Positive electrode active material precursor, preparation method, positive electrode active material, positive plate and battery

By designing a cobalt-free cathode active material precursor with the chemical formula NixMny(OH)2 and controlling its surface whisker morphology and internal structure, the problem of high cobalt element price and whisker shedding and stickiness in lithium batteries has been solved, and the Coulomb performance of the battery has been improved. efficiency and cycle performance, reducing material costs.

CN118754209APending Publication Date: 2024-10-11NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410756778.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The cobalt element in existing lithium battery cathode materials is expensive, and precursor materials with high specific surface areas are prone to whisker shedding and sticking problems during the sintering process, affecting the electrochemical performance of the battery.

Method used

The cobalt-free cathode active material precursor with the chemical formula NixMny(OH)2 is used to design the porosity of the core layer, transition layer, middle layer and outer layer by controlling the aspect ratio, stacking degree, curvature and particle size of the surface whiskers. Distribute to prepare a precursor with a stable structure, reducing whisker shedding and sticking.

Benefits of technology

It effectively suppresses the phenomenon of whisker shedding and sticking, improves the Coulombic efficiency and cycle performance of the battery, and reduces the material cost, especially by improving the structural stability and capacity performance of the manganese-rich precursor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754209A_ABST
    Figure CN118754209A_ABST
Patent Text Reader

Abstract

The invention provides a positive active material precursor, a preparation method, a positive active material, a positive plate and a battery. The chemical composition of the positive electrode active material precursor does not use a cobalt element, the cost is reduced, the length-diameter ratio of surface whiskers is 5-15, the stacking degree is lower than 80, the phenomena of whisker falling and whisker adhesion occurring in the sintering process of the positive electrode active material precursor are obviously inhibited, and the performance of the positive electrode active material precursor is improved. And the anode active material obtained by sintering has excellent cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a positive electrode active material precursor, in particular to a positive electrode active material precursor, a preparation method, a positive electrode active material, a positive electrode sheet and a battery, belonging to the technical field of lithium ion battery materials. Background Art

[0002] The ternary precursor materials for lithium batteries are mainly composed of three metal elements: nickel, cobalt and manganese. The price of cobalt has remained high all year round, which has seriously hindered the popularization of lithium batteries. Therefore, preparing low-cobalt or cobalt-free precursor materials is an important way to solve this problem.

[0003] The stability of the whisker morphology of the precursor material has an important influence on its sintering performance. Some positive electrode materials have high requirements for the specific surface area of ​​the precursor. Generally speaking, the whisker morphology of the precursor material with a high specific surface area is poorly stable, and problems such as whisker shedding and sticking are prone to occur during the sintering process, which seriously affects the performance of the positive electrode active material and thus affects the electrochemical performance of the battery.

[0004] A cobalt-free positive electrode active material precursor that is not prone to problems such as whisker shedding and sticking during sintering has good application prospects. Summary of the invention

[0005] The present invention provides a positive electrode active material precursor, a preparation method, a positive electrode active material, a positive electrode sheet and a battery. The whisker shedding and whisker sticking phenomena occurring during the sintering process of the positive electrode active material precursor are significantly suppressed. Therefore, the positive electrode active material precursor of the present invention improves the coulombic efficiency and cycle performance of the battery by maintaining the structural integrity of the positive electrode active material.

[0006] The present invention also provides a method for preparing a positive electrode active material precursor. By means of the preparation method, a positive electrode active material precursor can be prepared, and the whisker shedding and whisker sticking phenomena occurring during the sintering process of the positive electrode active material precursor are significantly suppressed.

[0007] The present invention also provides a positive electrode active material, the surface whisker morphology of the positive electrode active material is complete, which is beneficial to improving the coulombic efficiency and cycle performance of the battery.

[0008] The present invention also provides a positive electrode sheet, which comprises the positive electrode active material.

[0009] The present invention also provides a lithium ion battery, which comprises the positive electrode sheet and has good coulombic efficiency and cycle performance.

[0010] The first aspect of the present invention provides a positive electrode active material precursor, wherein the chemical formula of the positive electrode active material precursor is: Ni x Mny (OH)2, where 0<x<1, 0<y<1, x+y=1;

[0011] The aspect ratio of the whiskers on the surface of the positive electrode active material precursor is 5-15, and the stacking degree is less than 80.

[0012] The positive electrode active material precursor as described above, wherein the curvature of the surface whiskers is less than 15°; and / or the particle size of the positive electrode active material precursor is 5-15 μm; and / or the length of the surface whiskers is 0.1-0.8 μm.

[0013] The positive electrode active material precursor as described above, wherein, in the field of view of a scanning electron microscope with a magnification of 1000, the proportion of fine powder in the positive electrode active material precursor is not higher than 12%; wherein, the fine powder is the part of the positive electrode active material precursor with a particle size lower than 1 / 2 of the positive electrode active material precursor D50.

[0014] The positive electrode active material precursor as described above, wherein the positive electrode active material precursor comprises a core layer, a transition layer, an intermediate layer and an outer layer in the radial direction from the inside to the outside, the widths of the core layer, the transition layer, the intermediate layer and the outer layer are R1, R2, R3 and R4 respectively, the particle size of the positive electrode active material precursor is R, R1+R2+R3+R4=1 / 2*R, and R1=(6%-8%)*R, R2=(1%-2%)*R, R3=(24%-26%)*R, R4=(15%-16%)*R;

[0015] The average porosity of the core layer, transition layer, middle layer and outer layer decreases in sequence.

[0016] The positive electrode active material precursor as described above, wherein the average porosity of the core layer, transition layer, intermediate layer and outer layer are 25%-30%, 20%-25%, 15%-20% and 5%-10% respectively.

[0017] The second aspect of the present invention provides a method for preparing a positive electrode active material precursor according to the first aspect, wherein the preparation method comprises a first stage, a second stage, a third stage and a fourth stage;

[0018] In the first stage, the rotation speed of the reaction system is 500-600 rpm, the pH is 10.5-11.0, the oxygen content is 0.70%-0.90%, the solid content is 0-100 g / L, the feed flow rate of the metal salt solution is 3-4 L / h, and the D50 of the first intermediate product satisfies: 12%*target particle size<D50 of the first intermediate product<16%*target particle size;

[0019] In the second stage, the speed of the reaction system is 400-500 rpm, the pH is 10.0-10.5, the oxygen content is 0.90%-1.1%, the solid content is 100-150 g / L, the feed flow rate of the metal salt solution is 4-5 L / h, and the D50 of the second intermediate product satisfies: 14%*target particle size<D50 of the second intermediate product<20%*target particle size;

[0020] In the third stage, the rotation speed of the reaction system is 300-400 rpm, the pH is 9.8-10.2, the oxygen content is 1.2%-1.5%, the solid content is 150-250 g / L, the feed flow rate of the metal salt solution is 5-6 L / h, and the D50 of the third intermediate product satisfies: 62%*target particle size<D50 of the third intermediate product<72%*target particle size;

[0021] In the fourth stage, the rotation speed of the reaction system is 200-300 rpm, the pH is 9.9-10.3, the oxygen content is 1.0%-1.3%, the solid content is greater than 250 g / L, and the feed flow rate of the metal salt solution is 5-6 L / h. When the D50 of the fourth intermediate product is the target particle size, the reaction system is aged, washed with water, and centrifuged to obtain the positive electrode active material precursor;

[0022] The reaction system includes the metal salt solution and a precipitant, the metal salt solution includes a mixed solution of nickel salt and manganese salt with a total molar concentration of 1.5-2.0 mol / L, the molar ratio of nickel to manganese is x:y, 0<x<1, 0<y<1, and x+y=1.

