Preparation method of boron-nitrogen co-doped lithium vanadate / carbon composite lithium ion battery negative electrode material

Bowl-shaped Li3VO4/B-NC composite materials are prepared through chemical cross-linking and spray drying technology, which solves the problems of difficult morphology control and poor conductivity of lithium vanadate, achieves high capacity and high cycle stability, simplifies the process and reduces the cost. Reduce costs and improve the overall performance of lithium-ion battery anode materials.

CN118754198APending Publication Date: 2024-10-11CHINA THREE GORGES UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410787548.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing lithium-ion battery anode materials such as carbon materials, lithium titanate and silicon-based materials have problems such as low lithium insertion potential, poor conductivity, and severe volume expansion. Moreover, the morphology of lithium vanadate is difficult to control and the conductivity is insufficient, which affects its application. value.

Method used

Bowl-shaped Li3VO4/B-NC composite materials were prepared using chemical cross-linking and spray drying techniques. By adjusting the cross-linking degree of acrylic acid and boric acid, a bowl-shaped hemispheric structure was formed, which improved the packing density and conductivity, and enhanced the electrochemical performance.

Benefits of technology

It achieves high capacity, high cycle stability and excellent electrochemical performance, simplifies the preparation process, reduces costs, relieves stress through the hollow structure, and increases the contact area between Li+ and the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754198A_ABST
    Figure CN118754198A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a boron-nitrogen co-doped lithium vanadate / carbon lithium ion battery negative electrode material. The bowl-shaped Li3VO4 / B-NC composite material is successfully prepared by adopting a synthesis process of spray drying and subsequent calcination. The preparation method specifically comprises the following steps: 1, taking beta-cyclodextrin, an acrylic acid solution and boric acid, adding a proper amount of deionized water, and uniformly stirring to obtain a solution A; and 2, dissolving vanadium pentoxide, lithium carbonate and hexamethylenetetramine in a proper amount of deionized water, carrying out hydrothermal treatment to obtain a colorless transparent solution B, mixing the two solutions, uniformly stirring, and carrying out spray drying. And finally, sintering in a nitrogen environment to obtain the bowl-shaped Li3VO4 / B-NC composite material which can be used as a negative electrode material of a lithium ion battery. According to the bowl-shaped Li3VO4 / B-NC composite material, chemical crosslinking of BA and acrylic acid is utilized for the first time in synthesis of the Li3VO4 negative electrode material to regulate and control the morphology, the preparation process is simple, and the synthesized bowl-shaped Li3VO4 / B-NC composite material solves the problems that Li3VO4 is poor in conductivity, difficult to regulate and control the morphology and low in yield, and can show excellent electrochemical performance as a lithium ion battery negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a novel negative electrode material for a lithium ion battery, in particular to a method for preparing a bowl-shaped Li3VO4 / B-NC composite material as a negative electrode material for a lithium ion battery by spray drying, and belongs to the field of electrochemical energy. Background Art

[0002] Lithium-ion batteries have been widely used in energy storage systems due to their many advantages such as high energy density, long cycle life, and green environmental protection. As the application of lithium-ion batteries becomes more and more widespread, the requirements for lithium-ion batteries are also getting higher and higher, so it is more worthy for researchers to explore and develop new negative electrode materials with higher stability, high safety, and low cost. At present, the active negative electrode materials used in the commercial lithium battery industry are mainly carbon materials, lithium titanate, and silicon-carbon negative electrodes. However, they all have corresponding problems in practical applications, such as the low lithium insertion potential of carbon materials and easy lithium precipitation, the poor conductivity and rate performance of lithium titanate negative electrode materials, and the serious volume expansion and greater safety hazards of silicon-based negative electrode materials during the cycle. Lithium vanadate (Li3VO4) has a high theoretical capacity (592 mAh g -1 ), low volume expansion, excellent chemical stability and low cost, but also has the disadvantages of poor conductivity and difficult morphology control. In previous studies, researchers found that heteroatom doping can significantly improve its electrochemical and mechanical properties, and the material morphology has a crucial influence on the electrochemical performance. Hollow spherical structures have received extensive attention in the field of energy storage due to their high contact area between electrolyte and electrode and the unique characteristics of buffering electrode volume change. Despite many advantages, the large voids inside the hollow nanostructures lead to low packing density of active materials. When used as electrode materials, the large inner cavity leads to relatively low volume energy density, which affects its practical application. Bowl-shaped, as a special hollow structure, can effectively improve the volume energy density, and the stacked hollow bowl-shaped structures are also conducive to the formation of favorable conductive channels. The hard template method is a common method for preparing bowl-shaped hollow structure materials, but the preparation of spherical templates and hard templates needs to be removed by acid / base etching or organic solvent dissolution, which makes the process cumbersome and not environmentally friendly.

