Preparation method of fluorescent solar concentrating microcrystalline glass
The fluorescent solar-concentrating crystallized glass is prepared through high-temperature melting-annealing crystallization method, which solves the problems of complex preparation and poor stability of fluorescent materials, realizes efficient and environmentally friendly fluorescent solar-concentrating crystallized glass, and improves the luminous efficiency and Stable and suitable for industrial production.
Patent Information
- Application Number
- CN202410851113.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
AI Technical Summary
The preparation methods of fluorescent materials in existing fluorescent solar concentrators are complicated, the materials have poor stability, low quantum yield, poor purity and uniformity, and traditional materials use toxic chemicals, which limits their application scope and industrial production.
Fluorescent solar-concentrating glass-ceramics are prepared using a high-temperature melting-annealing crystallization method. The mixed powders of B2O3-SiO2-ZnO, all-inorganic boron halide-based perovskite, and copper-based halide perovskite are melted and annealed at high temperature. An efficient and stable fluorescent material is formed, and combined with polishing treatment, crystallized glass with high luminous efficiency and stability is prepared.
A fluorescent solar concentrator glass-ceramic with high luminous efficiency, uniform morphology, high light transmittance and good stability has been achieved. The fluorescence quantum yield reaches more than 90%. The material is environmentally friendly and suitable for large-scale industrial production.
Smart Images

Figure HDA0004916849370000011 
Figure HDA0004916849370000012 
Figure HDA0004916849370000013
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing fluorescent solar energy concentrating microcrystalline glass, and belongs to the field of preparation of novel photovoltaic power generation devices. Background Art
[0002] Luminescent Solar Concentrators (LSC) are devices used to collect and utilize solar energy. They convert sunlight into fluorescence through special fluorescent materials, and then guide the fluorescence to the edge of the concentrator for photoelectric conversion through solar cells. The device is expected to become an important part of BIPV technology. LSC can not only concentrate light from a large area onto a small area of solar thin-film cells, but also, unlike traditional solar concentrators, it does not need to track sunlight to match the angle, so it can use sunlight more efficiently. LSC reduces the cost of photovoltaic power generation by reducing the area of photovoltaic materials used, and can be "invisibly" integrated into translucent photovoltaic glass systems, becoming part of beautiful urban buildings. It provides electricity for buildings while maintaining people's quality of life. It is a very promising green urban energy technology.
[0003] At present, the factors that affect the performance of fluorescent solar concentrators (LSCs) include the selection and performance of matrix materials, optical waveguide design, self-absorption and optical loss, temperature effects, light concentration and coupling efficiency, and manufacturing processes. One of the most important factors is the preparation of fluorescent materials. Current research is also mainly focused on the development of new fluorescent materials to improve the conversion efficiency and stability of LSCs, reduce costs, and expand the scope of application.
[0004] The preparation method of fluorescent materials for fluorescent solar concentrators (LSC) mainly has the following difficulties and problems:
[0005] 1. Complex synthesis methods: The preparation of efficient and stable fluorescent materials usually requires complex chemical synthesis processes, which include high temperature and high pressure conditions, complex precursors and solvent systems.
[0006] 2. Poor material stability: Fluorescent materials need to have good stability in practical applications, especially under conditions such as lighting, temperature changes, and chemical environments. Some fluorescent materials may experience light attenuation or degradation during long-term use, affecting their performance.
[0007] 3. Low quantum yield: Quantum yield is an important indicator to measure the efficiency of fluorescent materials, and materials with high quantum yield are difficult to prepare.
[0008] 4. Poor material purity and uniformity: The performance of fluorescent materials is highly dependent on their purity and uniformity. Impurities or uneven materials may cause reduced fluorescence efficiency or changes in luminescent color.
[0009] 5. Limited scope of application: Traditional fluorescent materials such as phosphors and quantum dots may use toxic or harmful chemicals during the preparation process, which poses potential risks to the environment and human health.
[0010] In response to the above problems, current research is mainly focused on the development of new fluorescent materials. In the prior art, some technicians have prepared more excellent focusing microcrystalline glass to make its microstructure, light transmittance, thermal stability and radiation stability better, and then obtained fluorescent solar focusing microcrystalline glass based on non-lead metal halide with high luminous efficiency, uniform morphology, high light transmittance and good stability. However, the existing methods for preparing fluorescent solar focusing microcrystalline glass cannot be used for large-scale industrial production. Summary of the invention
[0011] The present invention proposes a method for preparing fluorescent solar concentrating microcrystalline glass, which adopts a high-temperature melting-annealing crystallization method to prepare solar concentrating microcrystalline glass. This concentrating microcrystalline glass can absorb a part of the transmitted light, and then transmit it to the edge of the glass in the form of visible light and infrared light, providing a new idea for generating electricity at the edge of the glass. In addition, the concentrating microcrystalline glass also has a filtering and energy-saving effect, absorbs the energy in the sunlight, can effectively reduce the indoor temperature in the hot summer, and at the same time reduces the sunlight reflection of the building curtain wall, effectively reducing light pollution, assembling solar cells around the microcrystalline glass, absorbing the fluorescence converted by fluorescence and waveguided to the edge of the glass, and generating electricity.
