Flocculating agent for industrial wastewater treatment and preparation method thereof
By combining modified silica with polyethylene polymer and introducing thioglycolic acid functional groups, a highly efficient flocculant is prepared, which solves the problems of poor heavy metal removal effect and limited application range of existing flocculants, and achieves It effectively removes heavy metals and impurities from industrial wastewater, significantly better than commercially available products.
Patent Information
- Application Number
- CN202411004210.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-25
AI Technical Summary
Existing silica and polyethylene flocculants are not effective in removing heavy metals, have limited scope of application, and are sensitive to water quality factors, resulting in waste of resources and low removal efficiency.
The urethane-based silane-modified silica is combined with polyethylene polymer, and a flocculant with modified functions is prepared through ultrasonic treatment and melt extrusion to enhance its adsorption capacity for heavy metal ions, and through thioglycolic acid Modification improves flocculation performance.
It significantly improves the removal rate of Cu2+, Pb2+, Cr3+, Zn2+, Cd2+, and COD, reaching more than 97%, which is better than commercially available flocculants. It is suitable for various water quality conditions and extends the service life of the flocculant.
Smart Images

Figure CN118754277A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical industry, and particularly relates to a flocculant for industrial wastewater treatment and a preparation method thereof. Background Art
[0002] Flocculants are water treatment agents that can cause suspended particles in water to aggregate into flocs and accelerate sedimentation. In the field of water treatment, flocculants play a vital role, especially in removing suspended matter in water, regulating water quality, and promoting solid-liquid separation. With the acceleration of industrialization and urbanization, water pollution problems are becoming increasingly serious, and the demand for flocculants is also increasing.
[0003] Silica flocculants are an inorganic polymer flocculant composed of silica and other oxides. They are mainly used to remove pollutants such as suspended matter, colloids and organic matter in water. However, it is necessary to pay attention to its limitations during use. This flocculant has a limited scope of application and is not effective in removing heavy metals. A larger amount of it can achieve a better flocculation effect, or it needs to be combined with other treatment methods to improve the treatment effect. At the same time, factors such as suspended matter, hardness, and alkalinity in the water will also affect the flocculation effect of silica flocculants, and it is difficult to recover from the water after use, which will cause a certain waste of resources.
[0004] Polyethylene flocculant is an organic polymer flocculant, and its performance will be affected by the environment. At higher temperatures, the activity of flocculant molecules decreases, reducing its flocculation effect. In a high-salinity environment, the effect of polyethylene flocculants will be inhibited to a certain extent. This is because salinity affects the interaction between flocculants and pollutants. The adsorption capacity of polyethylene flocculants is affected by the type and chemical properties of heavy metal ions. Different heavy metal ions have different charges, radii and chemical properties, resulting in differences in their binding ability and selectivity with flocculants, making the adsorption capacity of polyethylene flocculants for heavy metal ions relatively low. When treating high-concentration heavy metal wastewater, a large amount of flocculants or multiple adsorption treatments are required to achieve sufficient removal effect.
[0005] The present invention aims to provide a silicon dioxide composite polyethylene flocculant for heavy metal treatment of industrial wastewater. Summary of the invention
[0006] The first object of the present invention is to provide a flocculant for industrial wastewater treatment, and the second object of the present invention is to provide a method for preparing the flocculant.
[0007] The first object of the present invention is achieved by providing a flocculant for industrial wastewater treatment, which is composed of urethane silane, silicon dioxide and polyethylene polymer in a mass ratio of 2-3:1-2:10.
[0008] The second object of the present invention is achieved by the method for preparing the flocculant, which is specifically achieved by the following steps: 1) Urethane silane modified silica: Add silica powder to a wax-water mixture at 60-70°C and ultrasonically treat at a power of 50000-60000 Hz for 1-2 h, then cool to room temperature, add urethane silane, and continue stirring for 3-4 h; then, centrifuge, wash with deionized water, and dry to obtain modified silica; 2) The modified silica and polyethylene polymer are mixed in a ratio of 2-3:10, reacted at 200-220°C for 2-3 h to obtain polyethylene containing modified silica, and then the polyethylene containing modified silica is processed by a melt extrusion method to obtain a target flocculant; during the melt extrusion process, the temperature is controlled at 210-230°C, the extruder speed is 300-500rpm, and the processing pressure is 0.5-1.5 MPa.
