Preparation method of high-first-effect nano blocky sodium ion battery negative electrode biomass hard carbon

Through pre-treatment, pickling, pre-carbonization, oxidation and hydrothermal carbonization processes, nano-block hard carbon materials are prepared, which solves the problems of low Coulombic efficiency and poor morphology uniformity in sodium-ion batteries for the first time, and achieves high energy density and Cycle stability, suitable for large-scale production.

CN118754099APending Publication Date: 2024-10-11JIANGSU UNIV OF TECH

Patent Information

Application Number
CN202410979875.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, biomass hard carbon materials in sodium-ion batteries suffer from low coulombic efficiency, low reversible sodium storage capacity, and poor morphology uniformity, which results in limited energy density improvement, complex processes, high energy consumption, and high pollution.

Method used

Using pre-treatment, pickling, pre-carbonization, oxidation and hydrothermal carbonization processes, nano-massive hard carbon materials are obtained through high-temperature final carbonization to optimize their structure and conductive properties.

Benefits of technology

It achieves high first Coulombic efficiency and high reversible sodium storage capacity, reduces the specific surface area and oxygen content, improves conductivity and morphology uniformity, is suitable for large-scale production, and significantly improves the energy density and cycle stability of sodium-ion batteries. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754099A_ABST
    Figure CN118754099A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of high-first-effect nano blocky sodium ion battery negative electrode biomass hard carbon. The preparation method comprises the following steps: pretreating a biomass raw material; carrying out acid pickling on the pretreated biomass raw material; carrying out pre-carbonization under the protection of an inert atmosphere; an oxidizing agent is added for oxidation after pre-carbonization; carrying out hydrothermal carbonization reaction on the biomass carbon material obtained by oxidation; and finally, carrying out high-temperature final carbonization treatment under the protection of an inert atmosphere. The biomass hard carbon material prepared by the method has a nano blocky structure, and has the characteristics of small specific surface area, large interlayer spacing, rich closed pores and the like. The prepared hard carbon shows excellent sodium storage performance, can well solve the technical problems of low first coulombic efficiency, low reversible sodium storage capacity and poor cycling stability of the current sodium ion battery negative electrode, and when the hard carbon is used as the sodium ion battery negative electrode material, the reversible specific capacity of the battery can reach 393.52 mAh / g under the current density of 50mA / g, and the reversible specific capacity of the battery can reach 393.52 mAh / g under the current density of 50mA / g. And the first effect reaches 90% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to a method for preparing a biomass hard carbon material with a high first-efficiency nano-block morphology and an application thereof in a negative electrode for sodium ion batteries. Background Art

[0002] With the popularity of new energy electric vehicles, smart phones and other portable electronic devices, the demand for high energy density, long cycle life and fast charge and discharge speed is increasing. Carbon materials, as an important negative electrode material, play a key role in electrochemical energy storage devices such as lithium-ion batteries. However, limited lithium resources, unbalanced distribution and high cost are not conducive to its large-scale application in the field of energy storage. However, sodium-ion batteries are considered to be a candidate material for grid energy storage systems with great development potential due to their high abundance, low cost, chemical and physical properties similar to lithium, and the wide distribution of sodium resources around the world. As a substitute for graphite, hard carbon has received widespread attention as a negative electrode material for sodium-ion batteries due to its good economic feasibility, high sodium ion absorption rate and good long-term stability.

[0003] Hard carbon materials have rich porous structures and high specific surface areas, which can increase the adsorption and diffusion rate of sodium ions on their surfaces, thereby increasing the charge and discharge speed and cycle life of the battery. In addition, hard carbon also has a high specific capacity and low cost, making it one of the new negative electrode materials that has attracted much attention. Hard carbon negative electrode materials are mostly obtained by carbonization using resin or biomass as a precursor carbon source, but the resin raw materials are expensive and do not meet the expectations of low cost for sodium ion batteries. The carbon structure in hard carbon materials prepared using biomass as a precursor is usually complex, containing rich heteroatoms and defect structures, resulting in relatively weak electrical conductivity. This may affect the conductivity of the electrode, reduce the output power and charging speed of the battery, and is not conducive to the improvement of energy density.

