Method for preparing nanometer lithium aluminum titanium phosphate solid electrolyte material by room-temperature aqueous gel method
The preparation of nanometer lithium titanium aluminum phosphate solid electrolyte through a room temperature aqueous gel method solves the problems of complex process, high cost and poor quality in traditional methods, and achieves efficient and environmentally friendly nanoscale material preparation with particle sizes between 50 and 300 nm. The time is adjustable.
Patent Information
- Application Number
- CN202411030759.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The existing technology has the problems of complex process, high cost, poor quality and uncontrollable particle size when preparing lithium titanium aluminum phosphate solid electrolyte materials. In particular, the traditional sol-gel method uses harmful raw materials and high energy consumption.
The room temperature aqueous gel method is used to dissolve lithium, aluminum and phosphorus sources in deionized water and react with titanium citrate to form a hydrogel, which is then heated to obtain a nano-lithium titanium aluminum phosphate solid electrolyte, and low-temperature sintering is used to control the particle size.
The preparation of a cheap and easily available nanolithium titanium aluminum phosphate solid electrolyte with uniform particle size, excellent electrochemical performance, simple process, low cost, environmental friendliness, and suitable for industrial production has been achieved.
Smart Images

Figure CN118754086A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of solid electrolyte preparation for lithium ion batteries, and in particular to a method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel process. Background Art
[0002] Lithium-ion batteries are the most mature lithium-based secondary batteries at present, with advantages such as high voltage, high specific energy, long cycle life, stable operating voltage, and low self-discharge. The liquid electrolytes commonly used in commercial lithium-ion batteries are easy to volatilize, leak, burn, and have poor impact resistance, resulting in safety hazards such as fire and explosion in lithium-ion batteries. Using inert inorganic solid electrolytes to replace flammable and explosive liquid electrolytes is an important way to improve the safety of lithium-ion batteries. Solid electrolytes are light in weight, high in energy density, and have good mechanical properties. They can effectively inhibit the growth of lithium dendrites and further improve the safety of batteries.
[0003] Solid electrolytes can be divided into two categories: polymers and inorganic solid electrolytes. Among them, the research on inorganic solid electrolytes with the advantages of easy preparation, high safety, high room temperature conductivity, and high electrochemical stability has attracted much attention. According to their structural classification, inorganic solid electrolytes can be divided into three major systems: oxides, sulfides, and halides. Among them, oxide solid electrolyte materials have become the most commercially promising solid electrolyte materials due to their easy availability of raw materials, relatively simple preparation process, strong compatibility with existing battery cell processes, high ionic conductivity, good chemical stability, no reaction with oxygen and moisture, and excellent processing performance. The oxide system mainly includes several major categories such as NASICON (sodium superionic conductor) structure system, LISICON (lithium superionic conductor) structure system, perovskite structure system and garnet structure system. Among them, the NASICON-type structured lithium aluminum titanium phosphate Li 1+x Al x Ti 2-x (PO4)3 (0<x≤1) solid electrolyte material has high ionic conductivity (room temperature ionic conductivity>10 -4 S / cm), a wide electrochemical window, good thermal / chemical stability and high mechanical strength. It is one of the most promising solid electrolyte materials for all-solid-state lithium-ion batteries and has attracted widespread attention at home and abroad.
[0004] There are many methods for preparing lithium titanium aluminum phosphate solid electrolytes, and the common ones are solid phase sintering method, coprecipitation method, sol-gel method, melt quenching method, microwave synthesis method, etc. Although the solid phase method is simple in process, it generally uses a variety of raw materials such as lithium source, titanium source, aluminum source, phosphorus source, etc. There are many types of raw materials, large differences in specific gravity, and large differences in particle size, which easily lead to poor precursor mixing effect, high required phase formation temperature, and serious energy consumption, resulting in low purity of prepared lithium titanium aluminum phosphate. At the same time, the sintered solid electrolyte has a high degree of hardening and serious wall sticking phenomenon, which increases the difficulty of subsequent processing. The coprecipitation method requires the introduction of precipitant mixing and heating and must go through the steps of filtering, washing, drying, etc. The steps are cumbersome, and the product after ball milling of inorganic powder is not easy to collect, which is time-consuming and labor-intensive, and the discharge rate is low, resulting in great waste, and increasing the cost of mass production of lithium titanium aluminum phosphate. The titanium source used in the traditional sol-gel method is generally titanium tetrachloride, which is very easy to react with moisture in the air to produce HCl acid mist, which is harmful to humans and the environment; or titanium alkoxides such as tetrabutyl titanate are used, which are expensive and costly raw materials. The raw materials are very easy to react with moisture in the air and are difficult to store. The raw materials are flammable and pose safety hazards. In addition, organic solvents that are harmful to the human body, such as ethylene glycol, need to be used, and the water solvent and organic solvent need to be removed by heating, which consumes a lot of energy and the process is complicated.