[0023] The preparation method as described above, wherein the pH of the reaction system in the second stage and the fourth stage is greater than the pH of the reaction system in the third stage; and / or the oxygen content of the reaction system in the second stage is higher than the oxygen content of the reaction system in the first stage, and the oxygen content of the reaction system in the third stage is higher than the oxygen content of the reaction system in the second stage and the fourth stage.

[0024] The third aspect of the present invention provides a positive electrode active material, wherein the positive electrode active material is formed by the positive electrode active material precursor described in the first aspect or the positive electrode active material precursor prepared by the preparation method described in the second aspect.

[0025] A fourth aspect of the present invention provides a positive electrode sheet, wherein the positive electrode sheet comprises the positive electrode active material described in the third aspect.

[0026] A fifth aspect of the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the positive electrode sheet described in the fifth aspect.

[0027] The present invention provides a positive electrode active material precursor, a preparation method, a positive electrode active material, a positive electrode sheet and a battery, the chemical formula of which is: Ni x Mn y (OH)2, wherein 0<x<1, 0<y<1, x+y=1; the aspect ratio of the whiskers on the surface of the positive electrode active material precursor is 5-15, and the stacking degree is lower than 80. The whisker shedding and whisker sticking phenomena occurring during the sintering process of the positive electrode active material precursor are significantly suppressed. Therefore, the positive electrode active material precursor of the present invention improves the coulombic efficiency and cycle performance of the battery by maintaining the structural integrity of the positive electrode active material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0029] Figure 1 This is a scanning electron microscope image of the positive electrode active material precursor of Example 1 at a magnification of 10000;

[0030] Figure 2 This is a scanning electron microscope image of the positive electrode active material precursor of Example 1 at a magnification of 1000;

[0031] Figure 3 This is a cross-sectional scanning electron microscope image of the positive electrode active material precursor of Example 1 at a magnification of 9000;

[0032] Figure 4 This is a scanning electron microscope image of the positive electrode active material prepared from the positive electrode active material precursor of Example 1 at a magnification of 30,000;

[0033] Figure 5 This is a scanning electron microscope image of the positive electrode active material prepared from the positive electrode active material precursor of Example 1 at a magnification of 5000;

[0034] Figure 6 This is a scanning electron microscope image of the positive electrode active material precursor of Comparative Example 1 at a magnification of 1000;

[0035] Figure 7 This is a scanning electron microscope image of the positive electrode active material precursor of Comparative Example 1 at a magnification of 10000;

[0036] Figure 8 This is a cross-sectional scanning electron microscope image of the positive electrode active material precursor of Comparative Example 1 at a magnification of 9000;

[0037] Fig. 9 This is a scanning electron microscope image of the positive electrode active material prepared from the positive electrode active material precursor of Comparative Example 1 at a magnification of 5000;

[0038] Fig.10 This is a scanning electron microscope image of the positive electrode active material precursor of Comparative Example 2 at a magnification of 1000;

[0039] Fig.11 This is a scanning electron microscope image of the positive electrode active material precursor of Comparative Example 2 at a magnification of 10,000. DETAILED DESCRIPTION

[0040] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The first aspect of the present invention provides a positive electrode active material precursor, the chemical formula of the positive electrode active material precursor is: Ni x Mn y (OH)2, where 0<x<1, 0<y<1, x+y=1;

[0042] The aspect ratio of the whiskers on the surface of the positive electrode active material precursor is 5-15, and the stacking degree is less than 80.

[0043] In a specific embodiment, the scanning electron microscope image of the positive electrode active material precursor at a magnification of 10000 is as follows: Figure 1 As shown, the surface whiskers of the above-mentioned positive electrode active material precursor are clearly seen.

[0044] The stacking degree reflects the number of whiskers on the surface of the positive electrode active material precursor particles, which can be obtained through the following process:

[0045] 1) adjusting the magnification parameters of the scanning electron microscope so that only a single complete positive electrode active material precursor particle appears in the field of view of the scanning electron microscope, and the whiskers on its surface can be clearly and accurately counted; obtaining a scanning electron microscope image of the positive electrode active material precursor particle;

[0046] 2) The area of ​​the above-mentioned single complete positive electrode active material precursor particle in the scanning electron microscope image can be approximated as a circle with a diameter of R. A circle with a diameter of r is drawn with the center of the circle as the center, where r = 1 / 10R. The surface whiskers of the precursor particles in the above circle are counted, and the number of surface whiskers in the above circle is obtained, which is the stacking degree.

[0047] The inventors found that when the aspect ratio of the whiskers on the surface of the positive electrode active material precursor is 5-15 and the stacking degree is lower than 80, the whiskers are not easy to fall off and the whiskers are not easy to stick during the sintering process of the positive electrode active material precursor. The positive electrode active material prepared using the positive electrode active material precursor has good processing performance, stable structure, and is not easy to break. The coulombic efficiency and cycle performance of the battery are improved. This may be because the aspect ratio of the whiskers on the surface of the above-mentioned positive electrode active material precursor is 5-15 and the stacking degree is lower than 80, which is conducive to improving the strength of the surface whiskers, so that the positive electrode active material precursor has a strong and stable surface whisker morphology, and thus the surface whiskers are not easy to break and fall off and the whiskers are not easy to stick during the sintering process. At the same time, the overall strength of the positive electrode active material precursor particles is improved, which is conducive to maintaining the structural integrity of the positive electrode active material, thereby improving the coulombic efficiency and cycle performance of the battery.

[0048] The whisker shedding and whisker sticking phenomena of the positive electrode active material precursor of the present invention during the sintering process are significantly suppressed. Therefore, the positive electrode active material precursor of the present invention improves the coulombic efficiency and cycle performance of the battery by maintaining the structural integrity of the positive electrode active material.

