Synergistic ecological overall utilization method for deep sea multi-metal complex minerals
Through the screening and cultivation of deep-sea industrial microorganisms, combined with bioleaching reactor technology, the efficient, low-cost, and environmentally friendly overall utilization of deep-sea polymetallic complex minerals has been achieved, solving the high energy consumption and pollution problems of traditional methods, and realizing the sustainability of resources. Continuous development and closed loops.
Patent Information
- Application Number
- CN202410735993.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
AI Technical Summary
Traditional deep-sea polymetallic complex mineral extraction methods consume high energy and cost, cause pollution to the environment, and cannot efficiently utilize these resources.
Using deep-sea industrial microorganism screening and cultivation, the microbial inoculants are mixed with deep-sea polymetallic complex minerals through a bioleaching reactor to achieve selective leaching and separation of valuable metals, and the leaching residues and deep-sea sediments are synergistically made into building materials or Ecological environment filler.
It achieves efficient, low-cost, and environmentally friendly overall utilization of deep-sea polymetallic complex minerals, solves the high energy consumption and pollution problems of traditional methods, and achieves sustainable development and closed-circuit circulation of resources.
Smart Images

Figure CN118754206A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a mineral processing method, and in particular to a method for coordinated ecological overall utilization of deep-sea polymetallic complex minerals. Background Art
[0002] The bottom of the ocean contains rich strategic mineral resources. Currently, the proven resources with great prospects for commercial exploitation mainly include polymetallic nodules, cobalt-rich crusts and polymetallic sulfides, etc. The reserves of rare metal resources such as copper, cobalt and nickel are far greater than those on land. With the continuous depletion of land resources and the huge demand for rare metals and non-ferrous metals in the emerging new energy industry, the rational development of deep-sea mineral resources is an inevitable choice for promoting the sustainable development of people's livelihood, resources, science and technology, and economy in the future. Deep-sea mineral resource exploration and development technology will be a key factor in measuring a country's comprehensive national strength and cutting-edge scientific and technological level, and it is of great strategic significance for maintaining the security of national marine resources and promoting the construction of a maritime power. Therefore, countries around the world are stepping up research on deep-sea mineral resource development technology in order to accelerate the commercial exploitation of deep-sea minerals. The key core technology of deep-sea mineral resource development is the key to the current deep-sea development field, and it is of great significance to ensure the security of national strategic mineral resources.
[0003] Ocean polymetallic ore is a potential important resource, which contains rich valuable metals such as copper, zinc, nickel, cobalt, etc. However, due to the fine particle size and complex composition of polymetallic ore, the traditional ore extraction method has high energy consumption and high cost when processing such minerals, and cannot efficiently extract its valuable metals. At the same time, the traditional ore extraction method will have a great impact on the environment. Summary of the invention
[0004] Based on the technical problems existing in the above-mentioned prior art, the present invention provides a method for the coordinated ecological overall utilization of deep-sea polymetallic complex minerals, which has a short process flow, high metal recovery rate, and is environmentally friendly, and can achieve the overall utilization of deep-sea polymetallic complex minerals.
[0005] The above objectives are achieved through the following solutions:
[0006] A method for coordinated ecological overall utilization of deep-sea polymetallic complex minerals, wherein the deep-sea polymetallic complex minerals are rich in valuable metals such as manganese, and / or iron, and / or copper, and / or nickel, and / or cobalt, and / or zinc, characterized in that the method comprises the following steps:
[0007] (1) Screening and cultivating microorganisms using collected ocean polymetallic ores to obtain bacterial agents for directional leaching of deep-sea polymetallic complex minerals;
[0008] (2) combining the bacterial agent with a substrate, allowing the bacterial agent to adhere to the substrate to form a medium, and mixing the medium with deep-sea polymetallic complex minerals in a bioleaching reactor to obtain a leachate and a leaching residue;
[0009] (3) The leaching solution is used to prepare metal oxides or ternary precursors, and the leaching residue is synergistically prepared with deep-sea sediments into building materials or ecological environment fillers.
