Fly ash-slag based geopolymer cementing material and preparation method thereof

By combining fly ash and blast furnace granulated slag with modified water glass and Bacillus bacterial solution, high-performance fly ash-slag-based polymer cementitious material was prepared, solving the high energy consumption and the cement-based material The problem of high carbon emissions has achieved the development of waste reuse and low-carbon grouting materials, providing efficient solid waste resource treatment and environmentally friendly construction solutions.

CN118955027APending Publication Date: 2024-11-15HAINAN UNIV +2
View PDF 0 Cites 9 Cited by

Patent Information

Application Number
CN202411028084.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing cement-based grouting materials are high energy consumption and high carbon emissions during the production process, and the chemical grouting materials are mostly toxic substances, making it difficult to achieve the goals of energy conservation, emission reduction and ecological protection. The research on existing geological polymers mainly focuses on raw materials and In alkali-exciting materials, there is a lack of effective solid waste resource reuse and low-carbon grouting materials.

Method used

Using fly ash and blast furnace granulated slag as main components, combined with modified water glass and Bacillus bacterial solution, a fly ash-slag base polymer gelling material was prepared by biological consolidation method, using water glass solution and Sodium hydroxide prepares an exciter to form a high-performance gelling material.

Benefits of technology

It realizes the resource utilization of waste, reduces energy consumption and CO2 emissions, provides high-performance gelling materials, has good permeability and mechanical strength, and has condensation flow characteristics, which is simple to construct and stable and reliable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118955027A_ABST
    Figure CN118955027A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of solid waste resource recycling and green low-carbon cementing materials, in particular to a fly ash-slag based geopolymer cementing material and a preparation method thereof. The material comprises 66-74 parts of fly ash, 28-32 parts of blast furnace granulated slag, 6-7 parts of an exciting agent, 47-52 parts of a solvent and 3-7 parts of bacillus. The preparation method comprises the following steps: preferentially preparing the exciting agent, then mixing the exciting agent with the fly ash and the blast furnace granulated slag, finally inoculating the bacillus, and fully stirring and mixing to form the fly ash-slag based geopolymer cementing material. The method has the advantages that cement is partially replaced; the economical problems of solid waste resource storage and resource application can be effectively solved; a high-performance material with condensation flow characteristics and mechanical strength characteristics is simple and economical in material taking, rapid and convenient to construct and reliable and stable in curing effect; microorganisms are introduced, so that the impermeability is better improved; the curing effect is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource recycling and green low-carbon cementitious materials, and in particular to a fly ash-slag-based polymer cementitious material and a preparation method thereof. Background Art

[0002] Grouting materials can be classified into two categories according to their raw materials: cement-based grouting materials and chemical grouting materials. Cement-based grouting materials are mainly composed of cement, and a large amount of greenhouse gases are emitted during the production of cement. Every ton of cement clinker produced will emit 1 tCO2 due to the decomposition of coal and limestone. It has the disadvantages of high energy consumption and environmental pollution, which will inevitably pose a threat to the ecological environment and seriously hinder the development of my country's construction of a resource-saving and environmentally friendly society. Chemical grouting materials are mainly various chemical resins (such as epoxy resins, polyurethanes, acrylic resins, etc.). For chemical materials, except for water glass (Na2SiO3), all chemical slurries (epoxy resins, acrylates, phenolic resins, polyurethanes, etc.) are toxic. Therefore, it is of great significance to study new grouting materials that are energy-saving, emission-reducing, ecologically friendly, and economically efficient.

[0003] Some microorganisms can produce calcium carbonate deposits on their cell walls through enzymatic action in an anaerobic environment or respiration in an aerobic environment. This technology is used to repair and improve the performance of stone and ordinary cement-based materials. Some people add Bacillus to fly ash modified mortar, and the results show that calcite precipitation deposited on the surface of ordinary concrete can improve its anti-seepage performance.