[0049] Since nickel is a rare and precious metal, domestic nickel mineral resources are scarce, while the output of manganese is relatively large, the content of Ni and Mn in the chemical formula of the positive electrode active material precursor can be further limited to 0<x<0.5, 0.5<y<1, x+y=1, and a manganese-rich precursor is obtained. The material cost of the manganese-rich precursor is reduced, and due to the high manganese content, it is beneficial to improve the structural stability of the precursor; at the same time, the aspect ratio of the surface whiskers of the manganese-rich precursor is 5-15, and the stacking degree is less than 80. Especially for manganese-rich materials with high specific surface area, the phenomenon of whisker shedding and whisker sticking during the sintering process is significantly suppressed, which is beneficial to maintaining the structural integrity of the positive electrode active material. Therefore, the manganese-rich precursor can be used to prepare a battery with high capacity, coulombic efficiency and excellent cycle performance.

[0050] The strength of the surface whiskers is also related to their curvature. Specifically, the smaller the curvature, the higher the strength of the surface whiskers, and the stronger and more stable the morphology of the surface whiskers. The curvature is determined by making tangents along both ends of the surface whiskers, and the angle between the two tangents extending in the same direction is the curvature. In some embodiments, the curvature of the surface whiskers of the positive electrode active material precursor is less than 15°, which is beneficial to further suppress the whisker shedding and whisker sticking phenomenon that occurs during the sintering process of the positive electrode active material precursor.

[0051] The spherical precursor is more stable than other precursors and has a shorter lithium ion insertion / extraction path, which is also beneficial to improving the tap density of the material. The positive electrode active material precursor of the present invention has a high sphericity, which makes the structure of the positive electrode active material precursor more stable, accelerates the lithium ion extraction speed, and improves the tap density of the material.

[0052] In some embodiments, the particle size of the cathode active material precursor of the present invention is 5-15 μm, and the upper limit of the particle size is relatively large, which is beneficial to improving the specific capacity, coulombic efficiency and cycle performance of the cathode active material.

[0053] When the length of the surface whiskers is 0.1-0.8 μm, the aspect ratio of the surface whiskers is 5-15, and the stacking degree is less than 80, it is beneficial to further improve the whisker shedding and whisker sticking phenomena during the sintering process of the positive electrode active material precursor.

[0054] In the field of view of a scanning electron microscope with a magnification of 1000, the proportion of fine powder in the positive electrode active material precursor is no more than 12%; wherein the fine powder is the part of the positive electrode active material precursor with a particle size lower than 1 / 2 of the positive electrode active material precursor D50. This indicates that there are fewer micropowders or small balls in the positive electrode active material precursor of the present invention, and the particle size distribution of the positive electrode active material precursor is narrow, which can effectively avoid uneven heating of large and small particles during the sintering process, avoid overburning of small particles, and is conducive to improving the specific capacity, coulombic efficiency and cycle performance of the positive electrode active material.

[0055] In some embodiments, Figure 3 As shown, the internal structure of the positive electrode active material precursor of the present invention is radially distributed in the radial direction from the inside to the outside, and the pores of the core layer, transition layer, intermediate layer and outer layer are all uniformly distributed, which means that the pores inside each layer are uniformly distributed. This structure is beneficial to increasing the deintercalation and extraction speed of lithium ions.

[0056] The positive electrode active material precursor includes a core layer, a transition layer, an intermediate layer and an outer layer in the radial direction from the inside to the outside. The widths of the core layer, transition layer, intermediate layer and outer layer are R1, R2, R3 and R4 respectively. The particle size of the positive electrode active material precursor is R, R1+R2+R3+R4=1 / 2*R, and R1=(6%-8%)*R, R2=(1%-2%)*R, R3=(24%-26%)*R, R4=(15%-16%)*R; wherein the average porosity of the core layer, transition layer, intermediate layer and outer layer decreases in sequence. The internal structure of the positive electrode active material precursor, which is dense on the outside and loose on the inside, is conducive to preventing the electrolyte from penetrating into the material, causing irreversible changes in the material structure, and thus reducing the cycle stability.

[0057] Furthermore, the average porosity of the core layer, transition layer, middle part and outer part are 25%-30%, 20%-25%, 15%-20% and 5%-10% respectively, which is beneficial to improving the structural stability and cycle stability of the material.

[0058] The abundant pores and thin and short whisker design greatly increase the specific surface area of ​​the precursor material, which is beneficial to provide more surface active sites for the insertion and extraction of lithium ions.

[0059] The second aspect of the present invention provides a method for preparing a positive electrode active material precursor according to the first aspect, the preparation method comprising a first stage, a second stage, a third stage and a fourth stage;

[0060] In the first stage, the rotation speed of the reaction system is 500-600 rpm, the pH is 10.5-11.0, the oxygen content is 0.70%-0.90%, the solid content is 0-100 g / L, the feed flow rate of the metal salt solution is 3-4 L / h, and the D50 of the first intermediate product satisfies: 12%*target particle size<D50 of the first intermediate product<16%*target particle size;

[0061] In the second stage, the speed of the reaction system is 400-500 rpm, the pH is 10.0-10.5, the oxygen content is 0.90%-1.1%, the solid content is 100-150 g / L, the feed flow rate of the metal salt solution is 4-5 L / h, and the D50 of the second intermediate product satisfies: 14%*target particle size<D50 of the second intermediate product<20%*target particle size;

[0062] In the third stage, the speed of the reaction system is 300-400 rpm, the pH is 9.8-10.2, the oxygen content is 1.2%-1.5%, the solid content is 150-250 g / L, the feed flow rate of the metal salt solution is 5-6 L / h, and the D50 of the third intermediate product satisfies: 62%*target particle size<D50 of the third intermediate product<72%*target particle size;

[0063] In the fourth stage, the rotation speed of the reaction system is 200-300rpm, the pH is 9.9-10.3, the oxygen content is 1.0%-1.3%, the solid content is greater than 250g / L, and the feed flow rate of the metal salt solution is 5-6L / h. When the D50 of the fourth intermediate product is the target particle size, the reaction system is aged, washed with water, and centrifuged to obtain the above-mentioned positive electrode active material precursor; wherein the reaction system includes a metal salt solution and a precipitant, the metal salt solution includes a mixed solution of nickel salt and manganese salt with a total molar concentration of 1.5-2.0mol / L, the molar ratio of nickel to manganese is x:y, 0<x<1, 0<y<1, and x+y=1.

[0064] The above-mentioned first stage is the nucleation stage, and the first intermediate product is the product of the first stage; the second stage, the third stage and the fourth stage are the main growth stages, and the second intermediate product, the third intermediate product and the fourth intermediate product are the products of the second stage, the third stage and the fourth stage respectively.