[0004] For example, in the prior art, CN201610966202.0 discloses a method for preparing a biomass hard carbon negative electrode material for a sodium ion battery, wherein the biomass raw material is crushed and then pre-burned and calcined in sequence to obtain a precursor carbon material, and then soaked in alkaline solution and acid solution to remove impurities and wash, and then microwave vacuum activated to obtain a biomass hard carbon negative electrode material, wherein the biomass raw material includes pine cones, coconut fruit, walnut shells, wheat straw, rice husks, blue algae, bean dregs, banana peels, cotton, asphalt, peat, seaweed, and cotton shells, and the first charge and discharge efficiency reaches 90%, and has stable cycle performance. However, the reversible capacity of the hard carbon material is only 300mAh / g, and the prepared hard carbon particles are too large, the accumulation and aggregation phenomenon is heavy, and the morphology uniformity is poor.

[0005] For example, in the prior art, CN202110783054.X discloses a nitrogen-doped hard carbon material and its preparation method and application. A nitrogen-doped hard carbon material with porous properties is obtained through primary purification, secondary purification, calcination, plasma treatment and other processes. The biomass raw materials include grapefruit peel, durian shell, coconut shell, almond, corn cob, shrimp shell, onion, soybean, mushroom, orchid leaf. The hard carbon has the characteristics of large interlayer spacing, high porosity, and large specific surface area. However, the first effect is not good. Excessive specific surface area will cause the formation of an undesirable solid electrolyte interface film (SEI). The morphology uniformity of the hard carbon material is also poor, and the process is complicated, requiring high-energy consumption and high-pollution ammonia plasma doping.

[0006] Therefore, how to effectively improve the hard carbon materials prepared with biomass as the precursor carbon source is an effective way to reduce the cost of sodium-ion batteries while ensuring the energy density of sodium-ion batteries. Summary of the invention

[0007] The object of the present invention is to provide a method for preparing a high-initial-efficiency nano-block sodium ion battery negative electrode biomass hard carbon to solve the above-mentioned defects caused by the prior art.

[0008] A method for preparing high-initial-efficiency nano-block sodium-ion battery negative electrode biomass hard carbon comprises the following specific steps:

[0009] S1: Pre-treat the biomass raw materials: soak the biomass raw materials in a solvent for 4-6 hours, transfer them to an oven, dry them at 60-120°C for 8-12 hours, and then crush them after drying.

[0010] Preferably, the solvent used for pretreatment of the biomass raw material in S1 includes one or more of deionized water, methanol, ethanol, isopropanol, and ethyl acetate. The mass volume ratio of the biomass to the solvent is 0.01-0.1 g / mL.

[0011] After soaking for a period of time, ash, pesticides and other impurities on the surface of the biomass can be removed, and the solvent molecules can fully infiltrate the biomass, providing a prerequisite for the formation of nano-spherical carbon materials.

[0012] S2: Acid washing: Add the product obtained in S1 into deionized water, then add dilute acid aqueous solution for washing, stir at room temperature for 4-8 hours, then wash with deionized water again, and dry.

[0013] Preferably, the dilute acid in S2 is one or more of hydrochloric acid, sulfuric acid, nitric acid, formic acid, and acetic acid, and the concentration is 1-6 M. The mass volume ratio of the product obtained in S1 to the deionized water is 0.01-0.1 g / mL.

[0014] After pickling, the ash, inorganic salts and other impurities in the biomass can be fully removed, providing a prerequisite for the preparation of pure hard carbon materials.

[0015] S3: Pre-carbonization: Place the product obtained in S2 in a tubular furnace, and under the protection of inert gas, heat it to 300-500°C at 3-10°C / min, calcine it at 300-500°C for 2-4 hours, and cool it naturally to room temperature.

[0016] Preferably, the inert gas in S3 is one or more of air, nitrogen, argon and hydrogen, and the calcination temperature is 300-500°C.

[0017] Pre-carbonization under these conditions can cause the organic matter in the biomass to undergo a carbonization reaction to form a carbonaceous structure, which can enable the negative electrode material to obtain higher conductivity, better mechanical stability, and improve the interface stability between it and the electrolyte.

[0018] S4: Oxidation: Add the pre-carbonized product obtained in S3 to deionized water, then add an oxidant, ultrasonicate for 30 minutes, stir and react at 60-120°C for 4-8 hours, cool to room temperature, then add to deionized water for dilution, wash to remove the oxidant, centrifuge and dry at 60-120°C for 8-12 hours.