[0010] The method as described above is characterized in that, in step (1), metal ions are added in a targeted manner during the screening and cultivation of microorganisms for domestication.
[0011] The method as described above is characterized in that the medium is reused.
[0012] The method as described above is characterized in that in step (1), the collected deep-sea polymetallic complex minerals are first washed with water purified to meet discharge standards after valuable metals are separated by leaching solution, and part of the sample is taken for screening and cultivation of microorganisms. During the screening and cultivation of microorganisms, iron ions, and / or manganese ions, and / or copper ions, and / or zinc ions are added for directional domestication, and a leaching agent is prepared in a fermentation tank.
[0013] The method as described above is characterized in that the process conditions for screening and culturing microorganisms in step (1) are: pH range is 1.5-10.5, temperature is not higher than 80°C, and the concentration of each added metal ion does not exceed 500 mg / L.
[0014] The method as described above is characterized in that in step (2), large pieces of deep-sea polymetallic complex minerals are first crushed, coarse and fine screened and separated before leaching. During leaching, heap leaching is used for coarse-grained deep-sea polymetallic complex minerals, and tank leaching is used for fine-grained deep-sea polymetallic complex minerals.
[0015] The method as described above is characterized in that in step (2), the leaching process is carried out at normal temperature and pressure.
[0016] The method as described above is characterized in that, during the leaching process, a plurality of pH sensors, and / or pressure sensors, and / or TDS salinity sensors, and / or conductivity sensors, and / or ion strength sensors are respectively placed in the ore pile at different positions in the horizontal direction and the vertical direction to monitor the leaching process.
[0017] The method as described above is characterized in that, in step (3), a precipitant is added to the leaching solution to obtain a precipitate, and then the precipitate is washed, dried, and roasted to obtain a metal oxide.
[0018] The method as described above is characterized in that in step (3), the Ni 2+ 、Co2+ and Mn 2+ The other metal cations except for the above are removed to obtain solution A, and a precipitant is added to solution A to obtain precipitates of nickel, cobalt and manganese to obtain a ternary precursor.
[0019] Beneficial effects of the present invention:
[0020] The method for coordinated ecological overall utilization of deep-sea polymetallic complex minerals of the present invention utilizes deep-sea industrial microorganisms to extract valuable metals from deep-sea minerals. It has a short process, low cost and high recovery rate. It not only solves the problems of high energy consumption, high cost and environmental pollution in traditional ore extraction methods to a certain extent, but also coordinates the resource utilization of leached slag and marine minerals to achieve overall utilization, completes the social cycle of sustainable development of deep-sea minerals, realizes a closed-loop cycle, and utilizes mineral resources and biological resources as a whole.
[0021] The method for the coordinated ecological overall utilization of deep-sea polymetallic complex minerals of the present invention realizes the selective leaching and separation of valuable metals by screening and cultivating microorganisms adapted to the deep-sea environment and utilizing their affinity and metabolic capacity for specific metals.
[0022] Compared with the traditional multi-metal leaching extraction technology, the present invention has the following advantages:
[0023] The biological leaching used is easy to obtain and can be directly screened and cultured from deep-sea polymetallic ores, reducing the load of bacterial agent expansion; in the process of screening and culturing specific microorganisms, various preparations such as microbial precipitants and microbial adsorbents can also be prepared by controlling substrate conditions; the microbial leaching environmental conditions of the present invention have a wide adaptability range and can be directly leached and extracted at normal temperature and pressure; the extraction effect of valuable metals in fine-grained ocean polymetallic ores is better than that of traditional extraction methods; deep-sea microorganisms have higher catalytic ability and strong adaptability; in the leaching and extraction process, no pollutants are generated, and the leaching reaction medium can be reused; due to the low heavy metal content of the bottom slag, the leached slag can be used as building materials or recycled to achieve comprehensive resource utilization.
[0024] In the present invention, deep-sea microorganisms are a highly efficient metal leaching agent, and the process is a closed cycle, which is not only applicable to deep-sea minerals, but can also be extended to the extraction of valuable elements from terrestrial difficult-to-select mineral resources and other secondary resources, thereby turning harm into benefit. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Preparation of MnO for deep-sea polymetallic complex minerals of the present invention 2 Schematic diagram of the process.