[0065] In the first stage, the rotation speed is relatively high, and the number of nuclei and the growth rate of nuclei are controlled by controlling the pH, oxygen content, solid content and feed flow rate of the metal salt solution. This saves raw materials while keeping the growth rate in this stage at a particle size increase of 0.1-0.3 μm every two hours for the precursor particles. The synergistic effect of the higher rotation speed and the slower growth rate is conducive to the generation of stable, highly crystalline, and highly spherical nuclei, laying a good foundation for the formation of surface whisker morphology with an aspect ratio of 5-15 and a stacking degree of less than 80.

[0066] When the D50 of the first intermediate product reaches 12%*target particle size to 16%*target particle size, it switches to the second stage. The second stage is a transition stage between nucleation and growth, and the overall reaction time is not long.

[0067] In the second stage, the growth rate is increased by reducing the rotation speed and pH and increasing the feed flow rate of the metal salt solution. At the same time, adjusting the oxygen content and the increase in the solid content in the reaction system helps to limit the growth rate and avoid excessive increase in the growth rate. The above factors interact with each other to keep the growth rate in the second stage at a particle size increase of 0.2-0.4μm every two hours. The growth rate is controlled while adjusting the growth of the particles to ensure a high sphericity. At the same time, a bridge is built between the core layer and the middle layer to avoid obvious stratification of the internal structure caused by sudden changes in the preparation parameters, improve the stability of the internal structure of the positive electrode active material precursor, and further lay a good foundation for the formation of a surface whisker morphology with an aspect ratio of 5-15 and a stacking degree of less than 80.

[0068] When the D50 of the second intermediate product reaches 14%*target particle size to 20%*target particle size, the process is switched to the third stage.

[0069] In the third stage, the particle size of the product is relatively large, and the higher rotation speed is not conducive to the deposition of the metal salt solution on the surface of the sphere with larger particle size, but is more inclined to form new nuclei, thus producing micropowder / small balls, that is, the fine powder with a particle size of <1 / 2*D50 of the positive electrode active material precursor in the aforementioned positive electrode active material precursor, and the above-mentioned small particles are prone to overburning during the sintering process; therefore, the rotation speed of the third stage continues to decrease on the basis of the second stage, and by increasing the feed flow rate of the metal salt solution, increasing the oxygen content, adjusting the pH and limiting the solid content, the time the metal salt solution stays on the surface of the sphere is extended, the probability of metal salt deposition on the surface of the sphere is increased, and the generation of micropowder / small balls is reduced; the growth rate of the third stage is still maintained at a particle size increase of 0.4-0.6μm every two hours of the precursor particles, and the growth of the particles is adjusted while controlling the growth rate, thereby ensuring a higher sphericity, improving the stability of the internal structure of the positive electrode active material precursor, and further laying a good foundation for the formation of a surface whisker morphology with an aspect ratio of 5-15 and a stacking degree of less than 80.

[0070] When the D50 of the third intermediate product reaches 62%*target particle size to 72%*target particle size, the process is switched to the fourth stage.

[0071] In the fourth stage, with the increase of products, the solid content of the reaction system increases significantly, which reduces the growth rate. In order to avoid too slow growth, the fourth stage continues to reduce the rotation speed and oxygen content on the basis of the third stage, and limits the pH and the feed flow rate of the metal salt solution. The growth rate in the fourth stage is maintained at a particle size increase of 0.1-0.3μm every two hours of the precursor particles, and at the same time, the growth of the particles is adjusted to form a strong and stable surface whisker morphology.

[0072] When the D50 of the fourth intermediate product is the target particle size, the reaction system is aged, washed with water, and centrifuged to obtain the positive electrode active material precursor of the present invention;

[0073] The aspect ratio of the surface whiskers of the positive electrode active material precursor is 5-15, and the stacking degree is less than 80.

[0074] The oxygen content in the above reaction system can be regulated by introducing an air / nitrogen mixed gas.

[0075] The rotation speed, pH, oxygen content, and feed flow rate of the metal salt solution in the above reaction system are closely related to the solid content and product particle size. The rotation speed, pH, oxygen content, and metal salt solution need to be adjusted in combination with the solid content and product particle size to control the growth rate and regulate the growth of the particles.

[0076] It is understandable that the metal salt solution can be prepared according to the chemical composition of the precursor. The metal salt solution used in the present invention includes a mixed solution of nickel salt and manganese salt with a total molar concentration of 1.5-2.0 mol / L, and the molar ratio of nickel to manganese is x:y, 0<x<1, 0<y<1, and x+y=1. The present invention does not specifically limit the types of the above-mentioned nickel salt, manganese salt and precipitant. The nickel salt is selected from at least one of nickel sulfate, nickel chloride and nickel nitrate, the manganese salt is selected from at least one of manganese sulfate, manganese chloride and manganese nitrate, and the precipitant is selected from at least one of sodium hydroxide, potassium hydroxide and sodium bicarbonate. The amount of the precipitant needs to be regulated in combination with the pH value of the reaction system. In addition, the present application does not specifically limit the reaction temperature. In some embodiments, the reaction temperature is 50°C, which is conducive to the rapid and smooth reaction.

[0077] The above preparation method adjusts the growth rate of the product particles by controlling the rotation speed, pH, oxygen content, feed rate of the metal salt solution, solid content and other factors of the reaction system in stages, adjusts the growth condition of the product particles, produces less micropowder / small balls, and the whisker shedding and whisker sticking phenomena of the obtained positive electrode active material precursor during the sintering process are significantly suppressed.

[0078] The above preparation process prepares the positive electrode active material precursor intermittently in stages and can be carried out in a single kettle, with low requirements on equipment and high applicability.

[0079] In some embodiments, after the fourth stage, the solid content of the reaction system in a single kettle is ≥300 g / L, which solves the problem of low production capacity of preparing large-particle positive electrode active material precursors by a single-pot intermittent method.

[0080] A complexing agent may also be used in the reaction system of the present invention to facilitate the coprecipitation process of the positive electrode active material precursor. The complexing agent is selected from at least one of ammonia water, sodium citrate and sodium oxalate.

[0081] The molar ratio of nickel to manganese is preferably x:y, 0<x<0.5, 0.5<y<1, and x+y=1. A manganese-rich precursor can be obtained by the above method. The aspect ratio of the surface whiskers of the manganese-rich precursor is 5-15, and the stacking degree is less than 80, which is beneficial to improving the capacity, coulombic efficiency and cycle performance of the battery.

[0082] Furthermore, the pH of the reaction system in the above-mentioned second stage and fourth stage is greater than the pH of the reaction system in the third stage. In this way, the pH of the first stage, the second stage and the third stage decreases successively. In the reaction system of the present invention, by controlling the pH of the first three stages to decrease successively, it is beneficial to control the growth direction of the unit cell, so that the whiskers extend in the radial direction from the inside to the outside, thereby forming a radial internal structure, which is beneficial to increase the deintercalation rate of lithium ions; in addition, since the fourth stage is the shaping stage of the surface whiskers, by controlling the pH of the fourth stage to be slightly increased on the basis of the pH of the third stage, combined with controlling the growth rate, it is beneficial to control the aspect ratio of the surface whiskers to be 5-15, and the stacking degree is less than 80, which is beneficial to suppress the whisker shedding and whisker sticking phenomenon that occurs in the sintering process of the positive electrode active material precursor.