[0009] In step 2), the preparation method of the polyethylene polymer is to mix low-density polyethylene and an initiator in a ratio of 100:0.1-1, stir at a speed of 200-300 rpm for 10-20 minutes, and then polymerize at 80-90°C for 8-10 hours. The obtained precipitate is filtered, washed, dried and crushed to obtain a polyethylene polymer.
[0010] Silicon dioxide is one of the most abundant resources on earth, easy to obtain, low cost, and has good thermal stability and chemical stability, is not easy to be hydrolyzed, and is suitable for long-term use. Silica particles have a large specific surface area and good mechanical strength, and can maintain a stable flocculation effect even under strong stirring. The silicon dioxide flocculant has good dispersibility in water and can effectively capture suspended matter after forming flocs. The present invention introduces various functional groups such as hydroxyl, thiol, etc. into silicon dioxide through chemical modification, which can enhance its flocculation performance, effectively adsorb heavy metal ions, and is beneficial to the removal of heavy metal ions in water treatment. The present invention uses a wax-modified silicon dioxide shell to coat a polyethylene polymer matrix to obtain a flocculant with excellent heavy metal ion removal performance. The silicon dioxide shell has good acid and alkali resistance, can provide additional protection and stability, reduce the degradation or inactivation of polyethylene polymers in the solution, can remain stable in a wide pH range, and is suitable for various water quality conditions, thereby improving the service life and effect of the flocculant and broadening the application range of the flocculant. The silica shell modified with thioglycolic acid can improve the flocculation performance of the flocculant, making it more effective in removing impurities such as suspended solids, colloids and organic matter.
[0011] The flocculant provided by the present invention has an effect on the treatment of Cu in industrial wastewater. 2+ , Pb 2+ Cr3+ 、Zn 2+ 、Cd 2+ The COD removal rates are both over 97%, which are significantly better than the commercially available polyvinyl amide flocculants and are suitable for promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is a microscopic picture of the flocculant prepared in Example 1. DETAILED DESCRIPTION
[0013] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments, but the present invention is not limited in any way. Any changes or improvements made based on the teachings of the present invention fall within the protection scope of the present invention.
[0014] The invention discloses a flocculant for industrial wastewater treatment, which is composed of urethane silane, silicon dioxide and polyethylene polymer in a mass ratio of 2-3:1-2:10.
[0015] The flocculant also includes thioglycolic acid.
[0016] The present invention also provides a method for preparing the flocculant, which is specifically achieved by the following steps: 1) Urethane silane modified silica: Add silica powder to a wax-water mixture at 60-70°C and ultrasonically treat at a power of 50000-60000 Hz for 1-2 h, then cool to room temperature, add urethane silane, and continue stirring for 3-4 h; then, centrifuge, wash with deionized water, and dry to obtain modified silica; 2) The modified silica and polyethylene polymer are mixed in a ratio of 2-3:10, reacted at 200-220°C for 2-3 h to obtain polyethylene containing modified silica, and then the polyethylene containing modified silica is processed by a melt extrusion method to obtain a target flocculant; during the melt extrusion process, the temperature is controlled at 210-230°C, the extruder speed is 300-500rpm, and the processing pressure is 0.5-1.5 MPa.
[0017] In step 2), the preparation method of the polyethylene polymer is to mix low-density polyethylene and an initiator in a ratio of 100:0.1-1, stir at a speed of 200-300 rpm for 10-20 minutes, and then polymerize at 80-90°C for 8-10 hours. The obtained precipitate is filtered, washed, dried and crushed to obtain a polyethylene polymer.
[0018] In step 2), the initiator is hydrogen peroxide.