[0004] Geopolymer is an inorganic polymer material synthesized by silicate and aluminate minerals through chemical reactions in an alkaline environment. This material has a structure and properties similar to traditional cement, but the carbon dioxide emissions generated by its production process are much lower. Through the study of industrial waste materials such as gypsum, lime, slag, and fly ash, it was concluded that it has good performance and potential as a grouting material. At present, the research on geopolymers mainly focuses on raw materials and alkali-activated materials, among which the raw materials are mainly slag, fly ash, gypsum, coal gangue, etc., and the alkali-activated material is mainly water glass. Therefore, the study of geopolymer-solidified soil as a grouting material can realize the resource utilization of waste and reduce construction costs, reduce energy consumption and CO2 emissions, which is beneficial to the environment and has great significance for the current development of my country. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a fly ash-slag based polymer gelling material and a preparation method thereof.

[0006] The first object of the present invention is to provide a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0007] 66-80 parts of fly ash;

[0008] 28-36 parts of blast furnace granulated slag;

[0009] 6-7 parts of stimulant;

[0010] 47-56 parts of solvent;

[0011] 3-10 parts of Bacillus;

[0012] The activator is modified water glass obtained by mixing water glass solution and sodium hydroxide particles, and the modulus of the modified water glass is 1.2-1.6.

[0013] Preferably, the Bacillus is Bacillus pasteurianus;

[0014] The water glass solution comprises the following components in mass fractions: 29.5-30.0% silicon dioxide, 13.5-14.0% sodium hydroxide and 56.0-56.5% water.

[0015] Preferably, the particle size of fly ash is 1-100 μm, and the specific surface area is 300-420 m 2 / Kg or density is 1.8~2.3g / cm 3 .

[0016] Preferably, the particle size of the blast furnace granulated slag is 0.01 to 120 μm, and the specific surface area is 400 to 500 m 2 / Kg or density is 2.67~3.33g / cm 3 .

[0017] Preferably, the solvent is water, with a pH value of ≥4.5; the sodium hydroxide particles in the activator are of analytical grade, with a solid content of 95-99%.

[0018] Preferably, the modulus of the modified water glass is 1.3.

[0019] Preferably, the fly ash is 70 parts, the blast furnace granulated slag is 30 parts, the activator is 6.5 parts, the solvent is 48 parts, and the Bacillus is 5 parts.

[0020] The second object of the present invention is to provide a method for preparing a fly ash-slag based polymer cementitious material, which specifically comprises the following steps:

[0021] S1. Weigh fly ash, blast furnace granulated slag, water glass solution, sodium hydroxide particles, solvent and Bacillus according to each weight portion;

[0022] S2. The sodium hydroxide particles are slowly added to the water glass solution, and the addition process is continuously stirred and exothermic until completely dissolved. After the solution is stabilized, the film is cooled to room temperature to prepare an activator;

[0023] S3. Stir the fly ash and blast furnace granulated slag thoroughly for 3 to 5 minutes until they are evenly mixed;

[0024] S4. The activator and solvent are added to the mixed powder of step S3 and stirred until the slurry is uniformly stirred;

[0025] S5. Prepare a spore-forming bacteria liquid, inoculate it into the mixed slurry in step S4, and stir again for 3 to 5 minutes until it is completely stirred and uniform, so as to obtain a fly ash-slag-based polymer cementitious material.

[0026] Preferably, the stirring in steps S3, S4 and S5 has a rotation speed of 110 to 130 r / min.

[0027] Preferably, the Bacillus bacterial solution is Bacillus pasteurian bacterial solution, and the urease activity of the Bacillus pasteurian bacterial solution is 1.6 mM urea hydrolysed / min.

[0028] Compared with the prior art, the present invention can achieve the following beneficial effects:

[0029] In the prior art, cement-based cementitious materials are often used to reinforce soft soil layers, which will face the problems of high energy consumption and increased carbon emissions, and cause multiple negative impacts on the ecological environment. The fly ash used in the present invention is a powder produced when concrete is crushed, which can promote the utilization of waste concrete, realize waste recycling, and is conducive to saving energy consumption, and partially replace cement; combining blast furnace slag and alkali to make geopolymer cementitious materials for soft soil reinforcement can also achieve a curing effect equivalent to that of cement-based cementitious materials, which can effectively solve the economic problems of solid waste resource storage and resource utilization; and adding Bacillus liquid to the cementitious material combined with the biological consolidation method can greatly make up for the lack of ductility of the geopolymer cementitious material, and better improve its impermeability; the curing effect is good. In summary, the present invention is a high-performance material with both coagulation flow characteristics and mechanical strength characteristics. The material is simple and economical, the construction is quick and convenient, and the curing effect is reliable and stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 The present invention is a flowchart of a method for preparing a fly ash-slag based polymer cementitious material according to an embodiment of the present invention. DETAILED DESCRIPTION

