calendering temperature is 135°C.

[0036] Example 2. A flame-retardant chlorinated polyethylene waterproofing coiled material of this embodiment includes the following raw materials in parts by weight: 50 parts of chlorinated polyethylene, 12 parts of lignin, 9 parts of flame retardant, 7 parts of paraffin, 5 parts of carbon black, 5 parts of barium stearate, and 4 parts of vulcanizing agent.

[0037] The Mooney viscosity of the chlorinated polyethylene of this embodiment is 85±5; the flame retardant is magnesium hydroxide; and the vulcanizing agent is dicumyl peroxide DCP.

[0038] The waterproofing membrane of this embodiment also includes 8 parts of a conditioning agent based on kaolin modification and 5 parts of a coupled nano-silica agent; The preparation method of the conditioning agent based on kaolin modification is: S01: Preparation of modified kaolin: S11: calcining kaolin at 135°C for 10 min, then cooling naturally to 55°C and keeping warm; S12: adding 3 parts of stearic acid and 3 parts of urea to 7 parts of 10% by mass sodium lignin sulfonate solution and mixing them evenly to obtain a modified solution; adding 6 parts of heat-calcined kaolin to the modified solution and shaking the solution for modification treatment, filtering and drying after the shaking is completed to obtain modified kaolin; S02: The modified kaolin and chitosan conditioning liquid are uniformly mixed in a weight ratio of 2:5 to obtain a chitosan-conditioned kaolin agent; The preparation method of chitosan conditioning solution is as follows: Fully mix 5 parts of 7% chitosan solution, 2 parts of 4% yttrium nitrate solution and 3 parts of sodium dodecylbenzene sulfonate to obtain a chitosan conditioning solution; S03: Chitosan-modified kaolin agent and lanthanum oxide treatment agent are mixed and ball-milled in a weight ratio of 5:3. The ball-milling speed is 1500r / min and the ball-milling is carried out for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin-modified conditioning agent.

[0039] In S12 of this embodiment, the oscillation power of the oscillation modification treatment is 400 W, and the oscillation time is 30 min.

[0040] The preparation method of the lanthanum oxide treating agent of this embodiment is: The lanthanum oxide powder was calcined at 170°C for 15 minutes, then heated to 330°C at a rate of 5°C / min, kept warm for 10 minutes, then heated to 420°C at a rate of 3°C / min, kept warm for 5 minutes, and finally air-cooled to room temperature to obtain a lanthanum oxide treating agent.

[0041] The preparation method of the coupled nano-silica agent of this embodiment is: S101: adding 2 parts of silane coupling agent KH560 to 7 parts of alcohol solution, and then adding 3 parts of sodium alginate solution and 5 parts of nano-silicon dioxide to mix well to obtain a coupling modified solution; S102: placing the glass fiber in a potassium permanganate solution of 5 times the total amount of the glass fiber for reaction treatment, washing with water and drying after the treatment, blending 3 parts of the dried glass fiber, 2 parts of tetrabutyl titanate and 7 parts of the coupling modification liquid for ultrasonic treatment, washing with water and drying after the treatment, to obtain a coupled nano-silica agent.

[0042] The alcohol solution of this embodiment is prepared by mixing ethanol and water in a weight ratio of 10:1; the mass fraction of the sodium alginate solution is 15%; and the mass concentration of the potassium permanganate solution is 2 mol / L.

[0043] The reaction temperature of the S102 reaction treatment in this embodiment is 55° C., the reaction speed is 500 r / min, and the reaction time is 45 min; the ultrasonic power of the blending ultrasonic treatment is 400 W, and the ultrasonic time is 30 min.

[0044] A method for preparing a flame-retardant chlorinated polyethylene waterproofing coiled material in this embodiment comprises the following steps: Chlorinated polyethylene, lignin, flame retardant, paraffin, carbon black, barium stearate, a conditioning agent based on kaolin modification, a coupled nano-silica agent and a vulcanizing agent are uniformly mixed; Then, the mixture was kneaded at 75°C for 5 minutes, and then kneaded at 120°C for 2 minutes. The kneading was completed to obtain a mixed material. The mixed material is calendered and formed, and finally compounded with non-woven fabric to form the flame-retardant chlorinated polyethylene waterproof coiled material of the present invention; wherein the calendering pressure is 15 MPa and the calendering temperature is 135°C.

[0045] Example 3. A flame-retardant chlorinated polyethylene waterproofing coiled material of this embodiment includes the following raw materials in parts by weight: 47.5 parts of chlorinated polyethylene, 10 parts of lignin, 7.5 parts of flame retardant, 6 parts of paraffin, 4 parts of carbon black, 4 parts of barium stearate, and 3 parts of vulcanizing agent.

