Method for preparing aluminum fluoride from aluminum electrolysis fluorine-containing waste

Aluminum fluoride is prepared through the acid-base wet treatment of aluminum electrolysis overhaul slag and carbon residue and the reaction of concentrated sulfuric acid, which solves the problems of waste and high cost of valuable F and Al elements in aluminum electrolysis production, and achieves high value of resources. Optimal utilization and closed circulation reduce production costs.

CN118754181APending Publication Date: 2024-10-11YUNNAN RUNXIN ALUMINUM
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410991311.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing technology fails to effectively utilize the valuable F and Al elements in the fluorine-containing waste from aluminum electrolysis, resulting in waste of resources and high production costs, and does not realize closed recycling of fluorine elements.

Method used

By mixing aluminum electrolysis overhaul slag and carbon slag, performing acid-base wet leaching treatment to generate regenerated cryolite and hydrogen fluoride, combined with concentrated sulfuric acid reaction, we can prepare aluminum fluoride that meets the requirements of aluminum electrolysis production and achieve high values ​​of valuable elements. utilization and recycling.

Benefits of technology

It realizes high-value utilization of surplus electrolyte and regenerated cryolite in aluminum electrolysis production, significantly reduces the consumption and disposal cost of concentrated sulfuric acid, increases the recovery rate of valuable elements, realizes closed recycling of resources, and reduces production costs. .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for preparing aluminum fluoride from aluminum electrolysis fluorine-containing waste, which comprises the following steps of: mixing overhaul slag and carbon slag for size mixing, and carrying out pressurized alkaline leaching, cyanogen removal and solid-liquid separation to obtain alkaline leaching liquid and alkaline leaching slag; carrying out acid leaching on the alkaline leaching residues, and carrying out solid-liquid separation to obtain acid leaching liquid and acid leaching residues; mixing the alkaline leaching solution and the acid leaching solution, neutralizing and precipitating, and separating to obtain regenerated cryolite; mixing the regenerated cryolite and an aluminum electrolyte, and treating to obtain mixed powder; reacting the mixed powder with concentrated sulfuric acid to obtain reaction residues and hydrogen fluoride; adding sodium hydroxide into filtrate obtained after the reaction residues are treated, and performing solid-liquid separation to obtain aluminum hydroxide; treating the obtained hydrogen fluoride, and reacting with aluminum hydroxide to obtain aluminum fluoride; according to the method, high-value utilization of valuable F and Al elements in surplus aluminum electrolyte is realized while the F and Al extracted from the electrolytic aluminum overhaul slag and the carbon slag are harmlessly treated, and remarkable economic benefits are generated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of resource recycling, and in particular to a method for preparing aluminum fluoride by utilizing fluorine-containing waste materials through aluminum electrolysis. Background Art

[0002] Fluorine-containing materials in aluminum electrolysis mainly include aluminum electrolysis overhaul slag, carbon slag, electrolyte, etc. In November 2020, the National Hazardous Waste List (2021 Edition) No. 15 of the Ministry of Ecology and Environment was officially released. Hazardous waste slags involved in the electrolytic aluminum industry include overhaul slag (321-023-48) and carbon slag (321-025-48). Their main hazardous characteristics include toxicity (T) and reactivity (R).

[0003] Among them, overhaul slag is the waste slag produced by the maintenance and replacement of the cathode lining of the electrolytic cell during the production of electrolytic aluminum; carbon slag is the carbon particles falling off due to the uneven combustion and selective oxidation of the carbon anode. The main components of aluminum electrolysis carbon slag are carbon and electrolyte, generally containing 20-30% carbon and 60-70% electrolyte. The main components of the electrolyte are Na3AlF6, Al2O3, CaF2, etc. Domestic university scholars have done a lot of research on the disposal and comprehensive utilization of resources of hazardous waste slag from aluminum electrolysis. At present, there are technologies at home and abroad. The harmless disposal and comprehensive utilization of resources of hazardous waste slag from aluminum electrolysis can be divided into two categories: wet treatment and pyrolysis. The wet treatment process mainly includes water leaching, alkali leaching, acid leaching, acid-base combined leaching, or using the waste cathode as a carbonaceous material with a usable calorific value resource, or high-temperature recovery of electrolyte. However, such treatment will cause the loss of valuable F and Al valuable elements in the overhaul slag and carbon slag, resulting in a waste of resources.