[0019] Preferably, the mass volume ratio of the pre-carbonized product obtained in S3 to the deionized water is 0.02-0.2 g / mL, and the mass ratio of the pre-carbonized product to the oxidant is 1:(1-5). The oxidant in S4 is one or more of nitric acid, hydrogen peroxide, potassium permanganate, and ammonium persulfate.

[0020] This oxidation can produce a large number of oxygen-containing functional groups for the pre-carbonization product, enhance the cross-linking effect between molecules, optimize the structural order of hard carbon materials, reduce some irreversible defects, and at the same time expand the interlayer spacing, providing a prerequisite for the efficient storage of sodium ions.

[0021] S5: Hydrothermal carbonization: Add the oxidation product obtained in S4, dispersant and sulfuric acid into a certain amount of solvent, and then perform magnetic stirring at room temperature. After stirring, perform ultrasonication for 10-40 minutes, and then transfer to an autoclave to react for 8-12 hours. After the reaction is completed, cool to room temperature, centrifuge, wash and dry.

[0022] Preferably, the mass ratio of the oxidation product obtained in S4 to the dispersant is 1:(0.01-0.2), and the concentration of sulfuric acid is 1-6 M. The mass volume ratio of the oxidation product to the solvent is 0.05-0.5 g / mL, the dispersant is one or more of hexadecyltrimethylammonium bromide, sodium dodecyl sulfate, and ammonium dodecyl sulfate, the oxidant is one or more of nitric acid, hydrogen peroxide, potassium permanganate, and ammonium persulfate, the solvent is one or more of deionized water, methanol, ethanol, isopropanol, and N,N-dimethylformamide, and the reaction temperature of the autoclave is 120-200°C.

[0023] The addition of dispersant can effectively disperse the oxidation products and inhibit the stacking and aggregation behavior between the products. The addition of sulfuric acid can further remove moisture and oxygen-containing functional groups in the products. In a high temperature and high pressure environment, the oxidation products obtained by S4 undergo dehydration and carbonization, effectively forming a spherical nanostructure.

[0024] S6: Final carbonization: The hydrothermal carbonization product obtained in S5 is placed in a tubular furnace, and under the protection of inert gas, the temperature is raised to 1000-1600°C at 3-10°C / min, and high-temperature calcination is performed for 2-4 hours, and then naturally cooled to room temperature to obtain a nano-block biomass hard carbon negative electrode material.

[0025] Preferably, the inert gas is one or more of air, nitrogen, argon and hydrogen, and the calcination temperature is 1000-1600°C.

[0026] At this high temperature, the biomass molecules begin to vibrate more strongly, and the chemical bonds within the molecules break, forming smaller molecules and ions. These molecules and ions further undergo thermal decomposition reactions at high temperatures, eventually forming hard carbon.

[0027] The hard carbon material prepared by this method presents a nano-spherical structure, has fewer defects, porosity, lower oxygen content and lower specific surface area, and has higher electronic conductivity.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] 1. Biomass as a precursor for synthetic hard carbon has the advantages of wide sources, renewable, low price, green and pollution-free, simple process, and easy large-scale production. This process is simple to operate, has good repeatability, and is suitable for large-scale preparation. Nano-spherical hard carbon can be prepared through simple pretreatment, pickling, pre-carbonization, oxidation, hydrothermal carbonization and final carbonization, and the nano-structure can be achieved without further crushing and granulation.

[0030] 2. The nano-block hard carbon prepared by this method has a large interlayer spacing of 0.38-0.42nm and a low specific surface area, all less than 10m 2 / g; has abundant interlaced short-range ordered carbon layers and closed pores. These structural features make the hard carbon prepared by this method have a high sodium storage capacity and a high first coulombic efficiency.

[0031] 3. The prepared hard carbon negative electrode material was made into an electrode as a negative electrode material for sodium ion batteries. The sodium ion batteries were assembled according to the structure of CR2032 standard button cells. The batteries were charged and discharged at a current density of 50 mA / g on a battery test platform. The initial specific capacity reached 393.52 mAh / g, and the first coulombic efficiency reached 90.48%. It has good slope capacity and platform capacity, surpassing most of the reported hard carbon materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The process flow chart of the method for preparing biomass hard carbon in the present invention.

[0033] Figure 2 This is a scanning electron microscope image of the grapefruit peel biomass hard carbon prepared in Example 1.

[0034] Figure 3 This is a scanning electron microscope image of litchi shell biomass hard carbon prepared in Example 2.