[0026] Figure 2 Schematic diagram of the process for preparing ternary precursors from deep-sea polymetallic complex minerals according to the present invention.
[0027] Figure 3 This is a schematic diagram of the process of collaboratively preparing building materials or ecological environment fillers using deep-sea polymetallic complex minerals according to the present invention.
[0028] Figure 4 This is a physical picture of the building material prepared by the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The present invention provides a method for the coordinated ecological overall utilization of deep-sea polymetallic complex minerals, wherein the deep-sea polymetallic complex minerals are rich in valuable metals such as manganese, and / or iron, and / or copper, and / or nickel, and / or cobalt, and / or zinc. The method comprises the following steps:
[0031] (1) Screening and cultivating microorganisms using collected ocean polymetallic ores to obtain bacterial agents for directional leaching of deep-sea polymetallic complex minerals;
[0032] (2) combining the bacterial agent with the substrate, allowing the bacterial agent to adhere to the substrate to form a medium, and mixing the medium with the deep-sea polymetallic complex minerals in a bioleaching reactor to obtain a leachate and a leaching residue;
[0033] (3) The leaching solution is used to prepare metal oxides or ternary precursors, and the leaching residue is synergistically prepared with deep-sea sediments into building materials or ecological environment fillers.
[0034] Wherein, in step (1), metal ions are added in a targeted manner during the screening and cultivation of microorganisms for domestication.
[0035] In the present invention, the substrate can be various organic and inorganic substances, such as biogas, biohydrogen production liquid, straw, molasses and other substances with wide sources and easy to obtain can all be used as substrates.
[0036] The mediator of the present invention can be reused, thereby reducing production costs.
[0037] In step (1), the collected deep-sea polymetallic complex minerals are first washed with water purified and discharged after valuable metals are separated from the leachate in the previous leaching process of other deep-sea polymetallic complex minerals, and some samples are taken for screening and cultivation of microorganisms. During the screening and cultivation of microorganisms, iron ions, and / or manganese ions, and / or copper ions, and / or zinc ions are added for directional domestication, and a leaching agent is prepared in a fermenter. The process conditions for screening and culturing microorganisms are: pH range of 1.5-10.5, temperature not higher than 80°C, and the concentration of each added metal ion does not exceed 500 mg / L.
[0038] In step (2), large pieces of deep-sea polymetallic complex minerals are first crushed, coarse and fine sieving and then leached. During leaching, heap leaching is used for coarse-grained deep-sea polymetallic complex minerals, and tank leaching is used for fine-grained deep-sea polymetallic complex minerals. The leaching process is carried out at normal temperature and pressure, and the cost is low.
[0039] Monitoring the leaching process by analyzing the solution during the leaching process can provide some information about the overall characteristics of the leaching; however, a single solution monitoring cannot determine the degree of oxidation at a specific location in the heap leaching. Multiple pH sensors, and / or pressure sensors, and / or TDS salinity sensors, and / or conductivity sensors, and / or ionic strength sensors are placed in the ore heap at different locations in the horizontal and vertical directions to monitor the leaching process.
[0040] When preparing the metal oxide, a precipitant is added to the leaching solution to obtain a precipitate, which is then washed, dried, and calcined to obtain the metal oxide.
[0041] When preparing the ternary precursor, the Ni 2+ 、Co 2+ and Mn 2+ The other metal cations except for the above are removed to obtain solution A, and a precipitant is added to solution A to obtain precipitates of nickel, cobalt and manganese to obtain a ternary precursor.
[0042] The following specific examples illustrate how to use the method of the present invention to prepare metal oxides and ternary precursor materials, as well as how to prepare building materials or ecological environment fillers.