[0005] Existing studies have shown that particle size plays a vital role in ionic conductivity, so lithium titanium aluminum phosphate materials with nanometer-scale particle size exhibit excellent ionic conductivity. However, existing methods generally have problems such as poor product quality, high cost of raw materials, or complicated processes that increase processing costs, and the particle size of lithium titanium aluminum phosphate materials with nanometer-scale particle size obtained by conventional methods is uncontrollable and has poor particle size uniformity. Therefore, in view of the problems existing in the existing preparation schemes, it is urgent to develop a lithium titanium aluminum phosphate solid electrolyte with good quality, uniform particle size, and excellent ionic conductivity, as well as a preparation method of a lithium titanium aluminum phosphate solid electrolyte with low cost and simple process. Summary of the invention
[0006] One of the technical problems to be solved by the present invention is to overcome the problems of complex preparation process, high cost (expensive raw materials, sintering agglomeration, wall sticking, need for crushing, etc.) and poor quality (large particle size, uneven distribution) of the prior art methods, and provide a method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method.
[0007] The present invention provides a method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, comprising the following steps: S1. Press Li 1+x Al x Ti 2-xA lithium source, an aluminum source, a phosphorus source and titanium citrate are weighed in a stoichiometric ratio of (PO4)3, and are dissolved in deionized water to obtain a lithium source dispersion system, an aluminum source dispersion system, a phosphorus source dispersion system and a titanium citrate aqueous solution, respectively, wherein 0<x≤1, each substance is weighed according to its corresponding molar ratio of lithium, aluminum, titanium and phosphorus, and the lithium source is in excess of 5% to 10%, and then the lithium source dispersion system, the aluminum source dispersion system and the phosphorus source dispersion system are stirred and mixed at room temperature until clarified to obtain a lithium-aluminum-phosphorus composite aqueous solution; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in the step S1 into the titanium citrate aqueous solution at room temperature while stirring to obtain a clear and transparent lithium aluminum titanium phosphate precursor aqueous solution, then aging the aqueous solution at room temperature to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel to obtain a lithium aluminum titanium phosphate precursor dry gel; S3, calcining the lithium aluminum titanium phosphate precursor dry gel obtained in step S2 to obtain a nano lithium aluminum titanium phosphate solid electrolyte material.
[0008] Compared with the prior art, especially compared with the traditional sol-gel method for preparing lithium titanium aluminum phosphate solid electrolyte, the present invention provides a method for preparing nano lithium titanium aluminum phosphate solid electrolyte material by room temperature aqueous gel method: firstly, a dispersion system of various raw materials of lithium titanium aluminum phosphate precursor is prepared, the dispersion system before reaction and mixing exists in a solution state, and the molecules of various raw materials of the precursor exist in ionic form, so that the subsequent mixing reaches the molecular or ionic level. A large number of titanium citrate molecules are hydrolyzed in situ in the indoor titanium citrate aqueous solution, and these released citric acid molecules are cross-linked to form a macromolecular network. When the molecules of lithium source, aluminum source and phosphorus source enter the cross-linked network formed by these citric acid molecules, they are quickly complexed into a larger cross-linked network, and finally form a hydrogel together with the water molecules in the system. In the lithium titanium aluminum phosphate hydrogel system, all the raw materials involved in the reaction are mixed at the molecular level, and the nucleated particles are confined to the tiny hydrogel network. When the dried hydrogel is calcined, these tiny hydrogel networks are used as growth units, which limits the growth space of the particles. Finally, nano-scale lithium titanium aluminum phosphate solid electrolyte materials are synthesized, and the range of particle size can be adjusted by controlling the calcination temperature and time.
[0009] Compared with the preparation method of the prior art, the present invention has the following beneficial effects: The preparation method of the present invention adopts cheap and readily available raw materials and uses a water-based system to synthesize lithium aluminum titanium phosphate. The preparation process is simple, the cost is low, the prepared material has a small particle size, a narrow particle size distribution, a large specific surface area, and good electrochemical performance. The produced product particles are closely arranged, the particle size is relatively uniform, and the particle size is adjustable between 50 and 300 nm. The present invention effectively solves the problems that the particle size of the product obtained by the traditional preparation method is uncontrollable, the process is complicated, or the raw materials used are expensive, the process is uneconomical, especially the traditional dissolution-gel process for preparing lithium aluminum titanium phosphate uses organic or inorganic additives or complexing agents, the sol evaporation process takes too long, and the energy consumption is high. The present invention uses a self-generated in-situ complexation technology to synthesize a hydrogel precursor of lithium aluminum titanium phosphate at room temperature with water as a solvent, and can obtain a nano-scale lithium aluminum titanium phosphate precursor through subsequent low-temperature sintering. The synthesized product shows good uniformity, and the particles are closely arranged and uniform in size. In addition, the solvent of the preparation method is mainly water, which is environmentally friendly, and can be industrially produced. Nano-lithium aluminum titanium phosphate solid electrolyte materials with particle sizes between 50 and 300 nm can be produced.