[0003] Based on the above background, this experiment developed a method for preparing Li3VO4 / B-NC composite materials with bowl-shaped morphology based on chemical crosslinking and spray drying. By adjusting the degree of boric acid crosslinking and combining spray drying technology to control the morphology, the prepared material is mainly bowl-shaped hemispheres connected to each other. The stacking of bowl-shaped hemispheres can increase the packing density and shorten the transmission path of ions. The internal hollow structure can effectively relieve stress and increase Li +The contact area with the electrolyte. In addition, the uniform composite of boron and nitrogen co-doped carbon can significantly improve the conductivity of the material. The prepared bowl-shaped Li3VO4 / B-NC composite material exhibits excellent electrochemical performance as a negative electrode for lithium-ion batteries and has great potential application value. Summary of the invention

[0004] The present invention proposes a method for preparing a novel bowl-shaped Li3VO4 / B-NC lithium-ion battery negative electrode material. The prepared bowl-shaped Li3VO4 / B-NC composite material is synthesized based on chemical crosslinking combined with simple spray drying technology, which solves the problems of difficult Li3VO4 morphology control and poor conductivity. For the first time, by adjusting the degree of chemical crosslinking between acrylic acid and BA, the purpose of regulating the morphology during the spray drying process was achieved, and a bowl-shaped hemisphere was successfully prepared, which is an expandable and simple method. Due to its anisotropic effect, the bowl-shaped structure can increase the packing density compared with the hollow structure, effectively eliminate mechanical stress, and the hemispheres are interconnected to form an interconnected path for lithium ion diffusion, and the stacking forms a conductive path that is conducive to ion transmission. Therefore, this material has excellent comprehensive electrochemical properties as a lithium-ion battery negative electrode and has potential application value in lithium-ion batteries.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A method for preparing a bowl-shaped array Li3VO4 / B-NC lithium-ion battery negative electrode material, the method comprising the following steps: (1) Take β-cyclodextrin, acrylic acid solution, BA (boric acid), add water and stir evenly to obtain a uniform transparent solution A; (2) Take V2O5, Li2CO3, C6H 12 N4 was hydrothermally treated to obtain a colorless and transparent Li3VO4 precursor solution B; (3) Mixing solution A and solution B, stirring evenly and spray drying to obtain Li3VO4 / B-NC precursor powder; (4) After spray drying, the mixture is placed in a nitrogen environment and calcined at 500-600 °C for 3-6 hours to obtain a bowl-shaped Li3VO4 / B-NC composite material as a negative electrode material for lithium-ion batteries.

[0006] Preferably, in step (1), β-cyclodextrin, acrylic acid solution and BA are used to prepare a spray drying precursor solution A, wherein the concentration of the acrylic acid solution is 20 wt.%-50 wt.%, and the boric acid accounts for 2 wt.%-15 wt.% of the total mass. Preferably, in step (2), the Li3VO4 precursor solution B is V2O5, Li2CO3, C6H 12 N4 is obtained by hydrothermal reaction, and the molar ratio of Li2CO3 and V2O5 is 3-5:1.12 N4 is used as solvent in a relatively excessive amount.

[0007] Preferably, in step (3), the volume ratio of solution A to solution B in the mixed solution is 1-5:20, and the inlet temperature of the spray drying is 150-160°C.