[0004] The production of electrolytic aluminum uses an electrolyte system based on cryolite. During the production process, aluminum fluoride needs to be continuously added to the electrolytic cell in order to control the electrolyte molecular ratio. However, since very little electrolyte is carried away by electrolytic flue gas, operation entrainment, etc., the electrolyte in the aluminum electrolytic cell will continue to increase, resulting in surplus. The main components of this surplus electrolyte are sodium fluoride, aluminum fluoride and cryolite, etc., with extremely high fluorine content, which is a good fluorine resource and needs to be utilized as a resource.

[0005] For example, the Chinese patent with publication number CN111892022A discloses a method for utilizing fluorine-containing waste and surplus electrolyte resources from aluminum electrolysis, wherein the fluorine-containing waste and surplus electrolyte from aluminum electrolysis are crushed and ground into electrolyte powder, and the electrolyte powder and acid are added to a negative pressure reactor for reaction. The hydrogen fluoride generated by the reaction is condensed and distilled to obtain a hydrofluoric acid product, and the reaction residue is treated with a neutralizer and filtered. The filter residue is a calcium salt, and the filtrate is a sodium aluminate solution, which is used for aluminum oxide production. The product produced by this method is a hydrofluoric acid product, and the closed-loop recycling of fluorine element in the aluminum electrolysis production process is not achieved.

[0006] Therefore, it is particularly important to use fluorine-containing materials in aluminum electrolysis to prepare aluminum fluoride that can be used in aluminum electrolysis production. Summary of the invention

[0007] The purpose of the present invention is to dispose of aluminum electrolytic overhaul slag and carbon slag harmlessly by acid and alkali wet leaching to extract F and Al, and to propose a method for synergistically preparing aluminum fluoride from aluminum electrolysis fluorine-containing materials, and to achieve synergistic treatment of surplus electrolyte in the aluminum electrolysis production process, to achieve high value and closed-loop recycling of valuable F and Al elements in the surplus aluminum electrolyte, and to produce significant economic benefits. Specifically, it relates to a method for preparing aluminum fluoride from aluminum electrolysis fluorine-containing waste.

[0008] The embodiments of the present invention are implemented by the following technical solutions:

[0009] A method for preparing aluminum fluoride by using aluminum electrolysis fluorine-containing waste, comprising the following steps:

[0010] (1) Aluminum electrolysis overhaul slag and carbon slag are mixed and slurried. Specifically, aluminum electrolysis overhaul slag and carbon slag are mixed (they can be mixed at a mass ratio of 3:1-10:1) so that the F content is not less than 20%, and the molar ratio of F to Al is 2-6; after the mixture is ground, water is added to the slurry at a liquid-to-solid ratio of 3:1-10:1, and then a NaOH solution is added to adjust the pH value to 9-12; when removing cyanide, ozone and calcium hypochlorite are added for oxidation and cyanide removal for 2-3 hours; then 50g / L-100g / L of NaOH solution is added to the slurry to a liquid-to-solid ratio of 8:1-12:1, and pressurized alkali leaching is performed in sequence (the pressurized parameters are: reaction temperature 100-120°C, reaction time 1h-2h, liquid-to-solid ratio 5:1-7:1, alkali concentration 50 -100g / L, pressure 0.2-0.3Mpa), decyanation treatment (adding ozone and calcium hypochlorite for oxidation decyanation for 2-3h), and obtaining alkaline leaching solution and alkaline leaching residue through solid-liquid separation; then adding concentrated sulfuric acid to the alkaline leaching residue obtained above to adjust the slurry solid content to 15%-20%, and staying for 4-12h in a continuous acid leaching tank under the process conditions of 50℃-70℃ for acid leaching, and obtaining acid leaching solution and acid leaching residue through solid-liquid separation;