[0010] In a possible embodiment, in step S1, the lithium source is selected from at least one of lithium oxide, anhydrous lithium hydroxide, lithium hydroxide monohydrate, lithium chloride, lithium nitrate, lithium formate, anhydrous lithium acetate, lithium acetate dihydrate, lithium carbonate, lithium oxalate, lithium citrate, lithium phosphate, lithium tartrate, lithium hydrogen phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, and lithium ammonium phosphate; the aluminum source is selected from at least one of aluminum chloride, anhydrous aluminum nitrate, nonahydrate aluminum nitrate, aluminum dihydrogen phosphate, aluminum acetate, aluminum phosphate, aluminum oxalate, aluminum carbonate, and aluminum hydroxide; the phosphorus source is selected from any one or more combinations of white phosphorus, red phosphorus, black phosphorus, phosphorus trioxide, phosphorus pentoxide, phosphoric acid, metaphosphoric acid, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, lithium dihydrogen phosphate, and dilithium hydrogen phosphate.
[0011] In a possible embodiment, the lithium source is at least one of lithium hydroxide monohydrate, lithium nitrate, anhydrous lithium acetate, lithium acetate dihydrate, and lithium carbonate; the aluminum source is at least one of aluminum chloride, aluminum nitrate nonahydrate, aluminum dihydrogen phosphate, aluminum hydroxide, and aluminum carbonate; and the phosphorus source is at least one of phosphoric acid, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and aluminum dihydrogen phosphate.
[0012] By selecting the above-mentioned lithium source, aluminum source and phosphorus source, the preparation cost of the method for preparing nano-titanium aluminum phosphate lithium solid electrolyte material by the room temperature aqueous gel method in the present invention is further reduced, and the quality of the final product is improved by selecting the raw materials in the above-mentioned possible implementation methods.
[0013] In a possible implementation, in step S2, the aging treatment conditions are: aging the lithium aluminum titanium phosphate precursor aqueous solution at room temperature for 5 to 30 minutes to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel; The lithium aluminum titanium phosphate precursor aqueous solution is gradually converted into a precursor hydrosol by aging at room temperature, and the hydrosol further swells into a wet gel. The selected aging time can ensure sufficient swelling of the sol without being too long to reduce production efficiency.
[0014] In a possible implementation, in step S2, the conditions for heating the aqueous wet gel are: heating at a temperature of 60 to 120° C. for 30 to 360 min to obtain a lithium titanium aluminum phosphate precursor dry gel.
[0015] The drying temperature of the selected wet gel is relatively mild, not too high, and the drying time is not too long. It is only necessary to ensure that there is no obvious moisture adhesion. Both of these ensure the maximum possible reduction in energy consumption and save production costs.
[0016] In a possible embodiment, in step S3, the calcination is performed in multiple stages, including a first stage and a second stage. The calcination temperature in the first stage is 300-500°C, the heating rate is 2-10°C / min, and the insulation time is 2-6 h; the calcination temperature in the second stage is 650-900°C, the heating rate is 2-10°C / min, and the insulation time is 0.5-10 h.
[0017] The first stage of low-temperature calcination can remove volatile components and organic impurities in the reactants, prevent impurity molecules from reacting with the reactants, and the calcination temperature in the low-temperature stage is low, which can reduce unnecessary energy waste; the second stage of calcination can ensure that the reactants fully react and crystallize, and the lower sintering temperature will not promote the growth of lithium aluminum titanium phosphate grains, so the obtained lithium aluminum titanium phosphate material has a smaller particle size, a narrower particle size distribution, and fewer agglomerates. At the same time, the obtained ultrafine lithium aluminum titanium phosphate nanoparticles also have ultra-high relative density, greater ion concentration, and larger interface contact area, high ion mobility, and can also form a larger continuous conduction path for lithium ion transmission.
[0018] The second technical problem to be solved by the present invention is to provide a nano-lithium titanium aluminum phosphate solid electrolyte to solve the problems of poor quality, uneven particle size and general ion conductivity of the nano-lithium titanium aluminum phosphate solid electrolyte in the prior art.
[0019] In order to solve the above problems, the present invention provides a nano-lithium aluminum titanium phosphate solid electrolyte, and the nano-lithium aluminum titanium phosphate solid electrolyte is prepared by the preparation method.
[0020] Compared with the prior art, the nano-lithium aluminum titanium phosphate solid electrolyte material in the present invention has a small particle size, a narrow particle size distribution, a large specific surface area, and good electrochemical performance. The particles of the product produced are tightly arranged, the particle size is relatively uniform, the particle size is adjustable between 50 and 300 nm, and it has a high ionic conductivity.
[0021] In a possible embodiment, the molecular formula of the solid electrolyte powder material is Li 1+x Al x Ti 2-x (PO4)3, and the particle size of the solid electrolyte material is 50 to 300 nm.
[0022] In one possible implementation, 0.3≤x≤0.5.
[0023] x can take any value between 0 and 1, such as x=0.3, 0.4, 0.5.