[0083] Furthermore, the oxygen content of the reaction system in the second stage is higher than that in the first stage, and the oxygen content of the reaction system in the third stage is higher than that in the second and fourth stages.

[0084] The growth rates of the above four stages satisfy the following relationship: the first stage ≈ the second stage < the third stage > the fourth stage. On this basis, by adjusting the oxygen content of the reaction system in the above four stages, the degree of manganese oxidation is controlled, and then the interplanar spacing is controlled, which is conducive to forming a structure that is dense on the outside and loose on the inside, and avoiding excessive oxidation that may cause the surface whiskers to be too thin and the curvature to increase, laying a good foundation for the formation of surface whiskers with an aspect ratio of 5-15 and a stacking degree less than 80, which is conducive to further inhibiting the whisker shedding and whisker sticking phenomena that occur in the sintering process of the positive electrode active material precursor.

[0085] Based on the same inventive concept, the third aspect of the present invention provides a positive electrode active material, which is formed by the positive electrode active material precursor of the first aspect or the positive electrode active material precursor prepared by the preparation method of the second aspect. The positive electrode active material exhibits good processing performance in the process of preparing a positive electrode sheet, and the particle structure is stable and not easy to break, which is conducive to improving the coulombic efficiency and cycle performance.

[0086] In some embodiments, the positive electrode active material is obtained by mixing the positive electrode active material precursor and lithium salt described above and then sintering them.

[0087] Based on the same inventive concept, the fourth aspect of the present invention provides a positive electrode sheet, which includes the positive electrode active material. The positive electrode sheet of the present invention specifically includes a positive electrode current collector and a positive electrode active layer formed by the positive electrode active material and arranged on the surface of the positive electrode current collector.

[0088] When preparing the positive electrode sheet, for example, the positive electrode active material of the present invention, the conductive agent and the binder are dispersed in an appropriate amount of N-methylpyrrolidone (NMP) solvent, and the mixture is stirred and mixed to form a uniform positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector, and the positive electrode sheet is obtained after drying, rolling and cutting. For example, the positive electrode active layer includes 70-99wt% of the positive electrode active material, 0.5-15wt% of the conductive agent, and 0.5-15wt% of the binder according to the mass percentage, and further includes 80-98wt% of the positive electrode active material, 1-10wt% of the conductive agent, and 1-10wt% of the binder.

[0089] The material of the above-mentioned positive electrode current collector can be at least one of aluminum foil and nickel foil; the conductive agent can be selected from at least one of carbon black, acetylene black, graphene, Ketjen black, and carbon fiber; the binder can be selected from at least one of polytetrafluoroethylene, polyvinylidene fluoride, polyvinyl fluoride, polyethylene, polypropylene, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, and polyurethane.

[0090] The battery prepared using the positive electrode sheet has high coulombic efficiency and capacity and excellent cycle performance.

[0091] Based on the same inventive concept, the fifth aspect of the present invention provides a lithium ion battery, which includes the above-mentioned positive electrode sheet. It is conceivable that the lithium ion battery of the present invention includes a negative electrode sheet, an electrolyte and a separator in addition to the above-mentioned positive electrode sheet.

[0092] The present invention does not strictly limit the negative electrode active material in the negative electrode sheet, and can be at least one of the negative electrode active materials commonly used in lithium-ion batteries, such as graphite, hard carbon, soft carbon, mesophase carbon microbeads, silicon-based negative electrode materials (mainly including silicon oxide, silicon-carbon negative electrode), tin-based negative electrode materials (mainly including tin, tin alloy), etc.

[0093] The present invention does not strictly limit the selection of the electrolyte, and may include one or more of the solvents commonly used in lithium-ion battery electrolytes, and electrolyte lithium salts commonly used in lithium-ion electrolytes, for example: the solvent may be ethylene carbonate, propylene carbonate, butylene carbonate, fluoroethylene carbonate (FEC), dimethyl carbonate (DMC), diethyl carbonate (DEC), difluoroethylene carbonate (DFEC), dipropyl carbonate, ethyl methyl carbonate (EMC), ethyl acetate, ethyl propionate, propyl acetate, propyl propionate, sulfolane, γ-butyrolactone, etc.; the lithium salt may be, for example, one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), and lithium bis(trifluoromethylsulfonyl)imide (LiTFSI).

[0094] The present invention does not strictly limit the material selection of the diaphragm, which can be a diaphragm material commonly used in lithium-ion batteries, such as a polypropylene diaphragm (PP), a polyethylene diaphragm (PE), a polypropylene / polyethylene double-layer composite film (PP / PE), a polyimide electrospinning diaphragm (PI), a polypropylene / polyethylene / polypropylene three-layer composite film (PP / PE / PP), a cellulose non-woven fabric diaphragm, or a diaphragm with a ceramic coating.

[0095] When preparing lithium-ion batteries, the positive electrode sheet, the separator and the negative electrode sheet are wound or stacked to obtain a bare cell, and the bare cell is packaged in a pre-stamped aluminum-plastic film bag. After the packaged battery is dried at 85°C, the electrolyte is injected into the dry battery, and the battery is placed, formed and sealed for the second time to complete the preparation of the lithium-ion battery. The lithium-ion battery has high coulomb efficiency and discharge capacity, and excellent cycle performance.

[0096] Hereinafter, the positive electrode active material precursor and the preparation method thereof of the present invention will be described in more detail through specific examples.

[0097] Example 1

[0098] This embodiment provides a method for preparing a positive electrode active material precursor, comprising a first stage, a second stage, a third stage and a fourth stage;

[0099] In the first stage, the speed of the reaction system is 550 rpm, the pH is 10.8-11.0, the oxygen content is 0.80%±0.05%, the solid content is 0-80 g / L, the feed flow rate of the metal salt solution is 3 L / h, and the D50 of the first intermediate product is 1.2 μm;

[0100] In the second stage, the speed of the reaction system is 450 rpm, the pH is 10.0-10.5, the oxygen content is 1.00%±0.05%, the thickener is turned on to perform a thickening operation to make the solid content 80-140 g / L, the feed flow rate of the metal salt solution is 4 L / h, and the D50 of the second intermediate product is 1.4 μm;

[0101] In the third stage, the rotation speed of the reaction system is 350 rpm, the pH is 9.8-10.0, the oxygen content is 1.40%±0.05%, the solid content is 140-250 g / L, the feed flow rate of the metal salt solution is 5 L / h, and the D50 of the third intermediate product is 6.2 μm;

[0102] In the fourth stage, the rotation speed of the reaction system is 200 rpm, the pH is 9.9-10.1, the oxygen content is 1.10%±0.05%, the solid content is 250-330 g / L, and the feed flow rate of the metal salt solution is 5 L / h. When the D50 of the fourth intermediate product is 10 μm, the reaction system is aged, washed with water, and centrifuged to obtain a positive electrode active material precursor;

[0103] The reaction system includes a metal salt solution and a precipitant, wherein the metal salt solution includes a mixed solution of nickel sulfate and manganese sulfate with a total molar concentration of 1.8 mol / L, and a molar ratio of nickel to manganese of 0.35:0.65; the precipitant is sodium hydroxide with a concentration of 11.00 mol / L; the temperature of the reaction system is 50°C, and an air / nitrogen mixed gas is introduced to adjust the oxygen content.