[0008] Preferably, in step (4), the precursor powder is sintered in a nitrogen atmosphere at a heating rate of 3-5°C / min and calcined at 500-600°C for 3-6 hours.

[0009] The present invention uses chemical crosslinking of acrylic acid and BA to obtain a bowl-shaped Li3VO4 / B-NC electrode material for the first time by spray drying. The hollow structure is conducive to electrolyte penetration and effectively buffers the volume effect. At the same time, the high tap density ensures a high volume energy density. The bowl-shaped stacking can shorten the ion transmission path and increase the Li + The contact area with the electrolyte. In addition, the boron-nitrogen co-doped carbon provides abundant active centers. Therefore, this material has excellent comprehensive electrochemical properties as a negative electrode material for lithium-ion batteries, and has the advantages of high capacity and high cycle stability.

[0010] The principle is: (1) V2O5, Li2CO3, C6H 12 The solution obtained by the hydrothermal reaction of N4 has good dispersibility. β-cyclodextrin, acrylic acid solution, and BA are uniformly mixed with it. Under vigorous stirring, a precursor solution containing a uniform mixture of lithium source, vanadium source, carbon source, and water molecules is formed; (2) Spray drying is a method of preparing particles by forming droplets in a solution, which are then evaporated and decomposed in a reactor. The water in the droplets gradually escapes under heating, and the precursor is layered and assembled. (3) During the spraying process, the hydroxyl groups in BA and the carboxylic acid groups of acrylic acid undergo a stable esterification reaction, thereby cross-linking, and the lithium source and vanadium source are uniformly dispersed in the cross-linked network. (4) During the evaporation process, due to the surface stress caused by the cross-linking of BA, the droplets gradually evolve into hollow spheres. The water in the droplets gradually escapes under heating, and the pressure difference on the surface of the hollow sphere increases, causing it to shrink inward, and finally evolve into a bowl-shaped hemisphere. (5) During the sintering process, on the one hand, the phase transition of Li3VO4 precursor to Li3VO4 and the carbonization of β-cyclodextrin and acrylic acid occur simultaneously, resulting in the formation of a large number of nano-sized Li3VO4 / C particles. On the other hand, the residual C6H 12 N4 and BA are decomposed to obtain B, N in situ doped with C. The bowl-shaped Li3VO4 / B-NC prepared by the present invention has good electrochemical properties and electrolyte wettability, can be used to prepare negative electrode materials for lithium ion batteries, and has the advantages of high capacity, high cycle stability, etc.

[0011] Compared with the prior art, the present invention has the following beneficial effects: (1) The synthesis process is simple, and the bowl-shaped hemispheres prepared by spray drying have high yield, low cost, and controllable morphology; (2) BA and acrylic acid are readily available raw materials. The carboxylic acid group of acrylic acid forms an ester bond with the hydroxyl group of boric acid to undergo a cross-linking reaction. The degree of chemical cross-linking can then be adjusted to affect the magnitude of stress during the spraying process, thereby regulating the morphology.

[0012] (3) The prepared bowl-shaped Li3VO4 / B-NC composite material has a hollow structure that is conducive to electrolyte penetration and effectively buffers the volume effect. The bowl-shaped hemispherical stacking can increase the packing density and shorten the ion transmission path, increasing the Li + At the same time, the boron-nitrogen co-doped carbon provides abundant active centers to improve the conductivity of the material, giving it high capacity and excellent cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 Optical photographs of the samples prepared after spray drying in Example 1: (a) spray-dried precursor powder, (b) precursor powder after sintering.

[0014] Figure 2 XRD pattern of the sample prepared in Example 1.

[0015] Figure 3 SEM images of the sample prepared in Example 1, (a) low magnification, (b) high magnification.

[0016] Figure 4 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 1: (a) the first three cycles of charge and discharge curves, (b) cycle performance diagram.

[0017] Figure 5 SEM images of the sample prepared in Example 2, (a) low magnification, (b) high magnification.

[0018] Figure 6 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 2: (a) the first three cycles of charge and discharge curves, (b) cycle performance diagram.

[0019] Figure 7 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 3: (a) the first three cycles of charge and discharge curves, (b) cycle performance diagram.