[0024] The present invention further improves the electrochemical performance of the solid electrolyte powder material product by further optimizing the above x data. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a process flow chart of a method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method in the present invention; Figure 2 The nano-lithium aluminum titanium phosphate Li prepared in Example 1 1.3 Al 0.3 Ti 1.7 Scanning electron microscope (SEM) image of (PO4)3; Figure 3 The nano-lithium aluminum titanium phosphate Li prepared in Example 1 1.3 Al 0.3 Ti 1.7 X-ray diffraction (XRD) pattern of (PO4)3; Figure 4 The nano-lithium aluminum titanium phosphate Li prepared in Example 2 1.3 Al 0.3 Ti 1.7 Scanning electron microscope (SEM) image of (PO4)3; Figure 5 The nano-lithium aluminum titanium phosphate Li prepared in Example 3 1.3 Al 0.3 Ti 1.7 Scanning electron microscope (SEM) image of (PO4)3; Figure 6 The nano-lithium aluminum titanium phosphate Li prepared in Example 4 1.4 Al0.4 Ti 1.6 X-ray diffraction (XRD) pattern of (PO4)3; Figure 7 The nano-lithium aluminum titanium phosphate Li prepared in Example 5 1.5 Al 0.5 Ti 1.5 X-ray diffraction (XRD) pattern of (PO4)3. DETAILED DESCRIPTION
[0026] The present invention is further described in detail below by specific embodiments in conjunction with the accompanying drawings. In the following embodiments, many detailed descriptions are intended to enable the present application to be better understood. However, those skilled in the art can effortlessly recognize that some of the features can be omitted in different situations, or can be replaced by other materials and methods. In some cases, some operations related to the present application are not shown or described in the specification, in order to avoid the core part of the present application being overwhelmed by too much description, and for those skilled in the art, it is not necessary to describe these related operations in detail, and they can fully understand the related operations according to the description in the specification and the general technical knowledge in the art.
[0027] In addition, the features, operations or characteristics described in the specification can be combined in any appropriate manner to form various implementations. At the same time, the steps or actions in the method description can also be interchanged or adjusted in a manner that is obvious to those skilled in the art. Therefore, the various sequences in the specification and the drawings are only for the purpose of clearly describing a certain embodiment and are not meant to be a required sequence, unless otherwise specified that a certain sequence must be followed.
[0028] It should be noted that the numerical values given in the following examples are as accurate as possible, but those skilled in the art understand that due to unavoidable measurement errors and experimental operation problems, each number should be understood as an approximate number rather than an absolutely accurate value. For example, due to the error of the weighing instrument, the weight value of each raw material for preparing the solid electrolyte material in each embodiment should be understood to have an error of ±2% or ±1%.
[0029] The present invention provides a nano-lithium aluminum titanium phosphate solid electrolyte powder and a preparation method thereof. Figure 1 The process flow chart of the method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method in the present invention is shown below in combination with Figure 1 The present invention provides a nano-lithium titanium aluminum phosphate solid electrolyte material prepared by a room temperature aqueous gel method and a preparation method thereof.
[0030] The present invention provides a method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, comprising the following steps: S1. Press Li 1+x Al x Ti 2-x A lithium source, an aluminum source, a phosphorus source and titanium citrate are weighed in a stoichiometric ratio of (PO4)3, and are dissolved in deionized water to obtain a lithium source dispersion system, an aluminum source dispersion system, a phosphorus source dispersion system and a titanium citrate aqueous solution, respectively, wherein 0<x≤1, each substance is weighed according to its corresponding molar ratio of lithium, aluminum, titanium and phosphorus, and the lithium source is in excess of 5% to 10%, and then the lithium source dispersion system, the aluminum source dispersion system and the phosphorus source dispersion system are stirred and mixed at room temperature until clarified to obtain a lithium-aluminum-phosphorus composite aqueous solution; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in the step S1 into the titanium citrate aqueous solution at room temperature while stirring to obtain a clear and transparent lithium aluminum titanium phosphate precursor aqueous solution, then aging the aqueous solution at room temperature to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel to obtain a lithium aluminum titanium phosphate precursor dry gel; S3, calcining the lithium aluminum titanium phosphate precursor dry gel obtained in step S2 to obtain a nano lithium aluminum titanium phosphate solid electrolyte material.
[0031] As a preferred scheme, in step S1, the lithium source is selected from at least one of lithium oxide, anhydrous lithium hydroxide, lithium hydroxide monohydrate, lithium chloride, lithium nitrate, lithium formate, anhydrous lithium acetate, lithium acetate dihydrate, lithium carbonate, lithium oxalate, lithium citrate, lithium phosphate, lithium tartrate, lithium hydrogen phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, and lithium ammonium phosphate; the aluminum source is selected from at least one of aluminum chloride, anhydrous aluminum nitrate, aluminum nitrate nonahydrate, aluminum dihydrogen phosphate, aluminum acetate, aluminum phosphate, aluminum oxalate, aluminum carbonate, and aluminum hydroxide; the phosphorus source is selected from any one or more combinations of white phosphorus, red phosphorus, black phosphorus, phosphorus trioxide, phosphorus pentoxide, phosphoric acid, metaphosphoric acid, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, lithium dihydrogen phosphate, and dilithium hydrogen phosphate.
[0032] As a preferred solution, the lithium source is at least one of lithium hydroxide monohydrate, lithium nitrate, anhydrous lithium acetate, lithium acetate dihydrate, and lithium carbonate; the aluminum source is at least one of aluminum chloride, aluminum nitrate nonahydrate, aluminum dihydrogen phosphate, aluminum hydroxide, and aluminum carbonate; and the phosphorus source is at least one of phosphoric acid, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and aluminum dihydrogen phosphate.
