A resin-based hard carbon anode material and its preparation method in sodium-ion batteries
By introducing phosphorus dopant during the preparation of resin-based hard carbon anode material, the high-temperature process of phosphorus dopant releases small gas molecules to create pores and increase the interlayer spacing, solving the problem of poor rate performance of resin-based hard carbon materials and realizing the efficient application of hard carbon materials in sodium-ion batteries.
Patent Information
- Application Number
- CN202410921620.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing hard carbon materials made from resins exhibit poor rate performance when used in sodium-ion batteries.
Phosphorus dopants are introduced during the preparation process. The high-temperature process of phosphorus dopant releases small gas molecules to create pores, and the larger atomic radius of phosphorus atoms increases the interlayer spacing of hard carbon, thereby improving the rate performance of hard carbon materials.
Phosphorus doping significantly improves the sodium storage capacity and rate performance of hard carbon materials, making them suitable for sodium-ion batteries.
Smart Images

Figure CN118754095B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of battery materials technology, and in particular to a resin-based hard carbon anode material, its preparation method, and a sodium-ion battery. Background Technology
[0002] Sodium is abundant, widely available, and inexpensive, and sodium-ion batteries, which operate on a similar principle to lithium-ion batteries, hold the promise of replacing lithium-ion batteries in energy storage. However, because the ionic radius of sodium ions is larger than that of lithium ions, existing negative electrode materials for lithium-ion batteries are not suitable for sodium-ion batteries. Therefore, there is an urgent need to find a suitable negative electrode material for sodium-ion batteries.
[0003] Hard carbon is considered a promising anode material for sodium-ion batteries due to its large interlayer spacing, good structural stability, and high reversible capacity. Resin is a commonly used raw material for hard carbon anode materials; however, while hard carbon materials prepared from resin exhibit high capacity in sodium-ion batteries, their rate performance is poor, limiting their application in these batteries. Summary of the Invention
[0004] To address the problem of poor rate performance of hard carbon materials prepared from resin in the prior art, this invention provides a method for preparing resin-based hard carbon anode materials. This method introduces a phosphorus dopant during the preparation process. By introducing phosphorus through the phosphorus dopant, and utilizing the large atomic radius of phosphorus, the interlayer spacing of the phosphorus-doped hard carbon is increased, which is beneficial to improving the rate performance of hard carbon and solves the problem of poor rate performance of hard carbon materials prepared from resin in the prior art.
[0005] The technical solution adopted by this invention to solve its technical problem is:
[0006] A method for preparing a resin-based hard carbon anode material includes the following steps:
[0007] S1: After pulverizing the resin material, heat it to 290℃-300℃ and keep it at that temperature to obtain the pre-oxidized resin material;
[0008] S2: Mix the pre-oxidized resin material with a phosphorus dopant to obtain a hard carbon precursor;
[0009] S3: Under an inert gas atmosphere, the hard carbon precursor is heated to 1200℃-1600℃ for carbonization to obtain a resin-based hard carbon anode material.
[0010] Optionally, during step S1, the temperature is increased to 290℃-300℃ at a heating rate of 2-8℃ / min.
[0011] Optionally, the resin material is selected from at least one of epoxy resin, phenolic resin, polycarbonate, polyurethane, polyvinyl chloride, polyethylene, polypropylene, ABS, furan resin, furfural resin, bismaleimide resin, and polyimide resin.
[0012] Optionally, the mass ratio of the pre-oxidized resin material to the phosphorus dopant ranges from (5-500):1.
[0013] Optionally, the phosphorus dopant is a mixture of phosphate esters and phosphates.
[0014] Optionally, the mass ratio of the phosphate ester to the phosphate in the phosphorus dopant is (10:1) to (1:10).
[0015] Optionally, the phosphate ester is selected from at least one of butyltriphenyl phosphate, toluenediphenyl phosphate, diethylhexyl diphenyl phosphate, tricresyl phosphate, tri(diethylhexyl) phosphate, triphenyl phosphate, N,N-hydroxyethylaminoethane phosphate, dimethylpropane phosphate, tri(2-chloroisopropyl) phosphate, triethyl phosphate, isopropylated triphenyl phosphate, and diethyl ethylphosphonate.
[0016] Optionally, the phosphate is selected from at least one of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, melamine phosphate, and ammonium polyphosphate.
[0017] Another object of the present invention is to provide a resin-based hard carbon anode material, which is prepared by the method described above for preparing resin-based hard carbon anode materials.
[0018] Another object of the present invention is to provide a sodium-ion battery comprising the resin-based hard carbon anode material as described above.