[0020] Figure 8 SEM images of the sample prepared in Example 4, (a) low magnification, (b) high magnification.

[0021] Fig. 9The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 4: (a) the first three cycles of charge and discharge curves, (b) the cycle performance diagram.

[0022] Fig.10 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 5: (a) the first three cycles of charge and discharge curves, (b) cycle performance diagram.

[0023] Fig.11 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 6: (a) the first three cycles of charge and discharge curves, (b) the cycle performance diagram.

[0024] Fig.12 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 7: (a) the first three cycles of charge and discharge curves, (b) the cycle performance diagram.

[0025] Fig.13 SEM images of the sample prepared in Example 8, (a) low magnification, (b) high magnification.

[0026] Fig.14 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 8: (a) the first three cycles of charge and discharge curves, (b) cycle performance diagram.

[0027] Fig.15 SEM images of the sample prepared in Example 9, (a) low magnification, (b) high magnification.

[0028] Fig.16 The first three cycles of charge and discharge curves and cycle performance diagram of the sample prepared in Example 9: (a) the first three cycles of charge and discharge curves, (b) the cycle performance diagram. DETAILED DESCRIPTION

[0029] Example 1 3.43 mL of 20. wt% acrylic acid solution, 0.1069 g of β-CD, and 0.0298 g of BA (BA accounts for 0.93% of the total mass) were accurately weighed and added to 10 mL of deionized water to form a uniform transparent solution A. 2 mmol of V2O5, 6.2 mmol of Li2CO3, and 10 mmol of C6H 12 N4 was added with 80 mL of deionized water and stirred evenly, and subjected to hydrothermal treatment to obtain a colorless and transparent solution B. Solution A and solution B were mixed and stirred to obtain a uniformly mixed precursor solution, which was then spray-dried to obtain a precursor powder ( Figure 1a). After spray drying is completed, the precursor powder is placed in a nitrogen environment, heated to 550 °C and calcined for 5 hours to obtain a bowl-shaped Li3VO4 / B-NC composite material as a negative electrode material for lithium-ion batteries ( Figure 1 b). The carbonized composite material was analyzed by XRD spectrum, and the obtained diffraction peaks corresponded well to those of Li3VO4 (PDF#38-1247) ( Figure 2 ). During the spray drying process, the material uses the hydroxyl group in BA to react with the carboxylic acid group of acrylic acid to undergo a stable esterification reaction, thereby cross-linking to form a cross-linked network. During the evaporation process, due to the surface tension caused by the cross-linking of BA, the droplets gradually evolve into hollow spheres. The water in the droplets gradually escapes under heating, and the pressure difference on the surface of the hollow sphere increases, causing it to shrink inward, and eventually evolve into a bowl-shaped hemisphere ( Figure 3 a, b). During the sintering process, the phase transformation of Li3VO4 precursor to Li3VO4 and the carbonization of β-cyclodextrin and acrylic acid occur simultaneously to prepare the material. The hollow structure is conducive to the penetration of electrolyte and effectively buffers the volume effect. While effectively relieving stress, the bowl-shaped hemispherical stacking can increase the packing density and shorten the ion transmission path, increasing Li + At the same time, the boron-nitrogen co-doped carbon provides abundant active centers, giving it high capacity and excellent cycle stability.

[0030] The material was made into a battery as follows: the prepared sample was mixed with acetylene black and polyvinylidene fluoride in a weight ratio of 8:1:1, and a slurry was prepared using N-methylpyrrolidone as a solvent. The slurry was coated on a copper foil with a thickness of 10 um, dried at 60 °C for 2 hours, cut into discs with a diameter of 14 mm, and vacuum dried at 120 °C for 10 hours. A metal lithium sheet was used as the counter electrode, a Celgard membrane was used as the diaphragm, and a solution of EC+DMC+DEC (volume ratio of 1:1:1) containing LiPF6 (1 mmol / L) was used as the electrolyte. The CR2025 battery was assembled in an argon-protected glove box. After the battery was assembled, it was left to stand for 8 hours, and then a constant current charge and discharge test was performed using a CT3001 battery test system. The test voltage was 3~0.01 V and the current density was 200 mA g -1 . Figure 4 The first three cycles of charge and discharge curves and cycle performance of the prepared bowl-shaped array Li3VO4 / B-NC lithium-ion battery. The first charge and discharge specific capacities are 813.2 and 1229.5 mAh g -1 ( Figure 4 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 896.7 and 905.6 mAh g, respectively. -1 ( Figure 4 b) exhibits excellent electrochemical performance.