[0104] Example 2

[0105] This embodiment provides a method for preparing a positive electrode active material precursor, comprising a first stage, a second stage, a third stage and a fourth stage;

[0106] In the first stage, the speed of the reaction system is 500 rpm, the pH is 10.7-10.9, the oxygen content is 0.85%±0.05%, the solid content is 0-100 g / L, the feed flow rate of the metal salt solution is 3 L / h, and the D50 of the first intermediate product is 1.6 μm;

[0107] In the second stage, the speed of the reaction system is 400 rpm, the pH is 10.1-10.5, the oxygen content is 1.00%±0.05%, the thickener is turned on to perform a thickening operation to make the solid content 100-150 g / L, the feed flow rate of the metal salt solution is 4 L / h, and the D50 of the second intermediate product is 2.0 μm;

[0108] In the third stage, the rotation speed of the reaction system is 300 rpm, the pH is 9.8-9.9, the oxygen content is 1.45%±0.05%, the solid content is 150-250 g / L, the feed flow rate of the metal salt solution is 5 L / h, and the D50 of the third intermediate product is 7.2 μm;

[0109] In the fourth stage, the rotation speed of the reaction system is 200 rpm, the pH is 9.9-10.1, the oxygen content is 1.20%±0.05%, the solid content is 250-330 g / L, and the feed flow rate of the metal salt solution is 5 L / h. When the D50 of the fourth intermediate product is 10 μm, the reaction system is aged, washed with water, and centrifuged to obtain a positive electrode active material precursor;

[0110] The reaction system includes a metal salt solution, a precipitant and an ammonia complexing agent, wherein the metal salt solution includes a mixed solution of nickel sulfate and manganese sulfate with a total molar concentration of 1.8 mol / L, and a molar ratio of nickel to manganese of 0.30:0.70; the precipitant is sodium hydroxide with a concentration of 11.00 mol / L; the amount of the ammonia complexing agent in the system is maintained at 0.5 g / L; the temperature of the reaction system is 50°C, and an air / nitrogen mixed gas is introduced to adjust the oxygen content.

[0111] Example 3

[0112] This embodiment is basically the same as Embodiment 1, except that:

[0113] The D50 of the first intermediate product is 0.9 μm, the D50 of the second intermediate product is 1.5 μm, the D50 of the third intermediate product is 4.6 μm, and the target particle size of the product, i.e., the D50 of the fourth intermediate product, is 6 μm; other conditions remain unchanged.

[0114] Example 4

[0115] This embodiment is basically the same as Embodiment 1, except that:

[0116] The D50 of the first intermediate product is 0.6 μm, the D50 of the second intermediate product is 0.9 μm, the D50 of the third intermediate product is 5 μm, and the target particle size of the product, i.e., the D50 of the fourth intermediate product, is 7 μm; other conditions remain unchanged.

[0117] Example 5

[0118] This embodiment is basically the same as Embodiment 1, except that:

[0119] In the fourth stage, the oxygen content is controlled at 1.1%-1.4%; other conditions remain unchanged.

[0120] Example 6

[0121] This embodiment is basically the same as Embodiment 1, except that:

[0122] The D50 of the first intermediate product is 2.2 μm, the D50 of the second intermediate product is 2.7 μm, the D50 of the third intermediate product is 11 μm, and the target particle size of the product, i.e., the D50 of the fourth intermediate product, is 16 μm; other conditions remain unchanged.

[0123] Example 7

[0124] This embodiment is basically the same as Embodiment 1, except that:

[0125] The D50 of the first intermediate product is 0.45 μm, the D50 of the second intermediate product is 0.55 μm, the D50 of the third intermediate product is 2.3 μm, and the target particle size of the product, i.e., the D50 of the fourth intermediate product, is 3.5 μm; other conditions remain unchanged.

[0126] Example 8

[0127] This embodiment is basically the same as Embodiment 1, except that:

[0128] The speed of the first stage is 600rpm, the speed of the second stage is 550rpm, the speed of the third stage is 550rpm, the speed of the fourth stage is 550rpm, and other conditions remain unchanged.

[0129] Example 9

[0130] This embodiment is basically the same as Embodiment 1, except that:

[0131] The oxygen content in the first stage is controlled at 0.5%-0.6%, in the second stage at 0.6%-0.8%, in the third stage at 0.8%-1.3%, and in the third stage at 1.1%-1.4%; other conditions remain unchanged.

[0132] Comparative Example 1

[0133] This comparative example provides a method for preparing a positive electrode active material precursor, comprising a first stage and a second stage;

[0134] In the first stage, the rotation speed of the reaction system is 550 rpm, the pH is 10.7-10.9, the oxygen content is 0.70%±0.05%, the solid content is 0-100 g / L, the feed flow rate of the metal salt solution is 3 L / h, and the D50 of the first intermediate product is 1.2 μm;

[0135] In the second stage, the speed of the reaction system is 450 rpm, the pH is 9.8-10.6, the oxygen content is 1.60%±0.05%, the thickener is turned on to perform a concentration operation to make the solid content 100-300 g / L, the feed flow rate of the metal salt solution is 4-5 L / h, and when the D50 of the second intermediate product is 10 μm, the reaction system is aged, washed with water, and centrifuged to obtain a positive electrode active material precursor;

[0136] The reaction system includes a metal salt solution and a precipitant, wherein the metal salt solution includes a mixed solution of nickel sulfate and manganese sulfate with a total molar concentration of 1.8 mol / L, and a molar ratio of nickel to manganese of 0.35:0.65; the precipitant is sodium hydroxide with a concentration of 11.00 mol / L; the temperature of the reaction system is 50°C, and an air / nitrogen mixed gas is introduced to adjust the oxygen content.