[0011] (2) mixing the alkaline leaching solution and the acid leaching solution in a mass ratio of 3.5:1-2.5:1, and adding soluble aluminum salt and liquid alkali to make the molar ratio of F and Al in the mixed solution 3-6 and the solution pH 7-8, stirring for 4 hours at a stirring speed of 600-800 r / min and a reaction temperature of 40-90° C. for neutralization precipitation to ensure that fluorine is completely precipitated (less than 200 mg / L), and obtaining regenerated cryolite through solid-liquid separation;

[0012] (3) After mixing the regenerated cryolite and / or aluminum electrolyte, drying, crushing, and grinding to obtain a mixed powder; the regenerated cryolite and the aluminum electrolyte can be used separately or mixed; when mixed, the mixing ratio of the regenerated cryolite and the aluminum electrolyte is 1:9 to 5:5;

[0013] (4) adding the powder obtained in step (3) into a reaction kettle, adding concentrated sulfuric acid and mixing, reacting under stirring and heating conditions to obtain reaction slag and hydrogen fluoride gas; wherein the concentrated sulfuric acid is industrial concentrated sulfuric acid with a concentration of 98%, and the amount of concentrated sulfuric acid added is 1.1-1.5 times the theoretical value; the reaction temperature is 150° C.-270° C.; the reaction time is 1-5 h; the stirring frequency is 100-200 r / min; the main reaction equation is as follows:

[0014] 2Na3AlF6+6H2SO4=3Na2SO4+Al2(SO4)3+12HF

[0015] 3Na3AlF6+2H2SO4=2Na2SO4+Na5Al3F 14 +4HF

[0016] 2Na3AlF6+3H2SO4=3Na2SO4+2AlF3+6HF

[0017] 2Na5Al3F 14 +5H2SO4=5Na2SO4+6AlF3+10HF

[0018] 2Na5Al3F 14 +14H2SO4=5Na2SO4+3Al2(SO4)3+28HF

[0019] 2AlF3+3H2SO4=Al2(SO4)3+6HF

[0020] 2NaF+H2SO4=Na2SO4+2HF

[0021] (5) adding water to dissolve the reaction residue obtained in step (4), filtering it, and returning the filter residue to the alkaline leaching step of step (1) to further improve the yield of fluorine; returning the filtrate to the acid leaching step of step (1) to achieve the reuse of dilute acid, soluble aluminum salts, etc., and reduce the disposal of water; the filtrate can also be used to prepare aluminum sulfate and aluminum hydroxide, and extract by-products such as potassium salt and lithium salt at the same time;

[0022] (6) purifying, drying and demisting the hydrogen fluoride obtained in step (4) and reacting it with aluminum hydroxide to obtain aluminum fluoride; specifically, the aluminum hydroxide here can be the aluminum hydroxide slurry obtained in step (5) or the aluminum hydroxide in an aluminum fluoride reaction equipment such as a rotary kiln or a fluidized bed or commercially available aluminum hydroxide or a combination thereof;

[0023] Wherein, the temperature of the aluminum hydroxide slurry is 70°C-90°C, the stirring frequency is 120-150r / min, and the reaction time is 3-4h; the reaction temperature of the rotary kiln is 500-550°C, the rotation speed is 20-30r / min, and the reaction time is 3-4h; the main reaction equation is as follows:

[0024] Al(OH)3+3HF=AlF3+3H2O

[0025] Al2O3+6HF→2AlF3+3H2O

[0026] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:

[0027] (1) The present invention takes the "preparation of hydrogen fluoride + conversion of aluminum fluoride" from surplus electrolyte produced by aluminum electrolysis, recycled cryolite and other fluorine-containing materials as the main line, effectively making high-value utilization of valuable F, Al and other elements in surplus electrolyte produced by aluminum electrolysis and recycled cryolite. While realizing the resource utilization and high-value utilization of surplus electrolyte produced by aluminum electrolysis and recycled cryolite, the closed-loop recycling of valuable F, Al and other elements in the aluminum electrolysis production process is realized.