[0031] Example 2 In this example, only the mass of BA in Example 1 is increased to 0.1453 g (BA accounts for 4.36% of the total mass), and the degree of cross-linking is enhanced. During the evaporation process, the water in the cross-linked network escapes under heating, the droplet concentration increases and gradually evolves into a solid sphere ( Figure 5 a), and then obtain the material under the same sintering conditions. The material obtained in Example 2 is made into a battery according to the method of Example 1. Figure 6 As shown in Figure 2, the first charge and discharge specific capacities are 644.6 and 820.1 mAh g -1 ( Figure 6 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 543.9 and 546.7 mAh g, respectively. -1 ( Figure 6 b) Poor electrochemical performance.

[0032] Example 3 In this example, the sintering temperature of the precursor powder in Example 1 was changed from 550°C to 600°C, and the powder was sintered into black particles after spray drying. The material obtained in Example 3 was made into a battery according to the method of Example 1. Figure 7 As shown in Figure 2, the first charge and discharge specific capacities are 500.4 and 756.6 mAh g -1 ( Figure 7 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 551.8 and 557.3 mAh g, respectively. -1 ( Figure 7 b) Poor electrochemical performance.

[0033] Example 4 In this example, 0.0641 g β-CD, 2.05 mL 20 wt.% acrylic acid solution, and 0.0178 g BA (BA accounts for 0.63% of the total mass) were accurately weighed according to stoichiometry, and 6 mL deionized water was added and stirred to obtain solution A. 2 mmol V2O5, 6.2 mmol Li2CO3, and 10 mmol C6H 12 N4 was added with 80 mL of deionized water and stirred evenly. After hydrothermal treatment, a colorless and transparent solution B was obtained. After mixing the A solution with the B solution, the precursor solution was stirred to obtain a uniform mixture, and then spray dried. During the evaporation process, due to the surface tension caused by the cross-linking of BA, a thin layer of hollow spheres was gradually formed. The water in the droplets gradually escaped under heating, and the hollow spheres evolved into a thin layer of bowl-shaped hemispherical arrangement ( Figure 8 a, b), after spray drying, the material was placed in a nitrogen environment and calcined at 550 °C for 5 hours to obtain a material. The material was made into a battery according to the method of Example 1. Fig. 9The first charge and discharge specific capacities were 502.5 and 646.8 mAh g -1 ( Fig. 9 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 487.2 and 490.4 mAh g, respectively. -1 ( Fig. 9 b).

[0034] Example 5 In this example, 0.1069 g β-CD, 3.43 mL 20 wt.% acrylic acid solution, and 0.0298 g BA (BA accounts for 14.15% of the total mass) were accurately weighed according to stoichiometry, added with 10 mL deionized water and stirred evenly to obtain solution A. 1 mmol V2O5, 3.1 mmol Li2CO3, and 5 mmol C6H 12 N4 was added with 40 mL of deionized water and stirred evenly, and a colorless transparent solution B was obtained by hydrothermal treatment. After the A solution and the B solution were mixed, they were stirred to obtain a uniformly mixed precursor solution, and then spray dried. After the spray drying was completed, it was placed in a nitrogen environment, heated to 550 ° C and calcined for 5 hours to obtain the material. It was made into a battery according to the method of Example 1. Fig.10 The first charge and discharge specific capacities were 479.1 and 717.6 mAh g -1 ( Fig.10 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 475.5 and 477 mAh g, respectively. -1 ( Fig.10 b).