[0033] As a preferred solution, in step S2, the aging treatment conditions are: aging the lithium aluminum titanium phosphate precursor aqueous solution at room temperature for 5 to 30 minutes to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel; As a preferred solution, in step S2, the conditions for heating the aqueous wet gel are: heating at a temperature of 60 to 120° C. for 30 to 360 min to obtain a lithium aluminum titanium phosphate precursor dry gel.
[0034] As a preferred scheme, in the step S3, the calcination is carried out in multiple stages, including a first stage and a second stage. The calcination temperature in the first stage is 300-500°C, the heating rate is 2-10°C / min, and the insulation time is 2-6 h; the calcination temperature in the second stage is 650-900°C, the heating rate is 2-10°C / min, and the insulation time is 0.5-10 h.
[0035] The present invention also provides a nano-lithium titanium aluminum phosphate solid electrolyte, and the nano-lithium titanium aluminum phosphate solid electrolyte is prepared by the preparation method.
[0036] As a preferred solution, the molecular formula of the solid electrolyte powder material is Li 1+x Al x Ti 2-x (PO4)3, and the particle size of the solid electrolyte material is 50 to 300 nm.
[0037] As a preferred solution, 0.3≤x≤0.5.
[0038] In order to better understand the technical solution provided by the present invention, the following multiple specific examples are used to illustrate the specific process and characteristics of preparing nano-lithium aluminum titanium phosphate solid electrolytes using the method provided by the present invention. However, it should be understood that these embodiments are only used for more detailed description and should not be understood as limiting the present invention in any form, that is, they are not intended to limit the scope of protection of the present invention.
[0039] If no specific technology or conditions are specified in the embodiments, they can be carried out according to the technology or conditions described in the literature in the field or according to the product instructions. In the following embodiments, the unit g is used to calculate the mass, and the case of converting it into a mass ratio should also be within the scope of protection of the present invention.
[0040] Example 1 This embodiment provides a method for preparing a nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, the preparation method comprising the following steps: S1. Press Li 1.3 Al 0.3 Ti 1.7The stoichiometric ratio of (PO4)3 (x=0.3) is as follows: 91.27 g of lithium hydroxide monohydrate (excess 10 wt%) is weighed and dissolved in 150 g of deionized water; 169.68 g of aluminum nitrate nonahydrate is weighed and dissolved in 150 g of deionized water; 517.55 g of 85% phosphoric acid solution is weighed and diluted with 125 g of deionized water; the three solutions are then mixed and stirred at room temperature until clear to obtain a lithium-aluminum-phosphorus composite aqueous solution; Weigh 927.82 g of titanium citrate and dissolve it in 1200 g of deionized water to obtain an aqueous solution of titanium citrate; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in step S1 into the titanium citrate aqueous solution at room temperature while stirring to obtain a clear and transparent lithium aluminum titanium phosphate precursor aqueous solution, then aging the aqueous solution at room temperature for 20 min to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel at 80 ° C for 120 min to obtain lithium aluminum titanium phosphate Li 1.3 Al 0.3 Ti 1.7 (PO4)3 precursor xerogel; S3, the lithium aluminum titanium phosphate Li obtained in step S2 1.3 Al 0.3 Ti 1.7 The (PO4)3 precursor dry gel is calcined to obtain lithium aluminum titanium phosphate Li 1.3 Al 0.3 Ti 1.7 (PO4)3 solid electrolyte material. The first stage calcination temperature is 300 ℃, the heating rate is 5 ℃ / min, and the holding time is 2 h; the second stage calcination temperature is 750 ℃, the heating rate is 5 ℃ / min, and the holding time is 2 h.
[0041] Figure 2 The nano solid electrolyte lithium aluminum titanium phosphate Li prepared in Example 1 1.3 Al 0.3 Ti 1.7 (PO4)3 SEM image, from which we can see that nano-titanium aluminum phosphate Li 1.3 Al 0.3 Ti 1.7 The (PO4)3 material exhibits good uniformity, with particles closely arranged and uniform in size, and an average particle size of about 70 nm.
[0042] Figure 3 The nano solid electrolyte lithium aluminum titanium phosphate Li prepared in Example 1 1.3 Al 0.3 Ti 1.7The XRD spectrum of (PO4)3 shows that the main characteristic diffraction peaks of the sample are consistent with the standard card (JCPDS#35-0754), the diffraction peaks are sharp, the intensity is high, and there are no impurity peaks, indicating that the sample has good crystallinity and high purity.