[0028] (2) The present invention studies and develops a process technology for preparing hydrogen fluoride gas by mixing surplus electrolyte, regenerated cryolite and low sulfuric acid ratio based on the valuable components of fluorine-containing materials such as surplus electrolyte and regenerated cryolite produced by aluminum electrolysis, so that valuable components such as fluoride, sodium salt, aluminum salt and lithium salt can be fully recycled in the system to produce high-value aluminum fluoride products that meet the requirements of aluminum electrolysis production and use, solves the problem of excess products such as cryolite and electrolyte in traditional processes, greatly saves the production cost of aluminum electrolytic enterprises, and improves the value of valuable F and Al in fluorine-containing materials in aluminum electrolysis.

[0029] (3) In the method of preparing aluminum fluoride from fluorine-containing waste from aluminum electrolysis of the present invention, the amount of concentrated sulfuric acid added is 1.1-1.5 times the theoretical value, which can achieve leaching of more than 95% of the fluorine element in the fluorine-containing waste from aluminum electrolysis, greatly reducing the amount of concentrated sulfuric acid used and the disposal cost, while also greatly reducing the amount of post-disposal liquid generated and reducing the post-disposal liquid treatment pressure.

[0030] (4) The wastewater generated by the present invention can be fed into the harmless disposal system of overhaul slag and carbon slag, or fed into the nanofiltration, freezing crystallization, evaporation crystallization and other systems to prepare products such as sodium sulfate and lithium salt. The fresh water obtained by the nanofiltration, evaporation crystallization and other processes can be fed into the slurry mixing process of overhaul slag and carbon slag. The prepared hydrogen fluoride gas can be used to produce aluminum fluoride products. The slag that has not reacted completely can be returned. Thus, a technical path has been found to maximize the value of solid waste resources.

[0031] (5) The present invention can achieve the leaching of valuable lithium elements from fluorine-containing materials such as surplus electrolyte and regenerated cryolite, and realize the comprehensive recovery and utilization of the valuable lithium elements through the lithium salt preparation process. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0033] Example 1

[0034] A method for preparing aluminum fluoride by using aluminum electrolysis fluorine-containing waste, comprising the following steps:

[0035] (1) Aluminum electrolysis overhaul slag and carbon slag are mixed in a mass ratio of 5:1, crushed and ball-milled, wherein the F element content is not less than 20%, and the molar ratio of F to Al element is 3; then NaOH solution is added to adjust the slurry to a liquid-solid ratio of 8:1-12:1, and the pH value is adjusted to 9-12; pressurized alkali leaching and cyanide removal treatment are carried out in sequence, and alkali leaching solution and alkali leaching residue are obtained through solid-liquid separation; during pressurized alkali leaching, the reaction temperature is 110°C, the reaction time is 1.5h, the liquid-solid ratio is 6:1, the alkali concentration is 80g / L, and the pressure is 0.25Mpa; during cyanide removal treatment, ozone and calcium hypochlorite are added to oxidize and remove cyanide for 2.5h

[0036] Then, concentrated sulfuric acid is added to the alkaline leaching residue obtained above to adjust the solid content of the slurry to 18%, and the slurry is acid-leached for 6 hours under the process condition of 60° C. in a continuous acid leaching tank, and the acid leaching liquid and acid leaching residue are obtained by solid-liquid separation;

[0037] (2) mixing the alkaline leaching solution and the acid leaching solution in a mass ratio of 3:1, and adding soluble aluminum salt and liquid alkali so that the molar ratio of F and Al elements in the mixed solution is 4 and the solution pH is 7, stirring for 4 hours at a stirring speed of 800 r / min and a reaction temperature of 90° C. for neutralization and precipitation, and obtaining regenerated cryolite by solid-liquid separation;

[0038] (3) mixing the regenerated cryolite and aluminum electrolyte in a mass ratio of 1:9, drying, crushing, and grinding to obtain a mixed powder;

[0039] (4) mixing the mixed powder obtained in step (3) with concentrated sulfuric acid and adding the mixture to a reactor for reaction to obtain reaction slag and hydrogen fluoride; wherein the concentrated sulfuric acid is industrial concentrated sulfuric acid with a concentration of 98%, and the amount of concentrated sulfuric acid added is 1.2 times that of the mixed powder; the reaction temperature is 250° C.; and the reaction time is 4.5 h;