[0035] Example 6 In this example, only the sintering temperature of the precursor powder in Example 1 was changed from 550°C to 500°C. The material obtained in Example 6 was made into a battery according to the method of Example 1. Fig.11 As shown in the figure, the first charge and discharge specific capacities are 430.7 and 554.4 mAh g -1 ( Fig.11 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 417.6 and 420.4 mAh g, respectively. -1 ( Fig.11 b).

[0036] Example 7 In this embodiment, only Li2CO3 in Example 1 is replaced with lithium hydroxide (LiOH·H2O), and the material obtained in Example 7 is made into a battery according to the method of Example 1. Fig.12 As shown in Figure 2, the first charge and discharge specific capacities are 448.6 and 678.3 mAh g -1 ( Fig.12 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 494.7 and 499.7 mAh g, respectively. -1 ( Fig.12 b).

[0037] Example 8 This example only uses 50 wt.% acrylic acid solution instead of Example 1, which has a high degree of crosslinking. The prepared sample has a uniformly arranged sphere and a smooth surface ( Fig.13 ). The battery was made according to the method of Example 1. Fig.14 As shown in Figure 2, the first charge and discharge specific capacities are 417.3 and 617.7 mAh g -1 ( Fig.14 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 320.6 and 323.7 mAh g, respectively. -1 ( Fig.14 b).

[0038] Example 9 In this example, BA is not added to the spray-dried precursor solution in Example 1. The morphology of the prepared sample is irregular flakes ( Fig.15 The material obtained in Example 9 was made into a battery according to the method in Example 1. Fig.16 As shown in Figure 2, the first charge and discharge specific capacities are 537.2 and 683.4 mAh g -1 ( Fig.16 a), there are obvious charging and discharging platforms. After 100 cycles, the charging and discharging capacities are 453.2 and 455.6 mAh g, respectively. -1 ( Fig.16 b).

Claims

1. A boron-nitrogen co-doped Li 3 VO 4 / C lithium ion battery negative electrode material preparation method, It is characterized in that The method comprises the following steps: (1) Take β-cyclodextrin, acrylic acid solution, BA, add water and stir evenly to obtain a uniform transparent solution A; (2) Take V 2 O 5 , Li 2 CO 3 , C 6 H 12 N 4 Hydrothermal treatment to obtain colorless and transparent Li 3 VO 4 Precursor solution B; (3) Mix solution A and solution B, stir evenly and spray dry to obtain Li 3 VO 4 / B-NC precursor powder; (4) After spray drying, place the mixture in a nitrogen environment and heat it at 500-600°C for 3-6 hours to obtain Li 3 VO 4 / B-NC composites as negative electrode materials for lithium-ion batteries.

2. The boron-nitrogen co-doped Li according to claim 1 3 VO 4 / C lithium ion battery negative electrode material preparation method, It is characterized in that In step (1), a spray drying precursor solution A is prepared from β-cyclodextrin, acrylic acid solution, and BA, wherein the concentration of the acrylic acid solution is 20 wt.%-50 wt.%, and boric acid accounts for 2 wt.%-15 wt.% of the total mass.

3. The boron-nitrogen co-doped Li according to claim 1 3 VO 4 / C lithium ion battery negative electrode material preparation method, It is characterized in that Step (2) 3 VO 4 Precursor solution B is V 2 O 5 , Li 2 CO 3 , C 6 H 12 N 4 After hydrothermal reaction, Li 2 CO 3 、V 2 O 5 The molar ratio is 3-5:

1.

4. The boron-nitrogen co-doped Li according to claim 1 3 VO 4 / C lithium ion battery negative electrode material preparation method, It is characterized in that In step (3), the volume ratio of solution A to solution B in the mixed solution is 1-5:20, and the inlet temperature of the spray drying is 150-160°C.

5. The boron-nitrogen co-doped Li according to claim 1 3 VO 4 / C lithium ion battery negative electrode material preparation method, It is characterized in that In step (4), the precursor powder is sintered in a nitrogen atmosphere at a heating rate of 3-5°C / min and calcined at 500-600°C for 3-6 hours.

6. Boron-nitrogen co-doped Li 3 VO 4 / C lithium-ion battery negative electrode material, It is characterized in that The method is prepared by any one of claims 1 to 5.