[0043] Example 2 This embodiment provides a method for preparing a nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, the preparation method comprising the following steps: S1. Press Li 1.3 Al 0.3 Ti 1.7 The stoichiometric ratio of (PO4)3 (x=0.3) is as follows: 91.27 g of lithium hydroxide monohydrate (excess 10 wt%) is dissolved in 150 g of deionized water, 35.1 g of aluminum hydroxide is dispersed in 100 g of deionized water, 517.55 g of 85% phosphoric acid solution is weighed, and 125 g of deionized water is added to dilute it. The three solutions are then mixed and stirred at room temperature until clear to obtain a lithium-aluminum-phosphorus composite aqueous solution; Weigh 927.82 g of titanium citrate and dissolve it in 1200 g of deionized water to obtain an aqueous solution of titanium citrate; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in step S1 into the titanium citrate aqueous solution at room temperature while stirring to obtain a clear and transparent lithium aluminum titanium phosphate precursor aqueous solution, then aging the aqueous solution at room temperature for 30 min to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel at 60 ° C for 240 min to obtain lithium aluminum titanium phosphate Li 1.3 Al 0.3 Ti 1.7 (PO4)3 precursor xerogel; S3, the lithium aluminum titanium phosphate Li obtained in step S2 1.3 Al 0.3 Ti 1.7 The (PO4)3 precursor dry gel is calcined to obtain lithium aluminum titanium phosphate Li 1.3 Al 0.3 Ti 1.7 (PO4)3 solid electrolyte material. The first stage calcination temperature is 350 ℃, the heating rate is 5 ℃ / min, and the holding time is 2 h; the second stage calcination temperature is 800 ℃, the heating rate is 5 ℃ / min, and the holding time is 2 h.
[0044] Figure 4 The nano solid electrolyte lithium aluminum titanium phosphate Li prepared in Example 2 1.3 Al 0.3 Ti 1.7(PO4)3 SEM image, from which we can see that nano-titanium aluminum phosphate Li 1.3 Al 0.3 Ti 1.7 The (PO4)3 material exhibits good uniformity, with particles closely arranged and uniform in size, and an average particle size of about 110 nm.
[0045] Example 3 This embodiment provides a method for preparing a nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, the preparation method comprising the following steps: S1. Press Li 1.3 Al 0.3 Ti 1.7 The stoichiometric ratio of (PO4)3 (x=0.3) is as follows: 91.27 g of lithium hydroxide monohydrate (excess 10 wt%) is dissolved in 150 g of deionized water, 35.1 g of aluminum hydroxide is dispersed in 100 g of deionized water, 517.55 g of 85% phosphoric acid solution is weighed, and 125 g of deionized water is added to dilute it. The three solutions are then mixed and stirred at room temperature until clear to obtain a lithium-aluminum-phosphorus composite aqueous solution; Weigh 927.82 g of titanium citrate and dissolve it in 1200 g of deionized water to obtain an aqueous solution of titanium citrate; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in step S1 into the titanium citrate aqueous solution at room temperature while stirring to obtain a clear and transparent lithium aluminum titanium phosphate precursor aqueous solution, then aging the aqueous solution at room temperature for 10 min to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel at 90 ° C for 180 min to obtain lithium aluminum titanium phosphate Li 1.3 Al 0.3 Ti 1.7 (PO4)3 precursor xerogel; S3, the lithium aluminum titanium phosphate Li obtained in step S2 1.3 Al 0.3 Ti 1.7 The (PO4)3 precursor dry gel is calcined to obtain lithium aluminum titanium phosphate Li 1.3 Al 0.3 Ti 1.7 (PO4)3 solid electrolyte material. The first stage calcination temperature is 300 ℃, the heating rate is 5 ℃ / min, and the holding time is 2 h; the second stage calcination temperature is 800 ℃, the heating rate is 5 ℃ / min, and the holding time is 4 h.
[0046] Figure 5 The nano solid electrolyte lithium aluminum titanium phosphate Li prepared in Example 3 1.3 Al 0.3Ti 1.7 (PO4)3 SEM image, from which we can see that nano-titanium aluminum phosphate Li 1.3 Al 0.3 Ti 1.7 The (PO4)3 material exhibits good uniformity, with particles closely arranged and uniform in size, with an average particle size of about 200 nm.
[0047] Example 4 This embodiment provides a method for preparing a nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, the preparation method comprising the following steps: S1. Press Li 1.4 Al 0.4 Ti 1.6 The stoichiometric ratio of (PO4)3 (x=0.4) is as follows: 98.29 g of lithium hydroxide monohydrate (excess 10 wt%) is weighed and dissolved in 150 g of deionized water; 226.24 g of aluminum nitrate nonahydrate is weighed and dissolved in 180 g of deionized water; 517.55 g of 85% phosphoric acid solution is weighed and diluted with 125 g of deionized water; the three solutions are then mixed and stirred at room temperature until clear to obtain a lithium-aluminum-phosphorus composite aqueous solution; Weigh 873.24 g of titanium citrate and dissolve it in 1200 g of deionized water to obtain an aqueous solution of titanium citrate; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in step S1 into the titanium citrate aqueous solution at room temperature while stirring to obtain a clear and transparent lithium aluminum titanium phosphate precursor aqueous solution, then aging the aqueous solution at room temperature for 10 min to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel at 60 ° C for 240 min to obtain lithium aluminum titanium phosphate Li 1.4 Al 0.4 Ti 1.6 (PO4)3 precursor xerogel; S3, the lithium aluminum titanium phosphate Li obtained in step S2 1.4 Al 0.4 Ti 1.6 The (PO4)3 precursor dry gel is calcined to obtain lithium aluminum titanium phosphate Li 1.4 Al 0.4 Ti 1.6 (PO4)3 solid electrolyte material. The first stage calcination temperature is 350 ℃, the heating rate is 5 ℃ / min, and the holding time is 2 h; the second stage calcination temperature is 750 ℃, the heating rate is 5 ℃ / min, and the holding time is 3 h.