[0040] (5) diluting the reaction residue obtained in step (4) with water, filtering, removing impurities, and then adding sodium hydroxide. After solid-liquid separation, the filter residue obtained is an aluminum hydroxide product, and the obtained filtrate is transported to a nanofiltration, freeze crystallization, evaporation crystallization or other system to prepare Glauber's salt;

[0041] (6) The hydrogen fluoride obtained in step (4) is purified, dried and demisted, and then introduced into the aluminum hydroxide slurry obtained in step (5) to react with aluminum hydroxide to obtain aluminum fluoride; wherein the temperature of the aluminum hydroxide slurry is 80° C., the stirring frequency is 130 r / min, and the reaction time is 4 h; the reaction temperature of the rotary kiln is 530° C., the rotation speed is 25 r / min, and the reaction time is 3 h; after testing, the fluorine content of the obtained aluminum fluoride is 65.1%, the aluminum content is 34.8%, and the sodium content is 0.10%; and the recovery rate of valuable lithium element is 92%.

[0042] Example 2

[0043] A method for preparing aluminum fluoride by using aluminum electrolysis fluorine-containing waste, comprising the following steps:

[0044] (1) Aluminum electrolysis overhaul slag and carbon slag are mixed in a mass ratio of 3:1, crushed and ball-milled, wherein the F element content is not less than 20%, and the molar ratio of F to Al element is 3; then NaOH solution is added to adjust the slurry to a liquid-solid ratio of 8:1-12:1, and the pH value is adjusted to 9-12; pressurized alkali leaching and cyanide removal treatment are carried out in sequence, and alkali leaching solution and alkali leaching residue are obtained through solid-liquid separation; during pressurized alkali leaching, the reaction temperature is 100°C, the reaction time is 1h, the liquid-solid ratio is 5:1, and the pressure is 0.2Mpa; during cyanide removal treatment, ozone and calcium hypochlorite are added to oxidize and remove cyanide for 2h

[0045] Then, concentrated sulfuric acid is added to the alkaline leaching residue obtained above to adjust the solid content of the slurry to 15%, and the slurry is kept in a continuous acid leaching tank at 50° C. for 5 minutes for acid leaching, and the acid leaching liquid and acid leaching residue are obtained by solid-liquid separation;

[0046] (2) mixing the alkaline leaching solution and the acid leaching solution in a mass ratio of 3.5:1, and adding soluble aluminum salt and liquid alkali, so that the molar ratio of F and Al elements in the mixed solution is 5 and the solution pH is 7.5, stirring for 4 hours at a stirring speed of 600 r / min and a reaction temperature of 90° C. for neutralization and precipitation, and obtaining regenerated cryolite by solid-liquid separation;

[0047] (3) drying, crushing and grinding the aluminum electrolyte to obtain a powder;

[0048] (4) mixing the powder obtained in step (3) with concentrated sulfuric acid in a reactor and reacting the mixture to obtain reaction slag and hydrogen fluoride; wherein the concentrated sulfuric acid is industrial concentrated sulfuric acid with a concentration of 98%, and the amount of concentrated sulfuric acid added is 1 times the amount of the mixed powder; the reaction temperature is 230° C.; and the reaction time is 4 h;

[0049] (5) The reaction residue obtained in step (4) is diluted with water, filtered, and impurities are removed, and then sodium hydroxide is added. After solid-liquid separation, the filter residue obtained is the aluminum hydroxide product, and the obtained filtrate is transported to step (1);

[0050] (6) the hydrogen fluoride obtained in step (4) is purified, dried, and demisted, and then introduced into the aluminum hydroxide slurry obtained in step (5), and commercially available aluminum hydroxide is added to react to obtain aluminum fluoride;

[0051] Among them, the temperature of the aluminum hydroxide slurry is 70°C-90°C, the stirring frequency is 120-150r / min, and the reaction time is 3-4h; the reaction temperature of the rotary kiln is 500-550°C, the rotation speed is 20-30r / min, and the reaction time is 3-4h; after testing, the fluorine content of the obtained aluminum fluoride is 64.7%, the aluminum content is 34.2%, and the sodium content is 0.15%; the recovery rate of valuable lithium elements is 93%.