[0035] Figure 4 This is a scanning electron microscope image of the peanut shell biomass hard carbon prepared in Example 3.

[0036] Figure 5 This is a scanning electron microscope image of coconut shell biomass hard carbon prepared in Example 4.

[0037] Figure 6 This is a high-magnification transmission electron microscopy image of the litchi shell biomass hard carbon prepared in Example 2.

[0038] Figure 7 This is a high-magnification transmission electron microscopy image of the peanut shell biomass hard carbon prepared in Example 3.

[0039] Figure 8 This is the first cycle charge and discharge curve of a sodium battery assembled with litchi shell biomass hard carbon prepared in Example 2 as the negative electrode.

[0040] Fig. 9 This is the first cycle charge and discharge curve of the sodium battery assembled with the peanut shell biomass hard carbon prepared in Example 3 as the negative electrode. DETAILED DESCRIPTION

[0041] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0042] Example 1: This example prepares a grapefruit peel biomass hard carbon negative electrode material, and the reaction steps are as follows:

[0043] (1) Pretreatment of biomass raw materials

[0044] Grapefruit peel (50 g) was soaked in deionized water (5000 mL) for 4 hours, then transferred to an oven and dried at 60° C. for 8 hours, and then crushed after drying.

[0045] (2) Pickling

[0046] The product (20 g) of step (1) was added to a 1 M aqueous solution of dilute hydrochloric acid (2000 mL) for washing, stirred at room temperature for 4 hours, centrifuged, then washed with deionized water and dried.

[0047] (3) Pre-carbonization

[0048] Under nitrogen protection, the above product (15 g) was placed in a quartz boat, placed in a tube furnace, and heated to 300° C. at 3° C. / min and calcined at 300° C. for 2 hours, and then naturally cooled to room temperature.

[0049] (4) Oxidation

[0050] The above product (5 g) was added to deionized water (250 mL), and then concentrated nitric acid (5 g) was added, ultrasonicated for 30 minutes, stirred at 60°C for 4 hours, cooled to room temperature, and then added to deionized water for dilution and washing to remove the oxidant. After centrifugation, it was dried at 70°C for 10 hours.

[0051] (5) Hydrothermal carbonization

[0052] The above product (5 g) was mixed with hexadecyltrimethylammonium bromide (0.05 g), added to deionized water (100 mL) and magnetically stirred, and then 1 M sulfuric acid (25 mL) was added. After stirring, the mixture was ultrasonicated for 15 minutes and then transferred to an autoclave to react at 120° C. for 8 hours. After the reaction was completed, it was cooled to room temperature, centrifuged, washed and dried.

[0053] (6) Final carbonization

[0054] Under nitrogen gas protection, the above product (4 g) was placed in a quartz boat, placed in a tube furnace, and the temperature was raised to 1000°C at 3°C / min and calcined at 1000°C for 2 hours. The mixture was naturally cooled to room temperature to obtain a grapefruit peel biomass hard carbon negative electrode material.

[0055] Example 2: In this example, a litchi shell biomass hard carbon negative electrode material is prepared, and the reaction steps are as follows:

[0056] (1) Pretreatment of biomass raw materials

[0057] Litchi shell (50 g) was soaked in methanol (2500 mL) for 5 hours, then transferred to an oven and dried at 80° C. for 10 hours, and then crushed after drying.

[0058] (2) Pickling

[0059] The product (20 g) of step (1) above was added to a 2 M aqueous solution of dilute sulfuric acid (1000 mL) for washing, stirred at room temperature for 6 hours, centrifuged, then washed with deionized water and dried.

[0060] (3) Pre-carbonization

[0061] Under nitrogen protection, the above product (15 g) was placed in a quartz boat, placed in a tube furnace, and the temperature was raised to 350° C. at 5° C. / min and calcined at 350° C. for 3 hours, and then naturally cooled to room temperature.

[0062] (4) Oxidation

[0063] The above product (5 g) was added to deionized water (100 mL), and then hydrogen peroxide (10 g) was added, ultrasonicated for 30 minutes, stirred at 80°C for 6 hours, cooled to room temperature, and then added to deionized water for dilution and washing to remove the oxidant. After centrifugation, it was dried at 70°C for 10 hours.