[0043] Example 1
[0044] Using biogas, biohydrogen production sludge, straw and molasses as substrates, microorganisms that leached manganese were cultivated for leaching of deep-sea manganese nodules. The microbial agent has a wide pH tolerance range and can withstand high physical and chemical shocks. At the same time, the reduction of oxide ores and the biological oxidation of sulfide ores are coupled, which not only greatly reduces the reaction temperature, but also the leaching process is carried out under anaerobic conditions, and the leaching time is greatly shortened to a level equivalent to that of high-temperature reactions. Dilute sulfuric acid and ammonia water are used as pH regulators in the leaching solution, ammonium carbonate / ammonium bicarbonate is used as a precipitant, and MnO is obtained by roasting under aerobic conditions. 2 , the process flow chart is as follows Figure 1 shown.
[0045] Test steps:
[0046] (1) The deep-sea polymetallic complex minerals collected are deep-sea manganese nodules, and their composition is shown in Table 1. First, the final purified aqueous solution is used for washing, and part of the sample is taken for microbial screening and cultivation. During the screening and cultivation of microorganisms, 10 g / L of iron ions, and / or 0-5 g / L of manganese ions, and / or 5 g / L of copper ions, and / or 5 g / L of zinc ions are added for directional domestication, and the leaching agent is prepared in a fermentation tank.
[0047] The following conditions were used to prepare Marine medium (200 ml (NH 4 ) 2 SO 4 0.05g / L, KCl0.05g / L, K 2 HPO 4 0.05g / L, MgSO 4 7H 2 O 0.50g / L, Ca(NO 3 ) 2 0.01g / L, FeSO 4 7H 2 O 10% take 2mL), pH range is 1.5-2.5, the mass ratio of inorganic substrate to organic substrate ranges from 1:1 to 1:3, BOD 5 / COD>0.45;
[0048] Table 1 Analysis results of deep-sea manganese nodules
[0049]
[0050]
[0051] (2) mixing the cultured dissimilatory reducing bacteria and acidophilic bacteria with alcohol wastewater and inorganic substrate to prepare a bacterial agent;
[0052] (3) mixing the bacterial agent with deep-sea manganese nodule ore powder, leaching in a reactor, and obtaining a leachate;
[0053] (4) adjusting the pH of the leaching solution with dilute sulfuric acid and ammonia water, purifying and separating, and using ammonium carbonate / ammonium bicarbonate as a manganese precipitant to obtain manganese carbonate;
[0054] (5) The precipitate is washed and dried, and then calcined at 600°C in the presence of oxygen to obtain MnO 2 .
[0055] The tank leaching test indicators are:
[0056] 1) The mass ratio of deep-sea polymetallic ore: organic-inorganic mixed substrate: leaching agent is 1:0.4:0.3;
[0057] 2) Bioreactor volume 70L;
[0058] 3) Slurry concentration 20%; mineral particle size distribution 92~196μm;
[0059] 4) Inoculation amount 10%; continuous leaching without inoculation;
[0060] 5) pH = 2-7.5;
[0061] 6) Temperature 20-40°C;
[0062] 7) The treated water quality standard reaches Class III surface water standard, and the discharged water that meets the standard can be used as washing water before the subsequent extraction of microorganisms from deep-sea polymetallic mines;
[0063] The experimental results and indicators are shown in Tables 2 and 3.