[0019] The beneficial effects of this invention are:
[0020] The method for preparing resin-based hard carbon anode material provided by the present invention introduces phosphorus dopant during the preparation process. On the one hand, the small gas molecules released by the phosphorus dopant during the high-temperature process are used to create pores and improve the sodium storage capacity of hard carbon. On the other hand, due to the large atomic radius of phosphorus atoms, the interlayer spacing of hard carbon increases after doping, which is beneficial to improving the rate performance of hard carbon. Attached Figure Description
[0021] The present invention will be further described below with reference to the accompanying drawings and embodiments.
[0022] Figure 1 These are the rate discharge performance test results of the coin cells prepared according to various embodiments and comparative examples of the present invention. Detailed Implementation
[0023] The present invention will now be described in further detail. The embodiments described below are exemplary and intended to explain the present invention, and should not be construed as limiting the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.
[0024] To address the problem of poor rate performance in hard carbon materials prepared from resins in existing technologies, this invention provides a method for preparing resin-based hard carbon anode materials, comprising the following steps:
[0025] S1: The resin material is pulverized, preferably to a particle size of 5-10 μm, and then heated to 290℃-300℃, preferably at a heating rate of 2-8℃ / min, and held at that temperature for 1-3 hours to obtain the pre-oxidized resin material; the pre-oxidation process is carried out in air or oxygen atmosphere.
[0026] The pre-oxidation process can adjust the microstructure of the resin material, making the subsequent phosphorus doping process more targeted and helping to improve the rate performance of the hard carbon anode material.
[0027] S2: The pre-oxidized resin material is mixed with phosphorus dopant. The mixing method can be dry mixing such as ball milling or canning, or wet mixing. Wet mixing is preferred. The wet mixing process involves first sand milling with water or organic solvent as the milling medium, linear velocity 0-25 m / s, and filling rate 0-90%, followed by spray drying with inlet air temperature 90-200℃, outlet air temperature 80-160℃, and outlet particle size 5-10 μm to obtain hard carbon precursor.
[0028] S3: Under an inert gas atmosphere, the hard carbon precursor is heated to 1200℃-1600℃ for carbonization, preferably at a heating rate of 1-3℃ / min to 1200℃-1600℃, and preferably for a carbonization time of 2-5h, to obtain a resin-based hard carbon anode material.
[0029] The method for preparing resin-based hard carbon anode material provided by the present invention introduces phosphorus dopant during the preparation process. On the one hand, the small gas molecules released by the phosphorus dopant during the high-temperature process are used to create pores and improve the sodium storage capacity of hard carbon. On the other hand, due to the large atomic radius of phosphorus atoms (0.110 nm), the interlayer spacing of hard carbon increases after doping, which is beneficial to improving the rate performance of hard carbon.
[0030] Furthermore, the present invention pre-oxidizes the resin material before mixing it with the phosphorus dopant and carbonizing it. This pre-oxidation process can adjust the microstructure of the resin material and remove some of the undesirable substances in the resin material through oxidation, making the subsequent phosphorus doping process more targeted and thus helping to improve the electrochemical performance of the material.
[0031] The preferred resin material of this invention is selected from at least one of epoxy resin, phenolic resin, polycarbonate, polyurethane, polyvinyl chloride, polyethylene, polypropylene, ABS, furan resin, furfural resin, bismaleimide resin, and polyimide resin.
[0032] It should be noted that the resins used in this invention are all cured resins.
[0033] To balance the capacity and rate performance of resin-based hard carbon anode materials, the present invention preferably uses a mass ratio of pre-oxidized resin material to phosphorus dopant in the range of (5-500):1.
[0034] To ensure the rate performance of the resin-based hard carbon anode material, the present invention preferably uses a mixture of phosphate ester and phosphate as the phosphorus dopant.
[0035] A mixture of phosphate esters and phosphates is used as a phosphorus dopant. The small gas molecules released during the high-temperature process of phosphate esters and / or phosphates create pores, enhancing the sodium storage capacity of hard carbon. The plasticizing effect of phosphate esters reduces the surface hardness of the dopant and precursor, which helps improve the dispersibility of the dopant, promotes the embedding of the dopant into the interlayer of hard carbon, expands the interlayer spacing, and improves rate performance. Combined with the process step of pre-oxidizing the resin material before mixing and carbonizing it with the phosphorus dopant, the pore structure of the material changes and the pore volume increases as small gas molecules such as CO and CO2 escape during the pre-oxidation process, which is conducive to the dopant entering the pore structure and embedding into the interlayer.