[0064] (5) Hydrothermal carbonization

[0065] The above product (5 g) was mixed with sodium dodecyl sulfate (0.1 g) and added to methanol (50 mL) for magnetic stirring. Then 2 M sulfuric acid (10 mL) was added. After stirring, ultrasonication was performed for 15 minutes. Then, the mixture was transferred to an autoclave and reacted at 140° C. for 10 hours. After the reaction was completed, it was cooled to room temperature, centrifuged, washed, and dried.

[0066] (6) Final carbonization

[0067] Under nitrogen gas protection, the above product (4 g) was placed in a quartz boat, placed in a tubular furnace, and the temperature was raised to 1200°C at 5°C / min and calcined at 1200°C for 3 hours. The mixture was naturally cooled to room temperature to obtain a lychee shell biomass hard carbon negative electrode material.

[0068] Example 3: This example prepares a peanut shell biomass hard carbon negative electrode material, and the reaction steps are as follows:

[0069] (1) Pretreatment of biomass raw materials

[0070] Peanut shells (50 g) were soaked in ethanol (1000 mL) for 6 hours, then transferred to an oven and dried at 100° C. for 12 hours. After drying, the peanut shells were crushed.

[0071] (2) Pickling

[0072] The product (20 g) of step (1) above was added to a 3 M dilute nitric acid aqueous solution (400 mL) for washing, stirred at room temperature for 8 hours, centrifuged, then washed with deionized water and dried.

[0073] (3) Pre-carbonization

[0074] Under nitrogen protection, the above product (15 g) was placed in a quartz boat, placed in a tube furnace, and heated to 400° C. at 8° C. / min and calcined at 400° C. for 4 hours, and then naturally cooled to room temperature.

[0075] (4) Oxidation

[0076] The above product (5 g) was added to deionized water (50 mL), and then potassium permanganate (15 g) was added, ultrasonicated for 30 minutes, stirred at 100°C for 8 hours, cooled to room temperature, and then added to deionized water for dilution and washing to remove the oxidant. After centrifugation, it was dried at 70°C for 10 hours.

[0077] (5) Hydrothermal carbonization

[0078] The above product (5 g) was mixed with ammonium dodecyl sulfate (0.5 g) and added to ethanol (25 mL) for magnetic stirring. Then 4 M sulfuric acid (10 mL) was added. After stirring, the mixture was ultrasonicated for 15 minutes and then transferred to an autoclave for reaction at 160° C. for 12 hours. After the reaction was completed, the mixture was cooled to room temperature, centrifuged, washed and dried.

[0079] (6) Final carbonization

[0080] Under argon gas protection, the above product (4 g) was placed in a quartz boat, placed in a tubular furnace, and the temperature was raised to 1500°C at 10°C / min and calcined at 1500°C for 3 hours. It was naturally cooled to room temperature to obtain a peanut shell biomass hard carbon negative electrode material.

[0081] Example 4: This example prepares a coconut shell biomass hard carbon negative electrode material, and the reaction steps are as follows:

[0082] (1) Pretreatment of biomass raw materials

[0083] Coconut shell (50 g) was soaked in ethanol (500 mL) for 5 hours, then transferred to an oven and dried at 120° C. for 12 hours, and then pulverized.

[0084] (2) Pickling

[0085] The product (20 g) of step (1) above was added to a 5 M aqueous formic acid solution (200 mL) for washing, stirred at room temperature for 6 hours, centrifuged, then washed with deionized water and dried.

[0086] (3) Pre-carbonization

[0087] Under nitrogen protection, the above product (15 g) was placed in a quartz boat, placed in a tube furnace, and heated to 500° C. at 5° C. / min and calcined at 500° C. for 3 hours, and then naturally cooled to room temperature.

[0088] (4) Oxidation

[0089] The above product (5 g) was added to deionized water (25 mL), and then ammonium persulfate (5 g) was added, ultrasonicated for 30 minutes, stirred at 120°C for 8 hours, cooled to room temperature, and then added to deionized water for dilution and washing to remove the oxidant. After centrifugation, it was dried at 70°C for 10 hours.

[0090] (5) Hydrothermal carbonization

[0091] The above product (5 g) was mixed with hexadecyltrimethylammonium bromide (1 g), added to isopropanol (10 mL) and magnetically stirred, and then 6 M sulfuric acid (10 mL) was added. After stirring, the mixture was ultrasonicated for 15 minutes and then transferred to an autoclave and reacted at 180° C. for 12 hours. After the reaction was completed, it was cooled to room temperature, centrifuged, washed and dried.