[0046] The Mooney viscosity of the chlorinated polyethylene of this embodiment is 85±5; the flame retardant is magnesium hydroxide; and the vulcanizing agent is dicumyl peroxide DCP.

[0047] The waterproofing membrane of this embodiment also includes 6.5 parts of a conditioning agent based on kaolin modification and 3.5 parts of a coupled nano-silica agent; The preparation method of the conditioning agent based on kaolin modification is: S01: Preparation of modified kaolin: S11: calcining kaolin at 130°C for 7.5 min, then cooling naturally to 55°C and keeping warm; S12: adding 2.5 parts of stearic acid and 2 parts of urea to 5.5 parts of 10% sodium lignin sulfonate solution and mixing them evenly to obtain a modified solution; adding 4.5 parts of heat-calcined kaolin to the modified solution and shaking the solution for modification treatment, filtering and drying after shaking to obtain modified kaolin; S02: The modified kaolin and chitosan conditioning liquid are uniformly mixed in a weight ratio of 2:5 to obtain a chitosan-conditioned kaolin agent; The preparation method of chitosan conditioning solution is as follows: 3.5 parts of 6% by mass chitosan solution, 1.5 parts of 4% by mass yttrium nitrate solution and 2.5 parts of sodium dodecylbenzene sulfonate were mixed thoroughly to obtain a chitosan conditioning solution; S03: The chitosan-modified kaolin agent and lanthanum oxide treatment agent are mixed and ball-milled in a weight ratio of 5:3. The ball-milling speed is 1250r / min and the ball-milling is performed for 1.5h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin-modified modifier.

[0048] The oscillation power of the oscillation modification treatment in S12 of this embodiment is 370 W, and the oscillation time is 25 min.

[0049] The preparation method of the lanthanum oxide treating agent of this embodiment is: The lanthanum oxide powder was calcined at 160°C for 12.5 min, then heated to 320°C at a rate of 3.5°C / min, kept warm for 7.5 min, then heated to 420°C at a rate of 2°C / min, kept warm for 3.5 min, and finally air-cooled to room temperature to obtain a lanthanum oxide treating agent.

[0050] The preparation method of the coupled nano-silica agent of this embodiment is: S101: adding 1.5 parts of silane coupling agent KH560 to 5.5 parts of alcohol solution, and then adding 2 parts of sodium alginate solution and 4 parts of nano-silicon dioxide to mix well to obtain a coupling modified solution; S102: placing the glass fiber in a potassium permanganate solution of 4 times the total amount of the glass fiber for reaction treatment, washing with water and drying after the treatment, blending 2 parts of the dried glass fiber, 1.5 parts of tetrabutyl titanate and 5.5 parts of the coupling modification liquid for ultrasonic treatment, washing with water and drying after the treatment, to obtain a coupled nano-silica agent.

[0051] The alcohol solution of this embodiment is prepared by mixing ethanol and water in a weight ratio of 10:1; the mass fraction of the sodium alginate solution is 12.5%; and the mass concentration of the potassium permanganate solution is 1.5 mol / L.

[0052] The reaction temperature of the S102 reaction treatment in this embodiment is 53° C., the reaction speed is 470 r / min, and the reaction time is 40 min; the ultrasonic power of the blending ultrasonic treatment is 375 W, and the ultrasonic time is 25 min.

[0053] A method for preparing a flame-retardant chlorinated polyethylene waterproofing coiled material in this embodiment comprises the following steps: Chlorinated polyethylene, lignin, flame retardant, paraffin, carbon black, barium stearate, a conditioning agent based on kaolin modification, a coupled nano-silica agent and a vulcanizing agent are uniformly mixed; Then, the mixture was kneaded at 75°C for 5 minutes, and then kneaded at 120°C for 2 minutes. The kneading was completed to obtain a mixed material. The mixed material is calendered and formed, and finally compounded with the non-woven fabric to form the flame-retardant chlorinated polyethylene waterproof coiled material of the present invention; wherein the calendering pressure is 15 MPa and the calendering temperature is 135°C.

[0054] Comparative Example 1. The difference from Example 3 is that no conditioning agent based on kaolin modification is added.

[0055] Comparative Example 2. The difference from Example 3 is that in the preparation of the conditioning agent based on modified kaolin, modified kaolin is replaced by kaolin.

[0056] Comparative Example 3. The difference from Example 3 is that no modifying liquid treatment is used in the preparation of the modified kaolin.

[0057] Comparative Example 4. The difference from Example 3 is that stearic acid and urea are not added to the modified liquid.

[0058] Comparative Example 5. The difference from Example 3 is that no lanthanum oxide treating agent is added in the preparation of the conditioning agent based on kaolin modification.