[0019] In step 1), the wax-water mixture is prepared by melting paraffin wax and adding it into water at 60-70° C., stirring evenly to obtain the wax-water mixture, wherein the mass ratio of paraffin wax to water is 1:3.
[0020] Add 20-30 g / L thioglycolic acid to the flocculant obtained in step 2), mix well, react at room temperature for 2-3 h, and stir at a stirring speed of 200-220 rpm to obtain a thioglycolic acid modified flocculant; The mass volume ratio of the flocculant to the thioglycolic acid is 1:22-24 g / ml.
[0021] Example 1 100 g of paraffin was melted in a 60°C water bath at a stirring speed of 400 rpm, and then added to 300 g of water at 60°C and stirred at a speed of 50 rpm for 30 min to obtain a wax-water mixture.
[0022] 10 g of silica powder with a particle size of 20 nm was slowly added to the wax-water mixture and ultrasonicated at a power of 50,000 Hz for 1 h to ensure the homogeneity of the system. Silica particles with a surface energy between the two liquids will be adsorbed to the liquid-liquid interface. It was then cooled to 25 °C to solidify the wax phase and lock the particles in place. Subsequently, 20 g of urethane silane (AMCS) was added to modify the surface of silica in the wax-water system for 3 h. After the modification was completed, urethane silane-modified silica was obtained by centrifugation, deionized water washing, and drying.
[0023] 100 g of low-density polyethylene and 0.1 g of initiator, hydrogen peroxide (H 2 O 2 ) and stirred at 200 rpm for 10 min to ensure that the initiator is evenly distributed in the monomer. After uniform mixing, the polymerization reaction was carried out at 80 °C for 8 h. After the reaction was completed, the product was taken out from the reactor, filtered, washed, dried and crushed after precipitation to obtain polyethylene polymer.
[0024] 20 g of urethane silane-modified silica was mixed with 100 g of polyethylene matrix and reacted at 200 °C for 2 h to obtain polyethylene containing modified silica, which was then processed into a flocculant ( Figure 1 ).from Figure 1It can be seen that the modified silica is attached to the surface of the polyethylene polymer. During the melt extrusion process, the temperature was controlled at 220 °C to fully mix the modified silica with the polyethylene. At the same time, the speed of the extruder was adjusted to 400 rpm and the processing pressure was controlled to 1 MPa to ensure the structural stability and performance reliability of the flocculant.
[0025] In order to further improve the removal efficiency of heavy metal ions, 200 ml of 20 g / L thioglycolic acid (MEA) was mixed with 10 g of the obtained flocculant. The unmodified surface of silica was fully contacted with MEA to introduce thiol functional groups. The mixture was reacted at 25 °C for 2 h and stirred at a stirring speed of 200 rpm to obtain a thioglycolic acid modified flocculant.
[0026] Example 2 100 g of paraffin wax was melted in a 65° C. water bath at a stirring speed of 400 rpm, and then added to 300 g of water at 60° C. and stirred at a speed of 50 rpm for 30 min to obtain a wax-water mixture.
[0027] 15 g of silica powder with a particle size of 30 nm was slowly added to the wax-water mixture and ultrasonicated at a power of 55,000 Hz for 1.5 h to ensure the homogeneity of the system. Silica particles with a surface energy between the two liquids will be adsorbed to the liquid-liquid interface. Then it was cooled to 25 °C to solidify the wax phase and lock the particles in place. Subsequently, 25 g of urethane silane (AMCS) was added to modify the surface of silica in the wax-water system for 3.5 h. After the modification was completed, urethane silane-modified silica was obtained by centrifugation, deionized water washing, and drying.
[0028] 100 g of low-density polyethylene and 0.5 g of initiator, hydrogen peroxide (H 2 O 2 ) and stirred at 250 rpm for 15 minutes to ensure that the initiator is evenly distributed in the monomer. After uniform mixing, the polymerization reaction was carried out at 85 °C for 9 hours. After the reaction was completed, the product was taken out from the reactor, filtered, washed, dried and crushed after precipitation to obtain polyethylene polymer.