[0064] Table 2 Results of three cycles of 10kg / day tank immersion experiment
[0065]
[0066]
[0067] Table 3 Manganese sulfate monohydrate (MnSO 4 .H 2 O) Reach GB10648
[0068]
[0069] Embodiment 2:
[0070] Manganese, cobalt and nickel valuable metals are extracted and separated from the leaching solution of Example 1, and a battery ternary precursor material is prepared. The process flow is as follows: Figure 2 The specific steps are:
[0071] (1) Recovery and purification of iron and aluminum in the leachate: Use ammonia water to adjust the pH value to 3-5.5, the temperature to 70-90°C, react for 2-6 hours, and separate the solid and liquid to remove metallic iron and aluminum;
[0072] (2) Recovery and purification of copper in the leachate: adding sulfide to the iron and aluminum removal solution to remove copper ions, the amount of sulfide added is 1-1.6:1 molar ratio of copper in the leachate;
[0073] (3) Recovery and purification of Ca and Mg in the leachate: adding ammonium carbonate or ammonium bicarbonate to the solution in step (2) to perform deep removal of calcium and magnesium, the amount added being 2-3:1 of the mass ratio of calcium to magnesium in the leachate;
[0074] (4) Removal of other metal cations except manganese, cobalt and nickel in the leachate: Use ammonium carbonate or ammonium bicarbonate to adjust the pH value to 5-6, and remove all metal cations except Mn 2+ 、Co 2+ and Ni 2+ The other metal cations are removed by precipitation to obtain solution A;
[0075] (5) Adjusting the molar ratio of nickel, cobalt and manganese in solution A: Using nickel sulfate, cobalt sulfate and manganese sulfate to adjust the nickel content of solution A obtained in step (4) 2+ 、Co 2+ and Mn 2+ The molar ratio is (0.4-0.9):(0.05-0.4):(0.05-0.4), and the pH is adjusted to 5-6 using ammonium carbonate / ammonium bicarbonate and sulfuric acid;
[0076] (6) Precipitating nickel, cobalt and manganese: using ammonia water and ammonium carbonate / ammonium bicarbonate, under a nitrogen atmosphere, at a temperature of 30-60° C., stirring and precipitating for more than 10 hours, after which nickel, cobalt and manganese precipitates are obtained;
[0077] (7) After the precipitation reaction is completed, stop adding materials, maintain the synthesis reaction temperature and atmosphere conditions, and continue stirring for 3-6 hours; (8) After the ternary precursor is synthesized and aged, filter the aged material, wash and dry it to obtain the ternary precursor material.
[0078] Embodiment 3:
[0079] Deep-sea polymetallic mines have natural environmental advantages. Deep-sea polymetallic mine leaching residues, deep-sea sediments and clay minerals are used to prepare marine or coastal ecological environment materials. These materials themselves have the ability to adsorb heavy metal ions. When loaded with microorganisms, they can synergistically process the heavy metal ions released during deep-sea mining. In addition, new building materials can be prepared for walls, floors, roofs and other parts; infrastructure construction, used in infrastructure construction such as oceans, bridges, tunnels, roads, especially in environments that require durability and corrosion resistance; water conservancy and marine engineering, used in water conservancy projects such as dams, sluices, seawalls, and marine engineering such as offshore platforms and artificial islands. The processing process is as follows: Figure 3 As shown, the finished product is as follows Figure 4 The main performance tests are shown in Table 4 and Table 5.
[0080] Among them, deep-sea sediments are a kind of deep-sea mud and deep-sea clay rich in clay minerals, which are an important deep-sea mineral resource.
[0081] The deep-sea polymetallic ore leaching residue and deep-sea sediments of Example 2 are used as aggregates, clay minerals are used as adhesives and to develop diffusion pores, magnesium oxide is used to develop through pores, and sawdust is used as a pore-forming agent (gas generated at high temperature evaporates to form pores). They are mixed in a mass ratio of (5:1.5:1:0.3:1), granulated using a granulator, and then sintered at high temperature (1100°C) for two hours to prepare an artificial ceramic nodule-like material with both strength and porosity. The sawdust particle size is 0.178-0.425mm, and the particle size of the remaining materials is <0.150mm.
[0082] The specific implementation method includes, for example, mixing the slag from filter presses at various levels with a pore-forming agent, stirring evenly, putting into a mold, pressing into 250×70×70mm cuboids and 130×130×130mm cubes at a pressure of 20kg / cm2, and drying the pressed thin plates at room temperature for 48 hours. After drying, the thin plates are placed in a muffle furnace, calcined at a constant temperature of 1100°C for 12 hours, and nitrogen is introduced as a protective gas to ensure an anaerobic environment, thereby obtaining building materials.