[0036] Furthermore, the present invention preferably uses a mass ratio of phosphate ester to phosphate in the phosphorus dopant of (10:1) to (1:10).
[0037] Specifically, the phosphate esters of the present invention are preferably selected from at least one of butyltriphenyl phosphate, toluene diphenyl phosphate, diethylhexyl diphenyl phosphate, tricresyl phosphate, tricresyl phosphate, tri(diethylhexyl) phosphate, triphenyl phosphate, N,N-hydroxyethylaminoethane phosphate, dimethyl propane phosphate, tri(2-chloroisopropyl) phosphate, triethyl phosphate, isopropylated triphenyl phosphate, and diethyl ethylphosphonate; the phosphates are preferably selected from at least one of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, melamine phosphate, and ammonium polyphosphate.
[0038] Phosphate esters and phosphates can be mixed by wet mixing, specifically by mixing with an aqueous solution.
[0039] Another object of the present invention is to provide a resin-based hard carbon anode material, which is prepared by the method described above for preparing resin-based hard carbon anode materials.
[0040] The resin-based hard carbon anode material provided by this invention introduces phosphorus dopant during the preparation process. On the one hand, it utilizes the small gas molecules released by the phosphorus dopant during the high-temperature process to create pores and improve the sodium storage capacity of hard carbon. On the other hand, due to the large atomic radius of phosphorus atoms (0.110 nm), the interlayer spacing of hard carbon increases after doping, which is beneficial to improving the rate performance of hard carbon.
[0041] Another object of the present invention is to provide a sodium-ion battery comprising the resin-based hard carbon anode material as described above.
[0042] The sodium-ion battery provided by this invention introduces phosphorus dopant during the preparation of resin-based hard carbon anode material. On the one hand, the small gas molecules released by the phosphorus dopant during the high-temperature process are used to create pores, thereby improving the sodium storage capacity of the hard carbon. On the other hand, due to the large atomic radius of phosphorus atoms (0.110 nm), the interlayer spacing of the hard carbon increases after doping, which is beneficial to improving the rate performance of the hard carbon, thereby improving the rate performance of the sodium-ion battery.
[0043] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below.
[0044] Example 1
[0045] This embodiment provides a method for preparing a resin-based hard carbon anode material, which includes the following steps:
[0046] S1: Phenolic resin material is pulverized to a particle size of 7μm, and then heated to 295℃ in air at a heating rate of 5℃ / min and held for 2h to obtain pre-oxidized resin material.
[0047] S2: Toluene diphenyl phosphate and diammonium hydrogen phosphate are mixed evenly at a mass ratio of 1:1 to obtain a phosphorus dopant; the pre-oxidized resin material is mixed with the phosphorus dopant at a mass ratio of 250:1. The mixing method is wet mixing. The wet mixing process is as follows: first, sand milling is carried out with water as the milling medium, the linear velocity is 15m / s, the filling rate is 50%, and then spray drying is carried out with an inlet air temperature of 150℃ and an outlet air temperature of 100℃, and the output particle size is 8μm to obtain a hard carbon precursor.
[0048] S3: Under a nitrogen atmosphere, the hard carbon precursor is heated to 1400℃ at a heating rate of 2℃ / min for 4 hours to obtain a resin-based hard carbon anode material.
[0049] Example 2
[0050] This embodiment provides a method for preparing a resin-based hard carbon anode material, which includes the following steps:
[0051] S1: After pulverizing the epoxy resin material to a particle size of 7μm, heat it to 290℃ in air at a heating rate of 2℃ / min and hold it for 3h to obtain the pre-oxidized resin material.
[0052] S2: Butyltriphenyl phosphate and sodium dihydrogen phosphate are mixed evenly at a mass ratio of 1:10 to obtain a phosphorus dopant; the pre-oxidized resin material is mixed with the phosphorus dopant at a mass ratio of 80:1. The mixing method is wet mixing. The wet mixing process is as follows: first, sand milling is carried out with water as the milling medium, the linear velocity is 15m / s, the filling rate is 50%, and then spray drying is carried out with an inlet air temperature of 150℃ and an outlet air temperature of 100℃, and the output particle size is 8μm to obtain a hard carbon precursor.
[0053] S3: Under a nitrogen atmosphere, the hard carbon precursor is heated to 1200℃ at a heating rate of 1℃ / min for 5h to obtain a resin-based hard carbon anode material.
[0054] Example 3
[0055] This embodiment provides a method for preparing a resin-based hard carbon anode material, which includes the following steps:
[0056] S1: After pulverizing the epoxy resin material to a particle size of 7μm, heat it to 300℃ in air at a heating rate of 8℃ / min and hold it for 1h to obtain the pre-oxidized resin material.