[0029] 25 g of urethane silane-modified silica was mixed with 100 g of polyethylene matrix and reacted at 210 °C for 2.5 h to obtain polyethylene containing modified silica, which was then processed into a flocculant by melt extrusion. During the melt extrusion process, the temperature was controlled at 210 °C to fully mix the modified silica and polyethylene. At the same time, the speed of the extruder was adjusted to 300 rpm and the processing pressure was controlled to 0.5 MPa to ensure the structural stability and performance reliability of the flocculant.
[0030] In order to further improve the removal efficiency of heavy metal ions, 220 ml of 25 g / L thioglycolic acid (MEA) was mixed with 10 g of the obtained flocculant. The unmodified surface of silica was fully contacted with MEA to introduce thiol functional groups. The mixture was reacted at 30 °C for 2.5 h and stirred at a stirring speed of 210 rpm to obtain a thioglycolic acid modified flocculant.
[0031] Example 3 100 g of paraffin was melted in a 70°C water bath at a stirring speed of 600 rpm, and then added to 300 g of water at 60°C and stirred at 60 rpm for 30 min to obtain a wax-water mixture.
[0032] 20 g of silica powder with a particle size of 50 nm was slowly added to the wax-water mixture and ultrasonicated at a power of 60,000 Hz for 2 h to ensure the homogeneity of the system. Silica particles with a surface energy between the two liquids will be adsorbed to the liquid-liquid interface. It was then cooled to 25 °C to solidify the wax phase and lock the particles in place. Subsequently, 30 g of urethane silane (AMCS) was added to modify the surface of silica in the wax-water system for 4 h. After the modification was completed, urethane silane-modified silica was obtained by centrifugation, deionized water washing, and drying.
[0033] 100 g of low-density polyethylene and 1 g of initiator, hydrogen peroxide (H 2 O 2 ) and stirred at 300 rpm for 20 minutes to ensure that the initiator is evenly distributed in the monomer. After uniform mixing, the polymerization reaction was carried out at 90 °C for 10 hours. After the reaction was completed, the product was taken out from the reactor, filtered, washed, dried and crushed after precipitation to obtain polyethylene polymer.
[0034] 30 g of urethane silane-modified silica was mixed with 100 g of polyethylene matrix and reacted at 220 °C for 3 h to obtain polyethylene containing modified silica, which was then processed into a flocculant by melt extrusion. During the melt extrusion process, the temperature was controlled at 230 °C to fully mix the modified silica and polyethylene. At the same time, the speed of the extruder was adjusted to 500 rpm and the processing pressure was controlled to 1.5 MPa to ensure the structural stability and performance reliability of the flocculant.
[0035] In order to further improve the removal efficiency of heavy metal ions, 240 ml of 30 g / L thioglycolic acid (MEA) was mixed with 10 g of flocculant. The unmodified surface of silica was fully contacted with MEA to introduce thiol functional groups. The mixture was reacted at 40 °C for 3 h and stirred at 220 rpm to obtain thioglycolic acid modified flocculant.
[0036] Comparative Example 1 100 g of low-density polyethylene and 0.5 g of initiator, hydrogen peroxide (H 2 O 2 ) and stirred at 250 rpm for 15 minutes to ensure that the initiator is evenly distributed in the monomer. After uniform mixing, the polymerization reaction was carried out at 85 °C for 9 hours. After the reaction was completed, the product was taken out from the reactor, filtered, washed, dried and crushed after precipitation to obtain polyethylene polymer. Take 10 g of polyethylene polymer, add 220 ml of 25 g / L thioglycolic acid (MEA) and mix, react at 30 °C for 2.5 hours, and stir at a stirring speed of 210 rpm to obtain a flocculant.
[0037] Test example The wastewater treatment effects of the thioglycolic acid modified flocculants prepared in Examples 1-3, the polyethylene polymer not mixed with silicon dioxide in Example 1, the flocculant not modified with thioglycolic acid in Example 1, and the commercially available polyethyleneimine flocculant were tested.