[0031] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In the following description, the same modules are represented by the same reference numerals. In the case of the same reference numerals, their names and functions are also the same. Therefore, the detailed description thereof will not be repeated.

[0032] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.

[0033] Example 1

[0034] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0035] Fly ash: 68 parts;

[0036] Blast furnace granulated slag: 28 parts;

[0037] Exciter: 6.1 parts;

[0038] Solvent: 50 parts;

[0039] Bacillus: 3 parts;

[0040] The activator is a modified water glass prepared by mixing a water glass solution and sodium hydroxide particles. The water glass solution includes the following components by mass fraction: 29.9% silicon dioxide (SiO2), 13.75% sodium hydroxide (NaOH) and 56.35% water (H2O); the sodium hydroxide particles are of analytical grade with a solid content of 99%; the modified water glass modulus is 1.3.

[0041] The particle size of fly ash is less than 10 μm; the specific surface area of ​​fly ash is 410.2 m 2 / Kg or density is 2.31g / cm 3 The chemical composition is 48.88% SiO2, 30.29% Al2O3, 8.92% CaO, 0.55% MgO, 6.89% Fe2O3, 0.50% SO3, 0.32% Na2O, 1.26% K2O, 1.93% TiO2, and LOI (loss on ignition) is 28%.

[0042] The particle size of the blast furnace granulated slag is less than 120 μm; the specific surface area of ​​the blast furnace granulated slag is 467.40 m 2 / Kg, density is 3.01g / cm 3 ; The chemical composition is 30.41% SiO2, 15.26% Al2O3, 41.07% CaO, 8.33% MgO, 0.34% Fe2O3, 2.07% SO3, 0.46% Na2O, 0.46% K2O, 0.72% TiO2, 0.12% P2O5, 0.83% others, and the balance is loss on ignition.

[0043] The solvent is water, pH value ≥ 4.5, insoluble matter ≤ 10000 mg / L, soluble matter ≤ 10000 mg / L, chloride (as Cl - ≤3500mg / L, sulfate (as SO4 2- Calculated) ≤2700mg / L.

[0044] Urease activity of Bacillus pasteurianus culture 1.3mM urea hydrolysed / min, OD 600 The value is 2.4.

[0045] The preparation method specifically comprises the following steps:

[0046] S1. Weigh fly ash, blast furnace granulated slag, water glass, sodium hydroxide, solvent and Bacillus according to their weight parts:

[0047] S2. Slowly add the sodium hydroxide particles to the water glass, stirring and releasing heat during the addition process until the solution is completely dissolved, and after the solution is stabilized, the film is cooled to room temperature to prepare an activator;

[0048] S3. Stir the fly ash and slag powder for 3 to 5 minutes until they are evenly mixed. The speed during stirring is 120 ± 10 r / min;

[0049] S4. The activator and solvent are added to the fly ash and slag powder mixture obtained in step S3 and stirred for at least 10 min until the slurry is uniformly stirred, and the speed during stirring is 120 ± 10 r / min;

[0050] S5. Prepare a spore-forming bacteria liquid, inoculate it into the mixed slurry in step S4, and stir it again for 3 to 5 minutes until it is completely stirred and uniform, so as to obtain a fly ash-slag-based polymer cementitious material. The rotation speed during stirring is 120±10r / min.

[0051] The prepared fly ash-slag base polymer slurry will be tested for its slurry fluidity, initial setting and final setting time, and its 28d unconfined compressive strength and 28d flexural strength under standard curing conditions (20±1°C, humidity 85%) will be tested.