[0059] Comparative Example 6. The difference from Example 3 is that the lanthanum oxide treating agent was not prepared by heating to 320° C. at a rate of 3.5° C. / min and keeping the temperature for 7.5 min.

[0060] Comparative Example 7. The difference from Example 3 is that the chitosan conditioning liquid is replaced by a chitosan solution with a mass fraction of 6%.

[0061] Comparative Example 8. The difference from Example 3 is that no coupled nano-silica agent is added.

[0062] The products of Examples 1 to 3 and Comparative Examples 1 to 8 were subjected to conventional performance tests, and the test results are as follows

[0063] Wash the product 50 times to test its washing resistance stability;

[0064] It can be seen from Comparative Examples 1-8 and Examples 1-3 that; The product of Example 3 has excellent tensile strength and elongation at break, and the product has significant aging resistance stability effect, and the flame retardancy, aging resistance tensile strength and elongation at break can achieve coordinated improvement, and the product has significant performance stability effect under water washing conditions, and the product has significant water washing resistance stability effect; The product does not contain kaolin-modified conditioning agents or coupled nano-silica agents. The product's water-washing stability, aging-resistant mechanical properties, and flame retardancy all show a significant deterioration trend. The synergistic effect of the two agents is the most significant. In the preparation of the kaolin-modified regulating effect agent, the modified kaolin is replaced by kaolin, the modified kaolin is not treated with modifying liquid, stearic acid and urea are not added to the modifying liquid, the lanthanum oxide treating agent is not added in the preparation of the kaolin-modified regulating effect agent, the lanthanum oxide treating agent is not heated to 320°C at a rate of 3.5°C / min and kept warm for 7.5 minutes in the preparation of the lanthanum oxide treating agent, and the chitosan regulating effect liquid is replaced by a chitosan solution with a mass fraction of 6%. The performance of the products tends to deteriorate. The kaolin-modified regulating effect agent obtained by using the modifying liquid of the present invention in combination with the lanthanum oxide treating agent of the present invention and the chitosan regulating effect liquid has the most obvious performance effect, and the replacement by other methods is more significant than the effect of the present invention.

[0065] At the same time, the inventors of the present invention also found that without adding coupled nano-silica agent, the stability of the product under water washing conditions deteriorated significantly. Based on this, the present invention further explored the influence of the preparation of coupled nano-silica agent on product performance.

[0066] Experimental example 1. The only difference from Example 3 is that no dry glass fiber is added in the preparation of the coupled nano-silica agent.

[0067] Experimental example 2. The only difference from Example 3 is that tetrabutyl titanate is not added in the preparation of the coupled nano-silica agent.

[0068] Experimental Example 3. The only difference from Example 3 is that no nano-silicon dioxide is added to the coupling modification liquid.

[0069] Experimental Example 4. The only difference from Example 3 is that no sodium alginate solution is added to the coupling modification solution.

[0070] Experimental Example 5. The only difference from Example 3 is that no silane coupling agent KH560 is added to the coupling modification liquid.

[0071] Use the product under water washing conditions as the test background to test its performance;

[0072] It can be seen from Experimental Examples 1-5 that dry glass fiber is not added in the preparation of the coupled nano-silica agent, and the performance of the product changes. Among the preparation factors of the coupled nano-silica agent, the performance deterioration is the most obvious, followed by the fact that nano-silica is not added to the coupling modification liquid. At the same time, tetrabutyl titanate, sodium alginate solution, and silane coupling agent KH560 are not added in the preparation of the coupled nano-silica agent. The performance of the product has a tendency to deteriorate. The preparation process of the coupled nano-silica agent is unique. Only the coupled nano-silica agent obtained by the specific method of the present invention has the most significant product performance effect. Using other methods instead is not as significant as the effect of the present invention.

[0073] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0074] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A flame retardant chlorinated polyethylene waterproofing membrane, characterized in that: It includes the following raw materials in parts by weight: 45-50 parts of chlorinated polyethylene, 8-12 parts of lignin, 6-9 parts of flame retardant, 5-7 parts of paraffin, 3-5 parts of carbon black, 3-5 parts of barium stearate, and 2-4 parts of vulcanizing agent.

2. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 1, characterized in that: The waterproof coiled material comprises the following raw materials in parts by weight: 47.5 parts of chlorinated polyethylene, 10 parts of lignin, 7.5 parts of flame retardant, 6 parts of paraffin, 4 parts of carbon black, 4 parts of barium stearate, and 3 parts of vulcanizing agent.

3. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 1, characterized in that: The Mooney viscosity of the chlorinated polyethylene is 85±5; the flame retardant is magnesium hydroxide; and the vulcanizing agent is dicumyl peroxide DCP.

4. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 1, characterized in that: The waterproof roll material also includes 5 to 8 parts of a kaolin-modified conditioning agent and 2 to 5 parts of a coupled nano-silicon dioxide agent; The preparation method of the conditioning agent based on kaolin modification is: S01: Preparation of modified kaolin: S11: calcining kaolin at 125-135°C for 5-10 min, then cooling naturally to 55°C and keeping warm; S12: adding 2-3 parts of stearic acid and 1-3 parts of urea to 4-7 parts of 10% by mass sodium lignin sulfonate solution and mixing them evenly to obtain a modified solution; Add 3-6 parts of hot calcined kaolin to the modified solution and shake it for modification. After shaking, filter and dry it to obtain modified kaolin. S02: The modified kaolin and chitosan conditioning liquid are uniformly mixed in a weight ratio of 2:5 to obtain a chitosan-conditioned kaolin agent; The preparation method of chitosan conditioning solution is as follows: Fully mix 2-5 parts of 5-7% chitosan solution, 1-2 parts of 4% yttrium nitrate solution and 2-3 parts of sodium dodecylbenzene sulfonate to obtain a chitosan conditioning solution; S03: Chitosan-modified kaolin agent and lanthanum oxide treatment agent are mixed and ball-milled in a weight ratio of 5:(2~3) at a ball-milling speed of 1000~1500r / min for 1~2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a kaolin-modified modifier.

5. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 4, characterized in that: The oscillation power of the oscillation modification treatment in S12 is 350-400 W, and the oscillation time is 20-30 min.

6. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 4, characterized in that: The preparation method of the lanthanum oxide treating agent is: The lanthanum oxide powder is calcined at 150-170°C for 10-15 minutes, then heated to 310-330°C at a rate of 2-5°C / min, kept warm for 5-10 minutes, then heated to 420°C at a rate of 1-3°C / min, kept warm for 2-5 minutes, and finally air-cooled to room temperature to obtain a lanthanum oxide treating agent.

7. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 1, characterized in that: The preparation method of the coupled nano-silica agent is: S101: adding 1-2 parts of silane coupling agent KH560 to 4-7 parts of alcohol solution, and then adding 1-3 parts of sodium alginate solution and 3-5 parts of nano-silicon dioxide to mix well to obtain a coupling modified solution; S102: placing the glass fiber in a potassium permanganate solution of 3 to 5 times the total amount of the glass fiber for reaction treatment, washing with water and drying after the treatment, blending 1 to 3 parts of the dried glass fiber, 1 to 2 parts of tetrabutyl titanate and 4 to 7 parts of the coupling modification liquid for ultrasonic treatment, washing with water and drying after the treatment, to obtain a coupled nano-silica agent.

8. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 7, characterized in that: The alcohol solution is prepared by mixing ethanol and water in a weight ratio of 10:1; the mass fraction of the sodium alginate solution is 10-15%; and the mass concentration of the potassium permanganate solution is 1-2 mol / L.

9. The flame-retardant chlorinated polyethylene waterproofing membrane according to claim 7, characterized in that: The reaction temperature of the S102 reaction treatment is 52-55° C., the reaction speed is 450-500 r / min, and the reaction time is 35-45 min. The ultrasonic power of the blending ultrasonic treatment is 350-400 W, and the ultrasonic time is 20-30 min.

10. A method for preparing the flame-retardant chlorinated polyethylene waterproofing membrane according to any one of claims 1 to 9, characterized in that: The following steps are involved: Chlorinated polyethylene, lignin, flame retardant, paraffin, carbon black, barium stearate, a conditioning agent based on kaolin modification, a coupled nano-silica agent and a vulcanizing agent are uniformly mixed; Then, the mixture was kneaded at 75°C for 5 minutes, and then kneaded at 120°C for 2 minutes. The kneading was completed to obtain a mixed material. The mixed material is calendered and formed, and finally compounded with non-woven fabric to form the flame-retardant chlorinated polyethylene waterproof coiled material of the present invention; wherein the calendering pressure is 15 MPa and the calendering temperature is 135°C.

Citation Information

Patent Citations

  • Environmental-friendly polyvinyl chloride foamed wood plastic composite material for removing VOC by photocatalyst and acid induction double mechanisms, and preparation method thereof

    CN108299760A

  • Polyethylene waterproof coiled material and preparation method thereof

    CN118126462A

  • Resin composition for outer layer of antibacterial article, molded body, and antibacterial article

    WO2024010084A1

Cited By

  • Flame-retardant, wear-resistant and weather-resistant integrated multi-layer bamboo fiber composite pipe and preparation method thereof

    CN120245519A

  • Greenhouse efficient cultivation method for antrodia camphorata

    CN122319889A