[0052] Example 3

[0053] A method for preparing aluminum fluoride by using aluminum electrolysis fluorine-containing waste, comprising the following steps:

[0054] (1) Aluminum electrolysis overhaul slag and carbon slag are mixed in a mass ratio of 10:1, crushed and ball-milled, wherein the F element content is not less than 20%, and the molar ratio of F to Al element is 3; then NaOH solution is added to adjust the slurry to a liquid-solid ratio of 8:1-12:1, and the pH value is adjusted to 9-12; pressurized alkali leaching and cyanide removal treatment are carried out in sequence, and alkali leaching solution and alkali leaching residue are obtained through solid-liquid separation; during pressurized alkali leaching, the reaction temperature is 120°C, the reaction time is 2h, the liquid-solid ratio is 7:1, the alkali concentration is 100g / L, and the pressure is 0.3Mpa; during cyanide removal treatment, ozone and calcium hypochlorite are added to oxidize and remove cyanide for 3h

[0055] Then, concentrated sulfuric acid is added to the alkaline leaching residue obtained above to adjust the solid content of the slurry to 20%, and the slurry is acid-leached for 7 hours under the process condition of 70° C. in a continuous acid leaching tank, and the acid leaching liquid and acid leaching residue are obtained by solid-liquid separation;

[0056] (2) mixing the alkaline leaching solution and the acid leaching solution in a mass ratio of 2.5:1, and adding soluble aluminum salt and liquid alkali so that the molar ratio of F and Al elements in the mixed solution is 6 and the solution pH is 8, stirring for 4 hours at a stirring speed of 1000 r / min and a reaction temperature of 90° C. for neutralization and precipitation, and obtaining regenerated cryolite by solid-liquid separation;

[0057] (3) drying, crushing and grinding the regenerated cryolite to obtain powder;

[0058] (4) mixing the powder obtained in step (3) with concentrated sulfuric acid in a reactor and reacting the mixture to obtain reaction slag and hydrogen fluoride; wherein the concentrated sulfuric acid is industrial concentrated sulfuric acid with a concentration of 98%, and the amount of concentrated sulfuric acid added is 1.5 times that of the mixed powder; the reaction temperature is 270° C.; and the reaction time is 5 h;

[0059] (5) diluting the reaction residue obtained in step (4) with water, filtering, removing impurities, and then adding sodium hydroxide. After solid-liquid separation, the filter residue obtained is an aluminum hydroxide product, and the obtained filtrate is transported to a nanofiltration, freeze crystallization, evaporation crystallization or other system to prepare Glauber's salt;

[0060] (6) The hydrogen fluoride obtained in step (4) is purified, dried and demisted, and then introduced into the aluminum hydroxide slurry obtained in step (5) and an aluminum fluoride reaction equipment such as a rotary kiln and a fluidized bed to react with aluminum hydroxide, aluminum oxide, etc. to obtain aluminum fluoride; wherein the temperature of the aluminum hydroxide slurry is 90° C., the stirring frequency is 150 r / min, and the reaction time is 4 h; the reaction temperature of the rotary kiln is 550° C., the rotation speed is 30 r / min, and the reaction time is 4 h; after testing, the fluorine content of the obtained aluminum fluoride is 65.3%, the aluminum content is 33.8%, and the sodium content is 0.11%; and the recovery rate of valuable lithium element is 90%.