[0052] Various testing methods and processes:

[0053] The fluidity of geopolymer slurry is measured according to the standard "Test Method for Homogeneity of Concrete Admixtures" (GB / T8077-2012). The stirred geopolymer slurry is quickly injected into a truncated cone mold (upper inner diameter 36mm×lower inner diameter 60mm×height 60mm). The mold is lifted vertically for 30 seconds. The maximum diameters in two perpendicular directions are measured with a ruler, and the average value is taken as the fluidity of the geopolymer slurry.

[0054] The setting time of geopolymer slurry is measured with reference to the standard "Test Method for Water Consumption, Setting Time and Soundness of Cement Standard Consistency" (GBT1346-2011). During the test, the specimen is taken out of the moisture curing box and placed under the initial setting test needle of the standard Favica instrument. When the test needle sinks to 4mm±1mm from the bottom plate, it is the initial setting time of the slurry. Then replace it with the final setting needle of the annular attachment. When the annular attachment begins to leave no trace on the specimen, it is the final setting time of the clean slurry.

[0055] The unconfined compressive strength and flexural strength tests are tested in accordance with the "Test Method for Strength of Cement Mortar (ISO Method)" (GB / T17671-2021). The evenly stirred geopolymer slurry is divided into two layers and loaded into a 40mm×40mm×160mm prism triple mold and vibrated for 30 seconds. It is quickly placed in a curing room for curing for 2 hours (temperature 20±1℃, relative humidity not less than 85%), demolded, and cured for 28 days. The flexural strength and unconfined compressive strength of the test block are tested successively. The cement mortar test hydraulic press is used to load at a rate of 10mm / min. The flexural strength is taken as the average strength of three prisms, and the unconfined compressive strength is taken as the average strength of six broken half prisms. If a test block deviates from the mean by more than 10%, this group of test blocks shall be redone.

[0056] Test results: The initial setting and final setting times of the fly ash-slag-based polymer obtained according to the proportion of the components in this group are 135min and 190min respectively. According to the "General Portland Cement" (GB175-2007) specification, it can meet the requirements of cement paste for initial setting time ≥45min and final setting time ≤6h. The fluidity is 215mm, with good slurry fluidity. The unconfined compressive strength of the test block under 28d standard curing conditions is 45.32MPa, and the flexural strength is 5.29MPa. Fly ash can be effectively dissolved in the water glass solution under the flocculation and synergistic effect of slag, providing the [SiO4] and [AlO4] tetrahedral units required for the polymerization reaction and additional Ca 2 + nucleation sites, combined with the free SiO3 provided by water glass 2- and Na + , promoting the geopolymer system to form a hybrid bonding cement composed of gels such as C-(N)-ASH and C-(A)-SH, thereby forming a dense and compact microstructure and providing the required strength for the sample.

[0057] Example 2

[0058] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0059] Fly ash: 68 parts;

[0060] Blast furnace granulated slag: 29 parts;

[0061] Exciter: 6.2 parts;

[0062] Solvent: 49 parts;

[0063] Bacillus: 4 parts;

[0064] Modified water glass modulus: 1.3;

[0065] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the fly ash-slag based polymer gelling material is the same as that in Example 1.

[0066] Measurement results: The initial and final setting times of the fly ash-slag-based polymer obtained according to the proportion of components in this group are 128 min and 179 min respectively, the fluidity is 210 mm, and the unconfined compressive strength of the test block under 28 days of standard curing conditions is 49.12 MPa, and the flexural strength is 4.88 MPa.

[0067] Example 3

[0068] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0069] Fly ash: 68 parts;

[0070] Blast furnace granulated slag: 30 parts;

[0071] Exciter: 6.3 parts;

[0072] Solvent: 51 parts;

[0073] Bacillus: 5 parts;

[0074] Modified water glass modulus: 1.3;

[0075] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the fly ash-slag based polymer gelling material is the same as that in Example 1.

[0076] Measurement results: The initial and final setting times of the fly ash-slag-based polymer obtained according to the proportion of components in this group are 121 min and 178 min respectively, the fluidity is 211 mm, and the unconfined compressive strength of the test block under 28 days of standard curing conditions is 48.13 MPa, and the flexural strength is 3.97 MPa.