[0048] Figure 6 The nano solid electrolyte lithium aluminum titanium phosphate Li prepared in Example 4 1.4Al 0.4 Ti 1.6 The XRD spectrum of (PO4)3 shows that the main characteristic diffraction peaks of the sample are consistent with the standard card (JCPDS#35-0754), the diffraction peaks are sharp, the intensity is high, and there are no impurity peaks, indicating that the sample has good crystallinity and high purity.
[0049] Example 5 This embodiment provides a method for preparing a nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, the preparation method comprising the following steps: S1. Press Li 1.5 Al 0.5 Ti 1.5 The stoichiometric ratio of (PO4)3 (x=0.5) was 105.31 g of lithium hydroxide monohydrate (excess 10 wt%) was dissolved in 200 g of deionized water, 58.5 g of aluminum hydroxide was dispersed in 150 g of deionized water, 517.55 g of 85% phosphoric acid solution was weighed, and diluted with 125 g of deionized water, and then the three solutions were mixed and stirred at room temperature until clear to obtain a lithium-aluminum-phosphorus composite aqueous solution; Weigh 818.66 g of titanium citrate and dissolve it in 1000 g of deionized water to obtain an aqueous solution of titanium citrate; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in step S1 into the titanium citrate aqueous solution at room temperature while stirring to obtain a clear and transparent lithium aluminum titanium phosphate precursor aqueous solution, then aging the aqueous solution at room temperature for 20 min to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel at 80 ° C for 180 min to obtain lithium aluminum titanium phosphate Li 1.5 Al 0.5 Ti 1.5 (PO4)3 precursor xerogel; S3, the lithium aluminum titanium phosphate Li obtained in step S2 1.5 Al 0.5 Ti 1.5 The (PO4)3 precursor dry gel is calcined to obtain lithium aluminum titanium phosphate Li 1.5 Al 0.5 Ti 1.5 (PO4)3 solid electrolyte material. The first stage calcination temperature is 400 ℃, the heating rate is 5 ℃ / min, and the holding time is 2.5 h; the second stage calcination temperature is 850 ℃, the heating rate is 5 ℃ / min, and the holding time is 2 h.
[0050] Figure 7 The nano solid electrolyte lithium aluminum titanium phosphate Li prepared in Example 5 1.5 Al 0.5 Ti1.5 The XRD spectrum of (PO4)3 shows that the main characteristic diffraction peaks of the sample are consistent with the standard card (JCPDS#35-0754), the diffraction peaks are sharp, the intensity is high, and there are no impurity peaks, indicating that the sample has good crystallinity and high purity.
[0051] The above embodiments and the tests conducted on the embodiments further illustrate that a method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method in the present invention uses cheap and readily available raw materials and utilizes a water-based system to synthesize lithium aluminum titanium phosphate. The preparation process is simple and the cost is low. The prepared nano-lithium aluminum titanium phosphate solid electrolyte material has a small particle size, a narrow particle size distribution, a large specific surface area, and good electrochemical properties. The particles of the product produced are tightly arranged and the particle size is relatively uniform, and the particle size is adjustable between 50 and 300 nm.
[0052] The invention discloses a method for preparing nano-lithium titanium aluminum phosphate solid electrolyte material by a room temperature aqueous gel method, which effectively solves the problems that the particle size of the product obtained by the traditional preparation method is uncontrollable, the process is complicated, or the raw materials used are expensive, the process is not economical, and in particular, the traditional dissolution-gel method for preparing lithium titanium aluminum phosphate adopts organic or inorganic additives or complexing agents, the sol evaporation process takes too long, and the energy consumption is high. The invention discloses a method for preparing nano-lithium titanium aluminum phosphate solid electrolyte material by a room temperature aqueous gel method, which uses a self-generated in-situ complexation technology to synthesize a hydrogel precursor of lithium titanium aluminum phosphate at room temperature with water as a solvent, and a nano-scale lithium titanium aluminum phosphate precursor can be obtained by subsequent low-temperature sintering, and the synthesized product shows good uniformity, and the particles are closely arranged and uniform in size. In addition, the solvent of the preparation method is mainly water, which is environmentally friendly, and the nano-lithium titanium aluminum phosphate solid electrolyte material with a particle size between 50 and 300 nm can be industrially produced, thereby solving the problems existing in the background technology.
[0053] Those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present invention and to form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present invention and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
[0054] In the description of the present application, the description with reference to the terms "one embodiment", "some embodiments", "in the present embodiment", "specific example", or "some examples" etc. means that the specific features, mechanisms, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, mechanisms, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0055] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.