[0038] Method: Taking an industrial wastewater as a sample, 0.01 g of the performance-enhanced flocculants prepared in Examples 1-3, the polyethylene polymer of Example 1 without silica mixing, the flocculant of Example 1 without thioglycolic acid modification, and the commercially available polyethyleneimine flocculant were added to 100 ml of the industrial wastewater, respectively, and stirred at 300 rpm for 30 min. The Cu 2+ , Pb 2+ Cr 3 + 、Zn 2+ 、Cd 2+ And the removal rate of chemical oxygen content (COD), the specific results are shown in Table 1.
[0039] Table 1 Performance enhanced flocculants prepared in Examples 1-3 Cu in industrial wastewater 2+ , Pb 2+ Cr 3+ 、Zn 2+ 、Cd 2+ , COD removal rate As shown in Table 1, the flocculant prepared by the present invention without modification of thioglycolic acid has an effect on the removal of Cu in industrial wastewater. 2+ , Pb 2+ Cr 3+ 、Zn 2+ 、Cd 2+ , COD removal rate is better than that of commercially available polyvinyl amide flocculants. The flocculant modified by thioglycolic acid in the present invention has a significant effect on the removal of Cu in industrial wastewater. 2+ , Pb 2+ Cr 3+ 、Zn 2+ 、Cd 2+ , and COD removal rate are significantly better than those of commercially available polyacrylamide flocculants.
Claims
1. A flocculant for industrial wastewater treatment, characterized in that: The invention is composed of urethane silane, silicon dioxide and polyethylene polymer in a mass ratio of 2-3:1-2:
10.
2. The flocculant according to claim 1, characterized in that: The flocculant also includes thioglycolic acid.
3. The method for preparing the flocculant according to claim 1, characterized in that: To do this, follow these steps: 1) Urethane silane modified silica: Add silica powder to a wax-water mixture at 60-70°C and ultrasonically treat at a power of 50000-60000 Hz for 1-2 h, then cool to room temperature, add urethane silane, and continue stirring for 3-4 h; then, centrifuge, wash with deionized water, and dry to obtain modified silica; 2) The modified silica and polyethylene polymer are mixed in a ratio of 2-3:10, reacted at 200-220°C for 2-3h to obtain polyethylene containing modified silica, and then the polyethylene containing modified silica is processed by a melt extrusion method to obtain a target flocculant; during the melt extrusion process, the temperature is controlled at 210-230°C, the extruder speed is 300-500 rpm, and the processing pressure is 0.5-1.5 MPa.
4. The method for preparing a flocculant according to claim 3, characterized in that: In step 2), the preparation method of the polyethylene polymer is to mix low-density polyethylene and an initiator in a ratio of 100:0.1-1, stir at a speed of 200-300 rpm for 10-20 minutes, and then polymerize at 80-90°C for 8-10 hours. The obtained precipitate is filtered, washed, dried and crushed to obtain a polyethylene polymer.
5. The method for preparing a flocculant according to claim 3, characterized in that: In step 1), the wax-water mixture is prepared by melting paraffin wax and adding it into water at 60-70° C., stirring evenly to obtain the wax-water mixture, wherein the mass ratio of paraffin wax to water is 1:
3.
6. The method for preparing a flocculant according to claim 4, characterized in that: In step 2), the initiator is hydrogen peroxide.
7. The method for preparing a flocculant according to claim 3, characterized in that: Add 20-30 g / L thioglycolic acid to the flocculant obtained in step 2), mix well, react at room temperature for 2-3 h and stir at a stirring speed of 200-220 rpm to obtain a thioglycolic acid modified flocculant; The mass volume ratio of the flocculant to the thioglycolic acid is 1:22-24 g / ml.
Citation Information
Patent Citations
Preparing method for sulfhydrylation polyacrylamide heavy metal flocculant
CN105668752A
Silicone silica compositions
GB1366459A
Oil press
KR1020250012303A
Silicone-silica compositions
US3810843A