[0092] (6) Final carbonization

[0093] Under argon gas protection, the above product (4 g) was placed in a quartz boat, placed in a tube furnace, and the temperature was raised to 1600°C at 5°C / min and calcined at 1600°C for 4 hours, and then naturally cooled to room temperature to obtain a coconut shell biomass hard carbon negative electrode material.

[0094] Example 5: This example prepares a bamboo biomass hard carbon negative electrode material, and the reaction steps are as follows:

[0095] (1) Pretreatment of biomass raw materials

[0096] Moso bamboo (50 g) was soaked in ethyl acetate (1000 mL) for 6 hours, then transferred to an oven and dried at 120° C. for 12 hours, and then crushed after drying.

[0097] (2) Pickling

[0098] The product (20 g) of step (1) above was added to a 4 M dilute acetic acid aqueous solution (300 mL) for washing, stirred at room temperature for 8 hours, centrifuged, then washed with deionized water and dried.

[0099] (3) Pre-carbonization

[0100] Under nitrogen protection, the above product (15 g) was placed in a quartz boat, placed in a tube furnace, and the temperature was raised to 450° C. at 3° C. / min and calcined at 450° C. for 2 hours, and then naturally cooled to room temperature.

[0101] (4) Oxidation

[0102] The above product (5 g) was added to deionized water (50 mL), and then nitric acid (10 g) was added, ultrasonicated for 30 minutes, stirred at 120°C for 8 hours, cooled to room temperature, and then added to deionized water for dilution and washing to remove the oxidant. After centrifugation, it was dried at 70°C for 10 hours.

[0103] (5) Hydrothermal carbonization

[0104] The above product (5 g) was mixed with sodium dodecyl sulfate (0.5 g), added to N,N-dimethylformamide (20 mL) and magnetically stirred, and then 4 M sulfuric acid (10 mL) was added. After stirring, the mixture was ultrasonicated for 15 minutes and then transferred to an autoclave to react at 200° C. for 12 hours. After the reaction was completed, it was cooled to room temperature, centrifuged, washed, and dried.

[0105] (6) Final carbonization

[0106] Under argon gas protection, the above product (4 g) was placed in a quartz boat, placed in a tubular furnace, and the temperature was raised to 1600°C at 3°C / min and calcined at 1600°C for 2 hours. It was naturally cooled to room temperature to obtain a bamboo biomass hard carbon negative electrode material.

[0107] Example 6: Sodium ion batteries were prepared using the hard carbon negative electrode materials prepared in Examples 1-5 as negative electrode active materials, and the first coulombic efficiency of each battery was tested. The specific operation was as follows: the hard carbon negative electrode material was mixed with conductive carbon black and polyvinylidene fluoride in a mass ratio of 7:2:1, and N-methylpyrrolidone was added and mixed evenly to obtain a negative electrode slurry, which was coated on a copper foil to obtain a negative electrode sheet; a metal sodium sheet was used as a counter electrode, and NaClO4 was used as an electrolyte, and CR2032 button batteries were assembled in an argon glove box. The electrochemical performance of the prepared CR2032 button battery was tested using the Land battery test system. The specific test method was as follows: discharge to 0V at a current density of 50mA / g, and record the discharge capacity at this time as the first discharge capacity; then charge to 2.5V at a current density of 50mA / g, and record the charge capacity at this time as the first charge capacity; the first coulombic efficiency = first charge capacity / first discharge capacity × 100%. The test results are as follows:

[0108]

[0109] It can be seen from the above table that the sodium ion battery of the biomass hard carbon negative electrode material prepared based on Examples 1-5 of the present invention has a very high sodium storage capacity, and the first coulomb efficiency is close to about 90%. The first charging capacity of the lychee shell hard carbon prepared in Example 2 reached 385.82mAh / g, and the first coulomb efficiency reached 90.50%; the first charging capacity of the peanut shell hard carbon prepared in Example 3 reached 393.36mAh / g, and the first coulomb efficiency reached 90.48%. Since the prepared hard carbons all have a nano-block morphology, the specific surface areas of Examples 1-5 tested by nitrogen adsorption-desorption curves are 6.3m 2 / g, 5.2m 2 / g, 6.1m 2 / g, 5.8m 2 / g, 7.4m 2 / g, such a low specific surface area is extremely beneficial for reducing the formation of solid electrolyte interface film (SEI), which is also one of the important reasons why the first efficiency is so high.