Claims
1. A method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by a room temperature aqueous gel method, characterized in that: The following steps are involved: S1. Press Li 1+x Al x Ti 2-x A lithium source, an aluminum source, a phosphorus source and titanium citrate are weighed in a stoichiometric ratio of (PO4)3, and the mixture is dissolved in deionized water to obtain a lithium source dispersion system, an aluminum source dispersion system, a phosphorus source dispersion system and a titanium citrate aqueous solution, respectively, wherein 0<x≤1, and each substance is weighed according to its corresponding molar ratio of lithium, aluminum, titanium and phosphorus, and the lithium source is in excess of 5% to 10%. Subsequently, the lithium source dispersion system, the aluminum source dispersion system and the phosphorus source dispersion system are stirred and mixed at room temperature until they are clear to obtain a lithium-aluminum-phosphorus composite aqueous solution; S2, pouring the lithium-aluminum-phosphorus composite aqueous solution obtained in step S1 into the titanium citrate aqueous solution while stirring at room temperature to obtain a clear and transparent lithium titanium aluminum phosphate precursor aqueous solution, then aging the lithium titanium aluminum phosphate precursor aqueous solution at room temperature to obtain a lithium titanium aluminum phosphate precursor aqueous wet gel, and finally heating the aqueous wet gel to obtain a lithium titanium aluminum phosphate precursor xerogel; S3. calcining the lithium aluminum titanium phosphate precursor dry gel obtained in step S2 to obtain a nano-lithium aluminum titanium phosphate solid electrolyte material.
2. The method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by the room temperature aqueous gel method according to claim 1, characterized in that: In step S1, the lithium source is selected from at least one of lithium oxide, anhydrous lithium hydroxide, lithium hydroxide monohydrate, lithium chloride, lithium nitrate, lithium formate, anhydrous lithium acetate, lithium acetate dihydrate, lithium carbonate, lithium oxalate, lithium citrate, lithium phosphate, lithium tartrate, lithium hydrogen phosphate, lithium dihydrogen phosphate, dilithium hydrogen phosphate, and lithium ammonium phosphate; the aluminum source is selected from at least one of aluminum chloride, anhydrous aluminum nitrate, aluminum nitrate nonahydrate, aluminum dihydrogen phosphate, aluminum acetate, aluminum phosphate, aluminum oxalate, aluminum carbonate, and aluminum hydroxide; and the phosphorus source is selected from any one or more of white phosphorus, red phosphorus, black phosphorus, phosphorus trioxide, phosphorus pentoxide, phosphoric acid, metaphosphoric acid, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, lithium phosphate, lithium dihydrogen phosphate, and dilithium hydrogen phosphate.
3. The method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by the room temperature aqueous gel method according to claim 2, characterized in that: The lithium source is at least one of lithium hydroxide monohydrate, lithium nitrate, anhydrous lithium acetate, lithium acetate dihydrate, and lithium carbonate; the aluminum source is at least one of aluminum chloride, aluminum nitrate nonahydrate, aluminum dihydrogen phosphate, aluminum hydroxide, and aluminum carbonate; and the phosphorus source is at least one of phosphoric acid, ammonium phosphate, ammonium dihydrogen phosphate, diammonium hydrogen phosphate, and aluminum dihydrogen phosphate.
4. The method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by the room temperature aqueous gel method according to claim 1, characterized in that: In the step S2, the aging treatment condition is: aging the lithium aluminum titanium phosphate precursor aqueous solution at room temperature for 5 to 30 minutes to obtain a lithium aluminum titanium phosphate precursor aqueous wet gel.
5. The method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by the room temperature aqueous gel method according to claim 1, characterized in that: In step S2, the conditions for heating the aqueous wet gel of the lithium titanium aluminum phosphate precursor are: heating at a temperature of 60 to 120° C. for 30 to 360 minutes to obtain the lithium titanium aluminum phosphate precursor dry gel.
6. The method for preparing nano-lithium aluminum titanium phosphate solid electrolyte material by the room temperature aqueous gel method according to claim 1, characterized in that: In step S3, the calcination is carried out in multiple stages, including a first stage and a second stage. The calcination temperature in the first stage is 300-500°C, the heating rate is 2-10°C / min, and the holding time is 2-6 hours; the calcination temperature in the second stage is 650-900°C, the heating rate is 2-10°C / min, and the holding time is 0.5-10 hours.
7. A nano-lithium aluminum titanium phosphate solid electrolyte material, characterized in that: The nano-lithium aluminum titanium phosphate solid electrolyte material is prepared by the preparation method according to any one of claims 1 to 6.
8. The nano-lithium aluminum titanium phosphate solid electrolyte material according to claim 7, characterized in that The molecular formula of the nano-lithium aluminum titanium phosphate solid electrolyte powder material is Li 1+x Al x Ti 2-x (PO4)3, and the particle size of the nano-lithium aluminum titanium phosphate solid electrolyte material is 50 to 300 nm.
9. The nano-lithium aluminum titanium phosphate solid electrolyte material according to claim 8, characterized in that 0.3≤x≤0.5。
Citation Information
Patent Citations
Quasi-solid electrolyte as well as preparation method and application thereof
CN108365260A
Solid electrolyte, composite electrolyte membrane containing solid electrolyte, and preparation and application of solid electrolyte
CN116387608A
Method for preparing lithium aluminum titanium phosphate solid electrolyte step by step and application
CN117049497A
Composite solid electrolyte for lithium secondary battery and method for preparing same
EP4456235A1
Method for producing li-ion conductive lithium aluminium titanium phosphates and use thereof as a solid-state electrolyte
WO2013156116A1