[0057] S2: Trimethylbenzene phosphate and sodium dihydrogen phosphate are mixed evenly at a mass ratio of 10:1 to obtain a phosphorus dopant; the pre-oxidized resin material is mixed with the phosphorus dopant at a mass ratio of 500:1. The mixing method is wet mixing, which involves sand milling with water as the milling medium, a linear velocity of 15 m / s, and a filling rate of 50%, followed by spray drying with an inlet air temperature of 150℃ and an outlet air temperature of 100℃, resulting in an outlet particle size of 8 μm to obtain a hard carbon precursor.
[0058] S3: Under a nitrogen atmosphere, the hard carbon precursor is heated to 1600℃ at a heating rate of 3℃ / min for 2 hours to obtain a resin-based hard carbon anode material.
[0059] Comparative Example 1
[0060] This comparative example provides a method for preparing a resin-based hard carbon anode material, which includes the following steps:
[0061] S1: Phenolic resin material is pulverized to a particle size of 7μm, and then heated to 295℃ in air at a heating rate of 5℃ / min and held for 2h to obtain pre-oxidized resin material.
[0062] S2: Under a nitrogen atmosphere, the pre-oxidized resin material is heated to 1400℃ at a heating rate of 2℃ / min for carbonization for 4 hours to obtain a resin-based hard carbon anode material.
[0063] Comparative Example 2
[0064] This comparative example provides a method for preparing a resin-based hard carbon anode material, which includes the following steps:
[0065] S1: Phenolic resin material is pulverized to a particle size of 7μm, and then heated to 295℃ in air at a heating rate of 5℃ / min and held for 2h to obtain pre-oxidized resin material.
[0066] S2: The pre-oxidized resin material is mixed with toluene diphenyl phosphate at a mass ratio of 250:1. The mixing method is wet mixing. The wet mixing process is first sand milling with water as the milling medium, a linear velocity of 15m / s, and a filling rate of 50%. Then, spray drying is performed with an inlet air temperature of 150℃ and an outlet air temperature of 100℃. The output particle size is 8μm to obtain the hard carbon precursor.
[0067] S3: Under a nitrogen atmosphere, the hard carbon precursor is heated to 1400℃ at a heating rate of 2℃ / min for 4 hours to obtain a resin-based hard carbon anode material.
[0068] Comparative Example 3
[0069] This comparative example provides a method for preparing a resin-based hard carbon anode material, which includes the following steps:
[0070] S1: Phenolic resin material is pulverized to a particle size of 7μm, and then heated to 295℃ in air at a heating rate of 5℃ / min and held for 2h to obtain pre-oxidized resin material.
[0071] S2: The pre-oxidized resin material is mixed with diammonium hydrogen phosphate at a mass ratio of 250:1. The mixing method is wet mixing. The wet mixing process is first sand milling with water as the milling medium, a linear speed of 15m / s, and a filling rate of 50%. Then, spray drying is performed with an inlet air temperature of 150℃ and an outlet air temperature of 100℃. The output particle size is 8μm to obtain the hard carbon precursor.
[0072] S3: Under a nitrogen atmosphere, the hard carbon precursor is heated to 1400℃ at a heating rate of 2℃ / min for 4 hours to obtain a resin-based hard carbon anode material.
[0073] Comparative Example 4
[0074] This comparative example provides a method for preparing a resin-based hard carbon anode material, which includes the following steps:
[0075] S1: Phenolic resin material is pulverized to a particle size of 7μm to obtain resin material;
[0076] S2: Toluene diphenyl phosphate and diammonium hydrogen phosphate are mixed evenly at a mass ratio of 1:1 to obtain a phosphorus dopant; the resin material and phosphorus dopant are mixed at a mass ratio of 250:1 by wet mixing. The wet mixing process involves first sand milling with water as the milling medium at a linear velocity of 15 m / s and a filling rate of 50%, followed by spray drying at an inlet air temperature of 150℃ and an outlet air temperature of 100℃, resulting in an outlet particle size of 8 μm to obtain a mixture.
[0077] S3: The mixture is heated to 295°C in air at a heating rate of 5°C / min and held for 2 hours to obtain a hard carbon precursor.
[0078] S4: Under a nitrogen atmosphere, the hard carbon precursor was heated to 1400℃ at a heating rate of 2℃ / min for 4 hours to obtain a resin-based hard carbon anode material.