[0110] The morphology was further observed by scanning electron microscopy. Figure 2 This is a scanning electron microscope image of the grapefruit peel biomass hard carbon prepared in Example 1. It can be seen that it presents a nano-block structure, with some areas stacked together, and the particle size of the nano-block is about 2-6 um; Figure 3 This is a scanning electron microscope image of the litchi shell biomass hard carbon prepared in Example 2, showing a significant spherical structure with a particle size of about 3-5 um; Figure 4 This is a scanning electron microscope image of the peanut shell biomass hard carbon prepared in Example 3. It can be seen that the morphology distribution is very uniform, showing an obvious block structure, and there is no accumulation and aggregation phenomenon. The particle size distribution is about 4-8um; Figure 5 This is a scanning electron microscope image of coconut shell biomass hard carbon prepared in Example 4, showing a very obvious nano-block structure with relatively uniform distribution and a particle size of about 500nm-1000nm. From the morphological structure analysis of the hard carbon prepared in several examples, it can be seen that the hard carbon prepared by this method all presents a very uniform nano-block structure, and the specific surface area test also shows that it is less than 10m 2 / g, this structural feature is conducive to the full infiltration of the electrolyte and can greatly reduce the formation of the SEI film, which is an important prerequisite for high initial efficiency. Figure 6 and Figure 7 These are high-magnification transmission electron microscope images of Example 2 and Example 3, respectively. It can be seen that both exhibit typical hard carbon characteristics, with a large number of turbine-shaped graphite microcrystalline regions distributed, the lattice spacing is between 0.38nm-0.42nm, and a large number of closed-pore structures, which is very conducive to the storage of sodium ions. Figure 8 This is the first cycle charge and discharge curve of the sodium battery assembled with the lychee shell biomass hard carbon prepared in Example 2 as the negative electrode at a current density of 50mA / g. It can be seen that the first discharge capacity is 426.33mAh / g, the first charge capacity is 385.82mAh / g, and the first efficiency is as high as 90.5%. This is attributed to the prepared hard carbon having a uniformly dispersed block nanostructure, the electrolyte can fully contact and react, and the formation of SEI film is greatly reduced. At the same time, the large interlayer spacing and closed-pore structure are very suitable for the storage of sodium ions. Fig. 9 The first cycle charge and discharge curve of the sodium battery assembled with the peanut shell biomass hard carbon prepared in Example 3 as the negative electrode at a current density of 50mA / g shows that the first discharge capacity is 434.75mAh / g, the first charge capacity is 393.36mAh / g, and the first efficiency is as high as 90.48%. The results show that the present invention has very outstanding advantages in the preparation of hard carbon. The pretreatment of biomass and acid washing can effectively remove the ash and impurities in the biomass. Oxidation promotes the formation of pore structure in the biomass hard carbon negative electrode material and expands the carbon layer spacing, which is beneficial to the diffusion of electrolyte and the transmission of sodium ions, ensuring good sodium ion storage, cycle performance and higher stable reversible capacity. During the low-temperature hydrothermal carbonization process, abundant pores and oxygen-containing functional groups will be generated, which effectively improves the cycle stability and cycle life of the biomass hard carbon negative electrode material. The increase in pyrolysis temperature increases the closed pores of the biomass hard carbon negative electrode material. A large number of pore structures promote the penetration of electrolyte, which is more convenient for the storage of sodium ions, thereby improving its electrochemical performance.

[0111] In summary, the present invention provides a method for preparing high-first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon. The preparation method first pre-treats the biomass, then performs acid washing, and then performs pre-carbonization, and then performs oxidation treatment using a wet chemical method, and then reacts in an autoclave to obtain hydrothermal carbon, and finally performs high-temperature calcination to obtain biomass hard carbon with nano-block morphology, low specific surface area, and large interlayer spacing. The prepared hard carbon shows excellent sodium storage performance, and can well solve the technical problems of low first coulomb efficiency, low reversible sodium storage capacity, and poor cycle stability faced by the current sodium ion battery negative electrode. When the hard carbon prepared by the present invention is used as a sodium ion battery negative electrode material, the battery reversible specific capacity is as high as 393.52mAh / g at a current density of 50mA / g, and the first efficiency reaches more than 90%, surpassing the vast majority of reported hard carbon materials, and has very good theoretical and practical application value.