[0061] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing aluminum fluoride by using aluminum electrolysis fluorine-containing waste, characterized in that: The following steps are involved: (1) After overhaul slag and carbon slag are mixed and slurried, they are subjected to pressurized alkali leaching and cyanide removal treatment in sequence, and alkali leaching solution and alkali leaching residue are obtained through solid-liquid separation; the alkali leaching residue obtained above is then subjected to acid leaching, and acid leaching solution and acid leaching residue are obtained through solid-liquid separation; (2) mixing the alkaline leaching solution with the acid leaching solution, and adding soluble aluminum salt and liquid alkali to make the molar ratio of F and Al in the mixed solution be 3-6 and the solution pH be 7-8, performing neutralization precipitation, and then performing solid-liquid separation to obtain regenerated cryolite; (3) mixing the regenerated cryolite and / or aluminum electrolyte obtained in step (2) and treating the mixture to obtain a mixed powder; (4) mixing the mixed powder obtained in step (3) with concentrated sulfuric acid to obtain reaction slag and hydrogen fluoride; (5) adding water to dissolve the reaction residue obtained in step (4), filtering, returning the filter residue to the alkaline leaching step of step (1), and returning part of the filtrate to the acid leaching step of step (1); and adding sodium hydroxide to part of the filtrate to obtain aluminum hydroxide after solid-liquid separation; (6) The hydrogen fluoride obtained in step (4) is treated and then stirred and reacted with aluminum hydroxide or aluminum oxide to obtain aluminum fluoride.

2. The method for preparing aluminum fluoride by using fluorine-containing waste materials from aluminum electrolysis according to claim 1, characterized in that: In step (1), when the overhaul slag and carbon slag are mixed and slurried: the aluminum electrolysis overhaul slag and carbon slag are mixed so that the F content is not less than 20%, and the molar ratio of F to Al is 2-6; after the mixture is ground, water is added to the slurry at a liquid-solid ratio of 3:1-10:1, and then NaOH solution is added to adjust the pH value to 9-12; when decyanation treatment is performed, ozone and calcium hypochlorite are added to perform oxidative decyanation for 2-3 hours.

3. The method for preparing aluminum fluoride by using fluorine-containing waste materials from aluminum electrolysis according to claim 1, characterized in that: When the alkaline leaching residue in step (1) is acid leached, concentrated sulfuric acid is added to adjust the solid content of the slurry to 5%-20%, and concentrated sulfuric acid is added to adjust the pH value to less than 3.5, and the slurry is kept in a continuous acid leaching tank under process conditions of 50°C-70°C for 5-7h.

4. The method for preparing aluminum fluoride by using fluorine-containing waste materials from aluminum electrolysis according to claim 1, characterized in that: In step (2), the alkaline leaching solution is mixed with the acid leaching solution, and a soluble aluminum salt and liquid alkali are added to make the molar ratio of F and Al in the mixed solution 3-6 and the solution pH 7-8 for neutralization and precipitation.

5. The method for preparing aluminum fluoride by utilizing fluorine-containing waste materials from aluminum electrolysis according to claim 1, characterized in that: During the neutralization precipitation in step (2), the mixture is stirred for 4 hours at a stirring speed of 600-1000 r / min and a reaction temperature of 40-90° C. for neutralization precipitation.

6. The method for preparing aluminum fluoride by utilizing fluorine-containing waste materials from aluminum electrolysis according to claim 1, characterized in that: The regenerated cryolite and aluminum electrolyte described in step (3) can be used separately or mixed; when used in mixture, the mixing mass ratio of the regenerated cryolite and the aluminum electrolyte is 1:1-1:

9.

7. The method for preparing aluminum fluoride by utilizing fluorine-containing waste materials from aluminum electrolysis according to claim 1, characterized in that: The amount of concentrated sulfuric acid added in step (4) is 1.1-1.5 times the theoretical amount required to convert all fluorine in the mixed powder into hydrogen fluoride.

8. The method for preparing aluminum fluoride by utilizing fluorine-containing waste materials by aluminum electrolysis according to claim 1, characterized in that: In step (4), the reaction temperature is 150°C-300°C; the reaction time is 1-5.

9. The method for preparing aluminum fluoride by utilizing fluorine-containing waste materials by aluminum electrolysis according to claim 1, characterized in that: In step (6), the temperature of the aluminum hydroxide slurry is 70° C.-90° C., the stirring frequency is 120-150 r / min, and the reaction time is 3-4 h.

Citation Information

Cited By

  • Method for producing cryolite from overhaul slag

    CN119461441A

  • Flotation-based carbon residue overhaul slag resource collaborative utilization and multi-component recovery process

    CN121551372A