[0137] Comparative Example 2

[0138] This comparative example provides a method for preparing a positive electrode active material precursor, comprising a first stage and a second stage;

[0139] In the first stage, the rotation speed of the reaction system is 550 rpm, the pH is 10.7-11.0, the oxygen content is 0.80%±0.05%, the solid content is 0-100 g / L, the feed flow rate of the metal salt solution is 3 L / h, and the D50 of the first intermediate product is 1.6 μm;

[0140] In the second stage, the speed of the reaction system is 550 rpm, the pH is 9.8-10.5, the oxygen content is 1.40% ± 0.05%, the thickener is turned on to perform a concentration operation to make the solid content 100-300 g / L, the feed flow rate of the metal salt solution is 4-5 L / h, and when the D50 of the second intermediate product is 10 μm, the reaction system is aged, washed with water, and centrifuged to obtain a positive electrode active material precursor;

[0141] The reaction system includes a metal salt solution and a precipitant, wherein the metal salt solution includes a mixed solution of nickel sulfate and manganese sulfate with a total molar concentration of 1.8 mol / L, and a molar ratio of nickel to manganese of 0.30:0.70; the precipitant is sodium hydroxide with a concentration of 11.00 mol / L; the amount of ammonia complexing agent in the system is maintained at 0.5 g / L; the temperature of the reaction system is 50°C, and an air / nitrogen mixed gas is introduced to adjust the oxygen content.

[0142] Test Example 1

[0143] The following parameters of the positive electrode active material precursors of the above embodiments and comparative examples were tested:

[0144] 1) Length and aspect ratio of surface whiskers: The length and thickness of the whiskers were obtained by scanning electron microscope measurement program, and the aspect ratio was obtained by dividing the length by the thickness. The results are shown in Table 1.

[0145] 2) Stacking degree of surface whiskers: A scanning electron microscope image of a single complete positive electrode active material precursor particle was taken at a magnification of 10,000, such as Figure 1 As shown, a circle with a diameter of r is drawn with the center of the positive electrode active material precursor particle as the center, wherein r is 1 / 10 of the particle size of the positive electrode active material precursor particle, and the number of surface whiskers in the circle is counted, that is, the stacking degree of the surface whiskers. The results are shown in Table 1;

[0146] 3) Curvature of surface whiskers: Tangent lines are drawn along the two ends of the surface whiskers. The angle between the tangent lines and the same direction is the curvature. The results are shown in Table 1.

[0147] 4) D50 of the positive electrode active material precursor particles: measured using a particle size tester, the results are shown in Table 2;

[0148] 5) Content of fine powder in positive electrode active material precursor: In the field of view of a scanning electron microscope with a magnification of 1000, the number of fine powder in the positive electrode active material precursor and the total number of positive electrode active material precursor particles were counted. The ratio of the two was the proportion of fine powder in the positive electrode active material precursor, wherein the fine powder was the part of the positive electrode active material precursor with a particle size lower than 1 / 2 of the D50 of the positive electrode active material precursor. The specific results are shown in Table 2;

[0149] 6) Average porosity of the core, middle and outer parts of the positive electrode active material precursor particles: profile test analysis, the results are shown in Table 2;

[0150] 7) Widths R1, R2, R3, R4 of the core, middle, and outer parts of the positive electrode active material precursor particles: profile test analysis, and calculate the ratio of R1, R2, R3, R4 to R with D50 as R. The results are shown in Table 2;

[0151] 8) SEM scanning images of the positive electrode active material precursor particles of Example 1 and Comparative Example 1 and Comparative Example 2 are shown in Figure 1 , Figure 2 , Figure 3 , Figure 6 , Figure 7 , Figure 8 , Fig.10 , Fig.11 .

[0152] Table 1 Detection results of whiskers on the surface of positive electrode active material precursors

[0153] Length Aspect Ratio Stacking degree Curvature° Example 1 0.3-0.5 11-15 44 4 Example 2 0.3-0.5 9-15 51 8 Example 3 0.3-0.5 8-12 62 6 Example 4 0.3-0.5 10-14 58 9 Example 5 0.3-0.5 11-15 76 20 Example 6 0.1-0.4 5-8 80 13 Example 7 0.1-0.3 11-15 48 8 Example 8 0.3-0.5 6-12 80 4 Example 9 0.3-0.5 5-10 65 5 Comparative Example 1 0.2-0.4 20-25 87 76 Comparative Example 2 0.5-1.0 22-28 106 17

[0154] Data analysis of Table 1: The surface whiskers of the positive electrode active material precursor of each embodiment meet the aspect ratio of 5-15 and the stacking degree less than 80; further, the length of the surface whiskers is 0.1-0.5μm, and the curvature is less than 20°; while the aspect ratio, stacking degree and curvature of the surface whiskers of the positive electrode active material precursor of the comparative example are larger.

[0155] Table 2 Detection results of positive electrode active material precursor particles

[0156]

[0157]

[0158] Data analysis of Table 2: The proportion of fine powder in the positive electrode active material precursor of each embodiment is small, and the average porosity of the core layer, transition layer, middle layer and outer layer gradually decreases.

[0159] Test Example 2

[0160] The positive electrode active material is prepared by using the positive electrode active material precursors of the above-mentioned embodiments and comparative examples, which specifically includes the following steps:

[0161] The positive electrode active material precursor and lithium sulfate are mixed in a certain proportion and then sintered once to obtain the positive electrode active material.

[0162] The following parameters of the positive electrode active material are tested:

[0163] 1) Tap density of positive electrode active material: The tap density was measured according to the national material standard GB / T 5162-2006. The results are shown in Table 3.

[0164] 2) SEM scanning images of the positive electrode active materials of Example 1 and Comparative Example 1, see Figure 4 , Figure 5 and Fig. 9 .

[0165] Table 3 Detection results of whiskers on the surface of positive electrode active material precursors

[0166] <![CDATA[Tap density / g / cm 3 > Example 1 2.88 Example 2 2.93 Example 3 2.87 Example 4 2.88 Example 5 2.82 Example 6 2.79 Example 7 2.92 Example 8 2.90 Example 9 2.95 Comparative Example 1 2.78 Comparative Example 2 2.80

[0167] Data analysis of Table 3: The positive electrode active material of this embodiment has a good tap density.

[0168] Test Example 3

[0169] The positive electrode active materials corresponding to the examples and comparative examples are prepared into positive and negative electrode sheets, electrolytes and separators, and assembled into button batteries according to the following method. The method includes:

[0170] Each positive electrode active material is mixed with conductive carbon black (SP) and PVDF in a weight ratio of 80%:10%:10% to obtain a positive electrode slurry by dispersion. The slurry is coated on an aluminum foil current collector and rolled to prepare a positive electrode sheet. The positive electrode sheet is then punched into a small disc with a diameter of 12 mm using a film mold. After drying and weighing, a button battery is assembled in a glove box under an Ar protective atmosphere using a 2025 button battery shell, a Li metal disc as the negative electrode, and a conventional high-voltage lithium cobalt oxide electrolyte.