[0112] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing high-initial-efficiency nano-block sodium-ion battery negative electrode biomass hard carbon, characterized in that: The specific steps include: S1: Pre-treating the biomass raw materials: soaking the biomass raw materials in a solvent for 4-6 hours, then transferring them to an oven, drying them at 60-120°C for 8-12 hours, and then crushing them after drying; S2: Acid washing: Add the product obtained in S1 to deionized water, then add a 1-6M dilute acid aqueous solution for washing, stir at room temperature for 4-8 hours, then wash with deionized water and dry; S3: Pre-carbonization: The product obtained in S2 is placed in a tube furnace and pre-carbonized under the protection of an inert gas; S4: Oxidation: adding the pre-carbonized material obtained in S3 into deionized water, then adding an oxidant to carry out an oxidation reaction, and then centrifuging, washing, and drying to obtain an oxidized material; S5: hydrothermal carbonization: the oxidizing material obtained in S4, the dispersant, and 1-6M sulfuric acid are mixed, and then added into a solvent for magnetic stirring. After stirring, ultrasonication is performed for 10-40 minutes, and then the mixture is transferred to an autoclave for reaction at 120-200°C for 8-12 hours. After the reaction is completed, the mixture is cooled to room temperature, centrifuged, washed, and dried to obtain hydrothermal carbon; S6: Final carbonization: The hydrothermal carbon obtained in S5 is placed in a quartz boat, placed in a tubular furnace, and under the protection of an inert atmosphere, the temperature is raised to 1000-1600°C and calcined at 1000-1600°C for 2-4 hours, and then naturally cooled to room temperature to obtain a biomass hard carbon negative electrode material.

2. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The biomass raw material in S1 is one or more of grapefruit peel, lychee shell, peanut shell, coconut shell, and bamboo.

3. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The solvent used for pretreatment of biomass raw materials in S1 includes one or more of deionized water, methanol, ethanol, isopropanol, and ethyl acetate.

4. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The dilute acid in S2 is one or more of hydrochloric acid, sulfuric acid, nitric acid, formic acid, and acetic acid, and the concentration is 1-6M.

5. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The inert gas in S3 is one or more of air, nitrogen, argon and hydrogen, and the calcination temperature is 300-500°C.

6. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The oxidant in S4 is one or more of nitric acid, hydrogen peroxide, potassium permanganate, and ammonium persulfate.

7. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The dispersant in S5 is one or more of hexadecyltrimethylammonium bromide, sodium dodecyl sulfate, and ammonium dodecyl sulfate, the concentration of sulfuric acid is 1-6M, the solvent is one or more of deionized water, methanol, ethanol, isopropanol, and N,N-dimethylformamide, and the autoclave reaction temperature is 120-200°C.

8. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The heating rate of the programmed temperature in S6 is 3-10°C / min, and the calcination temperature is 1000-1600°C.

9. The method for preparing a high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to claim 1, characterized in that: The biomass hard carbon negative electrode material prepared in S6, acetylene black, and polyvinylidene fluoride are uniformly mixed in a certain proportion, stirred in deionized water for a period of time to obtain an electrode slurry, and used as a negative electrode material for a sodium ion battery.

10. A high first-efficiency nano-block sodium ion battery negative electrode biomass hard carbon according to any one of claims 1 to 9, characterized in that: Application of negative electrode materials for sodium ion batteries.

Citation Information

Patent Citations

  • Preparation method of waste biomass hard carbon negative electrode material for sodium ion battery

    CN115417397A

  • Biomass derived hard carbon material and preparation method thereof, sodium ion battery negative pole piece and sodium ion battery

    CN116803899A

  • Biomass hard carbon material prepared from waste biomass as well as method and application of biomass hard carbon material

    CN118183691A

  • Biomass-based functional-group-modified sodium-ion battery anode material, preparing method therefor and use thereof

    WO2020103138A1

Cited By

  • Hard carbon material prepared from atmosphere-modulated hard carbon closed pore and pseudo graphite domain as well as preparation method and application of hard carbon material

    CN119528116A

  • A hard carbon material prepared by atmosphere-adjusted hard carbon closed pores and pseudo-graphite domains and a preparation method and application thereof

    CN119528116B

  • Hard carbon material, preparation method thereof and battery

    CN119812324A

  • Hard carbon materials, their preparation methods and batteries

    CN119812324B

  • Easily-prepared low-cost high-performance sodium ion battery hydrogen peroxide modified hard carbon negative electrode material and preparation method thereof

    CN120922845A