[0077] Example 4

[0078] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0079] Fly ash: 70 parts;

[0080] Blast furnace granulated slag: 31 parts;

[0081] Exciter: 6.6 parts;

[0082] Solvent: 51 parts;

[0083] Bacillus: 6 parts;

[0084] Modified water glass modulus: 1.3;

[0085] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the fly ash-slag based polymer gelling material is the same as that in Example 1.

[0086] Measurement results: The initial and final setting times of the fly ash-slag-based polymer obtained according to the proportion of components in this group are 97min and 135min respectively, the fluidity is 199mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 50.25MPa, and the flexural strength is 4.85MPa.

[0087] Example 5

[0088] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0089] Fly ash: 73 parts;

[0090] Blast furnace granulated slag: 32 parts;

[0091] Exciter: 6.7 parts;

[0092] Solvent: 52 parts;

[0093] Bacillus: 7 parts;

[0094] Modified water glass modulus: 1.3;

[0095] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the fly ash-slag based polymer gelling material is the same as that in Example 1.

[0096] Measurement results: The initial and final setting times of the fly ash-slag-based polymer obtained according to the proportion of components in this group are 68 min and 98 min respectively, the fluidity is 195 mm, and the unconfined compressive strength of the test block under 28 days of standard curing conditions is 51.25 MPa, and the flexural strength is 5.69 MPa.

[0097] Example 6

[0098] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0099] Fly ash: 75 parts;

[0100] Blast furnace granulated slag: 32 parts;

[0101] Exciter: 6.8 parts;

[0102] Solvent: 53 parts;

[0103] Bacillus: 8 parts;

[0104] Modified water glass modulus: 1.3;

[0105] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the fly ash-slag based polymer gelling material is the same as that in Example 1.

[0106] Measurement results: The initial and final setting times of the fly ash-slag-based polymer obtained according to the proportion of components in this group are 68 min and 95 min respectively, the fluidity is 192 mm, and the unconfined compressive strength of the test block under 28 days of standard curing conditions is 52.79 MPa, and the flexural strength is 5.71 MPa.

[0107] Example 7

[0108] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0109] Fly ash: 77 parts;

[0110] Blast furnace granulated slag: 32 parts;

[0111] Exciter: 6.9 parts;

[0112] Solvent: 55 parts;

[0113] Bacillus: 9 parts;

[0114] Modified water glass modulus: 1.3;

[0115] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the fly ash-slag based polymer gelling material is the same as that in Example 1.

[0116] Measurement results: The initial and final setting times of the fly ash-slag based polymer obtained according to the proportion of components in this group are 65min and 100min respectively, the fluidity is 190mm, and the unconfined compressive strength of the test block under 28d standard curing conditions is 50.30MPa, and the flexural strength is 4.82MPa.

[0117] Example 8

[0118] This embodiment provides a fly ash-slag based polymer cementitious material, comprising the following components in parts by weight:

[0119] Fly ash: 79 parts;

[0120] Blast furnace granulated slag: 36 parts;

[0121] Stimulant: 7 parts;

[0122] Solvent: 56 parts;

[0123] Bacillus: 10 parts;

[0124] Modified water glass modulus: 1.3;

[0125] The physical and chemical indicators of the components are the same as those in Example 1; the preparation method of the fly ash-slag based polymer gelling material is the same as that in Example 1.

[0126] Measurement results: The initial and final setting times of the fly ash-slag-based polymer obtained according to the proportion of components in this group are 62 min and 97 min respectively, the fluidity is 188 mm, and the unconfined compressive strength of the test block under 28 days of standard curing conditions is 48.32 MPa, and the flexural strength is 3.98 MPa.

[0127] In summary, the weight percentage of fly ash should be less than 75 parts, because too high a weight percentage of fly ash will reduce the strength of geopolymer. Considering the economic efficiency, working performance and strength growth benefits, the weight percentage of blast furnace granulated slag is more suitable at 29-32 parts, and the weight percentage of the activator is 6.3-6.9 parts, which can make the fly ash-slag base polymer slurry obtain a suitable setting time and good fluidity of the geopolymer slurry. The setting rate of the slurry first slows down and then speeds up with the increase of the modulus. Reducing the modulus can improve the fluidity of the geopolymer slurry, but in general, the modulus does not have a significant effect on the working performance of the slurry system.