[0079] The performance of the negative electrode materials prepared in the above embodiments and comparative examples was evaluated using coin cells. The electrode slurry was prepared with a ratio of active material: conductive agent SP: binder CMC: dispersant SBR = 92:3.0:1.5:3.5. Appropriate amounts of ethanol and water were added to prepare the slurry, which was then coated to a thickness of 200 μm. After drying and pressing, the slurry was formed into an electrode sheet. Using sodium metal as the counter electrode, a 1 mol / L NaPF6 DEC / EC (1:1) solution as the electrolyte, and a glass fiber filter paper membrane GF / C as the separator, a 2032 coin cell was assembled. The electrode was tested at 0.1 A g. -1 Its charge-discharge performance was tested at a current density, and the test results are shown in Table 1. Figure 1 As shown.
[0080] The test results are shown in Table 1:
[0081] Table 1
[0082]
[0083]
[0084] Combining the above data and Figure 1 It can be seen that the resin-based hard carbon anode materials prepared in the various embodiments of the present invention have excellent electrochemical performance.
[0085] The difference between Comparative Example 1 and Example 1 is that no phosphorus dopant was added during the preparation process, and the specific capacity, first efficiency, and rate discharge performance of the prepared resin-based hard carbon anode material were significantly reduced.
[0086] The difference between Comparative Example 2 and Example 1 is that only phosphate esters were used as phosphorus dopants in the preparation process. The difference between Comparative Example 3 and Example 1 is that only phosphates were used as phosphorus dopants in the preparation process. The electrochemical performance of the resin-based hard carbon anode materials prepared by both examples is improved compared with Comparative Example 1, but there is still a gap between them and the performance of Example 1.
[0087] The difference between Comparative Example 4 and Example 1 is that the biomass material was mixed with phosphorus dopant and then pre-oxidized during the preparation process. The electrochemical performance of the prepared resin-based hard carbon anode material was still worse than that of Example 1.
[0088] Based on the above-described preferred embodiments of the present invention, and through the foregoing description, those skilled in the art can make various changes and modifications without departing from the inventive concept. The technical scope of this invention is not limited to the contents of the specification, but must be determined according to the scope of the claims.
Claims
1. A method for preparing a resin-based hard carbon anode material, characterized in that, Includes the following steps: S1: After pulverizing the resin material, heat it to 290℃-300℃ and keep it at that temperature to obtain the pre-oxidized resin material; S2: Mix the pre-oxidized resin material with a phosphorus dopant to obtain a hard carbon precursor; S3: Under an inert gas atmosphere, the hard carbon precursor is heated to 1200℃-1600℃ for carbonization to obtain a resin-based hard carbon anode material. The phosphorus dopant is a mixture of phosphate ester and phosphate. The mass ratio of the phosphate ester to the phosphate salt is (10:1)-(1:10); The phosphate ester is selected from at least one of butyltriphenyl phosphate, toluenediphenyl phosphate, diethylhexyl diphenyl phosphate, tricresyl phosphate, tri(diethylhexyl) phosphate, triphenyl phosphate, N,N-hydroxyethylaminoethane phosphate, dimethylpropane phosphate, tri(2-chloroisopropyl) phosphate, triethyl phosphate, isopropylated triphenyl phosphate, and diethyl ethylphosphonate. The phosphate is selected from at least one of diammonium hydrogen phosphate, ammonium dihydrogen phosphate, sodium dihydrogen phosphate, disodium hydrogen phosphate, sodium phosphate, melamine phosphate, and ammonium polyphosphate.
2. The method for preparing the resin-based hard carbon anode material as described in claim 1, characterized in that, During step S1, the temperature is increased to 290℃-300℃ at a rate of 2-8℃ / min.
3. The method for preparing the resin-based hard carbon anode material as described in claim 1, characterized in that, The resin material is selected from at least one of epoxy resin, phenolic resin, polycarbonate, polyurethane, polyvinyl chloride, polyethylene, polypropylene, ABS, furan resin, furfural resin, bismaleimide resin, and polyimide resin.
4. The method for preparing the resin-based hard carbon anode material as described in claim 1, characterized in that, The mass ratio of the pre-oxidized resin material to the phosphorus dopant ranges from (5-500):
1.
5. A resin-based hard carbon anode material, characterized in that, The resin-based hard carbon anode material is prepared by the method described in any one of claims 1-4.
6. A sodium-ion battery, characterized in that, Including the resin-based hard carbon anode material as described in claim 5.
Citation Information
Patent Citations
Soft carbon coated phosphorus / sodium co-doped hard carbon sodium ion battery negative electrode material and preparation method thereof
CN118315549A