[0083] Table 4 Main physical properties test results
[0084] Strength level Porosity / % Density of porous brick / kg / m3 Water absorption / % MU10 21.6 1 600 13.6
[0085] Table 5 Main mechanical and durability performance test results
[0086]
[0087] The above building materials can synergistically treat heavy metal ions released during deep-sea mining. Heavy metal adsorption experiment: The above materials were respectively exposed to 500 mg / L Cu 2+ 、Co 2+and Ni 2+ solution, showing good adsorption capacity for Cu 2+ 、Co 2+ The adsorption amounts of Ni2+ and Ni2+ are 40-50, 35-40 and 35-39 mg / g, respectively. The n value of the Freundlich model fitting can reflect the adsorption capacity of the adsorbent. n<1 means that the adsorption is difficult, and n>1 means that the adsorption is easy. The n values are all greater than 1, indicating that the attachment base is suitable for adsorption and removal of heavy metal ions in water. The thermodynamic parameter Gibbs free energy ΔG calculated by the Langmuir adsorption isotherm parameter KL is negative, which indicates that adsorption will lead to a decrease in Gibbs free energy, indicating that it has more ideal adsorption performance at high temperatures, and the adsorption will proceed spontaneously due to the interaction between molecules. It shows that the overall utilization of deep-sea minerals not only improves the economy, but also improves the environmental protection.
Claims
1. A method for the coordinated ecological overall utilization of deep-sea polymetallic complex minerals, wherein the deep-sea polymetallic complex minerals are rich in valuable metals such as manganese, and / or iron, and / or copper, and / or nickel, and / or cobalt, and / or zinc, characterized in that: The method comprises the following steps: (1) Screening and cultivating microorganisms using the collected deep-sea polymetallic complex minerals to obtain bacterial agents for directional leaching of deep-sea polymetallic complex minerals; (2) combining the bacterial agent with a substrate, allowing the bacterial agent to adhere to the substrate to form a medium, and mixing the medium with deep-sea polymetallic complex minerals in a bioleaching reactor to obtain a leachate and a leaching residue; (3) The leaching solution is used to prepare metal oxides or ternary precursors, and the leaching residue is synergistically prepared with deep-sea sediments into building materials or ecological environment fillers.
2. The method according to claim 1, characterized in that In step (1), metal ions are added in a targeted manner during the screening and cultivation of microorganisms for domestication.
3. The method according to claim 1, characterized in that The mediator is reused.
4. The method according to claim 2, characterized in that In step (1), the collected deep-sea polymetallic complex minerals are first washed with purified water after valuable metals are separated using a leaching solution, and a portion of the sample is taken for screening and culturing of microorganisms. During the screening and culturing of the microorganisms, iron ions, and / or manganese ions, and / or copper ions, and / or zinc ions are added for targeted domestication, and a leaching agent is prepared in a fermentation tank.
5. The method according to claim 4, characterized in that The process conditions for screening and culturing microorganisms in step (1) are as follows: pH range is 1.5-10.5, temperature is not higher than 80° C., and the concentration of each added metal ion does not exceed 500 mg / L.
6. The method according to claim 5, characterized in that In step (2), large pieces of deep-sea polymetallic complex minerals are first crushed, coarse and fine screened and separated before leaching. During leaching, heap leaching is used for coarse-grained deep-sea polymetallic complex minerals, and tank leaching is used for fine-grained deep-sea polymetallic complex minerals.
7. The method according to claim 5, characterized in that In step (2), the leaching process is carried out at normal temperature and pressure.
8. The method according to claim 7, characterized in that During the leaching process, a plurality of pH sensors, and / or pressure sensors, and / or TDS salinity sensors, and / or conductivity sensors, and / or ion strength sensors are respectively placed in the ore pile at different positions in the horizontal direction and the vertical direction to monitor the leaching process.
9. The method according to claim 8, characterized in that In step (3), a precipitant is added to the leaching solution to obtain a precipitate, and then the precipitate is washed, dried, and calcined to obtain a metal oxide.
10. The method according to claim 8, characterized in that In step (3), the Ni in the leaching solution is removed 2+ 、Co 2+ and Mn 2+ The other metal cations except for the above are removed to obtain solution A, and a precipitant is added to solution A to obtain precipitates of nickel, cobalt and manganese, thereby obtaining a ternary precursor.
Citation Information
Cited By
Dredging waste slag resource utilization potential assessment method based on layering characteristics
CN119250657A
Substrate based on deep-sea mining tail cement and shipborne in-situ smelting slag and preparation method
CN122102730A