[0128] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the disclosure of the present invention can be performed in parallel, sequentially or in different orders, as long as the desired results of the technical solution disclosed in the present invention can be achieved, and this document does not limit this.

[0129] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. Fly ash-slag based polymer cementitious material, characterized in that: The composition includes the following components in parts by weight: 66-80 parts of fly ash; 28-36 parts of blast furnace granulated slag; 6-7 parts of stimulant; 47-56 parts of solvent; 3-10 parts of Bacillus; The activator is modified water glass obtained by mixing water glass solution and sodium hydroxide particles, and the modulus of the modified water glass is 1.2-1.

6.

2. The fly ash-slag based polymer cementitious material according to claim 1, characterized in that: The bacillus is Bacillus pasteurianus; The water glass solution comprises the following components in mass fractions: 29.5-30.0% silicon dioxide, 13.5-14.0% sodium hydroxide and 56.0-56.5% water.

3. The fly ash-slag based polymer cementitious material according to claim 2, characterized in that: The particle size of the fly ash is 1-100 μm, and the specific surface area is 300-420 m 2 / Kg or density is 1.8~2.3g / cm 3 .

4. The fly ash-slag based polymer cementitious material according to claim 3, characterized in that: The particle size of the blast furnace granulated slag is 0.01-120 μm, and the specific surface area is 400-500 m 2 / Kg or density is 2.67~3.33g / cm 3 .

5. The fly ash-slag based polymer cementitious material according to claim 4, characterized in that: The solvent is water, with a pH value of ≥4.5; the sodium hydroxide particles in the activator are of analytical grade, with a solid content of 95-99%.

6. The fly ash-slag based polymer cementitious material according to claim 5, characterized in that: The modified water glass modulus is 1.

3.

7. The fly ash-slag based polymer cementitious material according to claim 6, characterized in that: The fly ash is 70 parts, the blast furnace granulated slag is 30 parts, the activator is 6.5 parts, the solvent is 48 parts, and the Bacillus is 5 parts.

8. The method for preparing the fly ash-slag based polymer cementitious material according to any one of claims 1 to 7, characterized in that: The specific steps include: S1. Weigh fly ash, blast furnace granulated slag, water glass solution, sodium hydroxide particles, solvent and Bacillus according to each weight portion; S2. The sodium hydroxide particles are slowly added to the water glass solution, and the addition process is continuously stirred and exothermic until completely dissolved. After the solution is stabilized, the film is cooled to room temperature to prepare an activator; S3. Stir the fly ash and blast furnace granulated slag thoroughly for 3 to 5 minutes until they are evenly mixed; S4. The activator and solvent are added to the mixed powder of step S3 and stirred until the slurry is uniformly stirred; S5. Prepare a spore-forming bacteria liquid, inoculate it into the mixed slurry in step S4, and stir again for 3 to 5 minutes until it is completely stirred and uniform, so as to obtain a fly ash-slag-based polymer cementitious material.

9. The method for preparing the fly ash-slag based polymer cementitious material according to claim 8, characterized in that: The stirring described in steps S3, S4 and S5 has a rotation speed of 110 to 130 r / min.

10. The method for preparing the fly ash-slag based polymer cementitious material according to claim 9, characterized in that: The Bacillus bacterial liquid is Bacillus pasteurianus bacterial liquid, and the urease activity of the Bacillus pasteurianus bacterial liquid is 1.6 mM ureahydrolysed / min.

Citation Information

Cited By

  • Medical solid waste-based geopolymer material as well as preparation method and application thereof

    CN119504163A

  • A medical solid waste-based polymer material and its preparation method and application

    CN119504163B

  • Method for increasing compression resistance of geopolymer based on urease induced calcium carbonate precipitation

    CN119735394A

  • Method for increasing the compressive strength of geopolymer based on urease-induced calcium carbonate precipitation

    CN119735394B

  • Coal gangue-biomass ash-based micro mineral gel material and alkali-free dry-process base layer preparation method

    CN120535247A