[0171] After each button cell was left to stand for 4 hours under normal conditions, the coulombic efficiency and charge / discharge capacity of the cell were tested according to the following steps:

[0172] Charge at 0.2C to 4.55V, charge at constant voltage to 0.025C and then let stand for 3 minutes, then discharge at 0.2C to 3.0V, obtain the charge and discharge curve, and record the first charge gram capacity C0 and the first discharge gram capacity D0, and calculate the first coulombic efficiency according to D0 / C0.

[0173] Follow the steps below to test the battery's cycling performance:

[0174] At 25°C, charge to 4.50V at a constant current of 1C, charge to 4.50V at a constant voltage of 0.05C, and then discharge to 3.0V at a discharge rate of 1C. Repeat this charge and discharge cycle 200 times, and measure the discharge capacity Q1 at the first cycle and the discharge capacity Q at the 200th cycle. 200 .

[0175] The capacity retention rate Q and thickness change rate after 500 cycles were calculated according to the following formula.

[0176] Capacity retention rate Q = Q 200 / Q1*100%

[0177] See Table 4 for relevant data.

[0178] Table 4 Test results of button batteries

[0179] C0 / mAh / g D0 / mAh / g D0 / C0 Capacity retention rate after 200 cycles Example 1 259.2 210.1 81.06% 96% Example 2 260.8 208.9 80.10% <![CDATA[ 97% ]]> Example 3 259.0 209.6 80.93% <![CDATA[ 97% <!-- 14 -->]]> Example 4 259.9 209.7 80.68% <![CDATA[ 96% ]]> Example 5 258.3 208.5 80.72% <![CDATA[ 92% ]]> Example 6 251.9 201.8 80.11% <![CDATA[ 90% ]]> Example 7 260.1 209.4 80.34% <![CDATA[ 94% ]]> Example 8 253.1 202.6 80.04% <![CDATA[ 90% ]]> Example 9 256.7 204.2 79.54% <![CDATA[ 89% ]]> Comparative Example 1 250.7 200.2 79.86% <![CDATA[ 78% ]]> Comparative Example 2 249.8 199.7 79.94% <![CDATA[ 84% ]]>

[0180] Data analysis of Table 4: The button cell of this embodiment has a high initial coulombic efficiency, a high capacity retention rate after 200 cycles, and good cycle performance.

[0181] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A positive electrode active material precursor, It is characterized in that The chemical formula of the positive electrode active material precursor is: Ni x Mn y (OH) 2 , where 0<x<1, 0<y<1, x+y=1; The aspect ratio of the whiskers on the surface of the positive electrode active material precursor is 5-15, and the stacking degree is less than 80.

2. The positive electrode active material precursor according to claim 1, It is characterized in that The curvature of the surface whiskers is less than 15°; and / or the particle size of the positive electrode active material precursor is 5-15 μm; and / or the length of the surface whiskers is 0.1-0.8 μm.

3. The positive electrode active material precursor according to claim 1 or 2, It is characterized in that In the field of view of a scanning electron microscope with a magnification of 1000, the proportion of fine powder in the positive electrode active material precursor is no more than 12%; wherein the fine powder is the part of the positive electrode active material precursor with a particle size lower than 1 / 2 of the positive electrode active material precursor D50.

4. The positive electrode active material precursor according to any one of claims 1 to 3, It is characterized in that The positive electrode active material precursor includes a core layer, a transition layer, an intermediate layer and an outer layer in the radial direction from the inside to the outside, and the widths of the core layer, the transition layer, the intermediate layer and the outer layer are R1, R2, R3 and R4 respectively. The particle size of the positive electrode active material precursor is R, R1+R2+R3+R4=1 / 2*R, and R1=(6%-8%)*R, R2=(1%-2%)*R, R3=(24%-26%)*R, and R4=(15%-16%)*R; The average porosity of the core layer, transition layer, middle layer and outer layer decreases in sequence.

5. The positive electrode active material precursor according to claim 4, It is characterized in that The average porosity of the core layer, transition layer, middle layer and outer layer are 25%-30%, 20%-25%, 15%-20% and 5%-10% respectively.

6. A method for preparing a positive electrode active material precursor according to any one of claims 1 to 5, It is characterized in that The preparation method comprises a first stage, a second stage, a third stage and a fourth stage; In the first stage, the rotation speed of the reaction system is 500-600 rpm, the pH is 10.5-11.0, the oxygen content is 0.70%-0.90%, the solid content is 0-100 g / L, the feed flow rate of the metal salt solution is 3-4 L / h, and the D50 of the first intermediate product satisfies: 12%*target particle size<D50 of the first intermediate product<16%*target particle size; In the second stage, the speed of the reaction system is 400-500 rpm, the pH is 10.0-10.5, the oxygen content is 0.90%-1.1%, the solid content is 100-150 g / L, the feed flow rate of the metal salt solution is 4-5 L / h, and the D50 of the second intermediate product satisfies: 14%*target particle size<D50 of the second intermediate product<20%*target particle size; In the third stage, the rotation speed of the reaction system is 300-400 rpm, the pH is 9.8-10.2, the oxygen content is 1.2%-1.5%, the solid content is 150-250 g / L, the feed flow rate of the metal salt solution is 5-6 L / h, and the D50 of the third intermediate product satisfies: 62%*target particle size<D50 of the third intermediate product<72%*target particle size; In the fourth stage, the rotation speed of the reaction system is 200-300 rpm, the pH is 9.9-10.3, the oxygen content is 1.0%-1.3%, the solid content is greater than 250 g / L, and the feed flow rate of the metal salt solution is 5-6 L / h. When the D50 of the fourth intermediate product is the target particle size, the reaction system is aged, washed with water, and centrifuged to obtain the positive electrode active material precursor; The reaction system includes the metal salt solution and a precipitant, the metal salt solution includes a mixed solution of nickel salt and manganese salt with a total molar concentration of 1.5-2.0 mol / L, the molar ratio of nickel to manganese is x:y, 0<x<1, 0<y<1, and x+y=1.

7. The preparation method according to claim 6, It is characterized in that The pH of the reaction system in the second stage and the fourth stage is greater than the pH of the reaction system in the third stage; And / or, the oxygen content of the reaction system in the second stage is higher than that in the first stage, and the oxygen content of the reaction system in the third stage is higher than that in the second and fourth stages.

8. A positive electrode active material, It is characterized in that The positive electrode active material is formed by the positive electrode active material precursor according to any one of claims 1 to 4 or the positive electrode active material precursor prepared by the preparation method according to any one of claims 5 to 7.

9. A positive electrode sheet, It is characterized in that The positive electrode sheet comprises the positive electrode active material according to claim 8.

10. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the positive electrode sheet according to claim 9.

Citation Information

Cited By

  • High BET lithium-rich manganese-based binary precursor and preparation method and application thereof

    CN119612618A