[0012] The technical solution of the present invention is as follows:
[0013] A method for preparing fluorescent solar concentrating glass-ceramics, the specific steps are as follows:
[0014] (1) Accurately weigh B2O3-SiO2-ZnO, all-inorganic boron halide perovskite, and copper-based halide perovskite, and grind the raw materials using an agate mortar and pestle for 10-15 minutes to fully physically mix to obtain a mixed powder;
[0015] (2) transferring the mixed powder of step (1) into a crucible, and then placing the crucible into a high-temperature box furnace for high-temperature melting, and then pouring the melt onto a preheated stainless steel plate, and then pressing a preheated copper plate onto the melt, and obtaining a prefabricated precursor glass after cooling, and annealing the prefabricated precursor glass to release thermal stress, thereby forming a precursor glass (PG);
[0016] (3) The precursor glass (PG) sample is processed into the required specifications by a diamond cutting machine, and then ground to a certain thickness on a polishing machine using a cast iron grinding wheel. Finally, it is polished on the polishing wheel using cerium oxide polishing liquid to obtain a focusing microcrystalline glass sample of suitable size.
[0017] Step (1) B2O3-SiO2-ZnO, all-inorganic boron halide perovskite, and copper-based halide perovskite are all commercially available products.
[0018] Step (1) Sampling is performed in a molar ratio of B2O3-SiO2-ZnO: all-inorganic boron halide perovskite: copper-based halide perovskite of 1:1 to 1.2:1 to 1.5.
[0019] The high temperature melting in step (2) is carried out in a high temperature box furnace at 1400-1500° C. in an ambient atmosphere for 40-50 minutes.
[0020] Step (2) Preheat the stainless steel plate and the copper plate to 350-500°C.
[0021] Step (3) Annealing: Anneal in a muffle furnace at 450-500° C. for 6-9 hours.
[0022] The beneficial effects of the present invention are:
[0023] (1) The preparation process of the present invention is simple, and the obtained solar concentrating microcrystalline glass has high luminous efficiency, uniform morphology, high light transmittance and good stability.
[0024] (2) The preparation method of the present invention is simple and low in cost.
[0025] (3) The fluorescent quantum yield (PLQY) of the concentrating microcrystalline glass prepared by the present invention, that is, the absorption of sunlight and conversion or emission into light within a certain visible wavelength range, enables the glass edge solar film cells to achieve efficient absorption and conversion of sunlight within the visible spectrum range. The fluorescent quantum yield is more than 90% and the Stokes shift reaches 300-800nm.
[0026] (4) The fluorescent solar concentrating glass-ceramics prepared by the present invention can be used to generate electricity and can absorb infrared light to reduce indoor temperature and can also convert the absorbed infrared light into visible light to be absorbed by the solar substrate for power generation.
[0027] (5) The raw materials and process used in the present invention are environmentally friendly, will not cause harm to the environment, and are in line with the concept of sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a flow chart for preparing the light-concentrating glass-ceramics of the present invention;
[0029] Figure 2 This is a photo of the light-concentrating glass-ceramics of Example 3 of the present invention;
[0030] Figure 3 The wavelength spectrum of the emitted light detected by the ultraviolet-visible-near-infrared spectrophotometer of the focusing micro-ceramic glass in Example 3 of the present invention. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with specific implementation modes, but the protection scope of the present invention is not limited to the described contents.
[0032] The all-inorganic boron halide-based perovskite and copper-based halide perovskite in the raw materials are prepared by referring to the published document "Reproducible X-ray Imaging with a Perovskite Nanocrystal ScintillatorEmbedded in a Transparent Amorphous Network Structure".
[0033] Example 1
[0034] A method for preparing fluorescent solar concentrating glass-ceramics, such as Figure 1 As shown, the specific steps are as follows:
[0035] (1) accurately weighing B2O3-SiO2-ZnO, all-inorganic boron halide perovskite, and copper-based halide perovskite in a molar ratio of 1:1:1 of B2O3-SiO2-ZnO: all-inorganic boron halide perovskite: copper-based halide perovskite, and grinding the raw materials with an agate mortar and pestle for 10 minutes to fully physically mix to obtain a mixed powder;
[0036] (2) transferring the mixed powder of step (1) into a crucible, and then placing the crucible into a high-temperature box furnace, melting it in an ambient atmosphere of 1400° C. for 40 min, performing high-temperature melting, and then pouring the melt onto a stainless steel plate preheated to 350° C., and then pressing it with a copper plate preheated to 350° C., and after cooling, removing the stainless steel plate and the copper plate to obtain a prefabricated precursor glass, and annealing the prefabricated precursor glass in a muffle furnace at 450° C. for 9 h to release thermal stress, thereby forming a precursor glass (PG);
[0037] (3) The precursor glass (PG) sample is processed into the required specifications by a diamond cutting machine, and then ground to a certain thickness on a polishing machine using a cast iron grinding wheel. Finally, it is polished on the polishing wheel using cerium oxide polishing liquid to obtain a microcrystalline glass sample of suitable size.
[0038] Example 2
[0039] A method for preparing fluorescent solar energy concentrating glass-ceramics, such as Figure 1 As shown, the specific steps are as follows:
[0040] (1) accurately weighing B2O3-SiO2-ZnO, all-inorganic boron halide perovskite, and copper-based halide perovskite in a molar ratio of B2O3-SiO2-ZnO: all-inorganic boron halide perovskite: copper-based halide perovskite of 1:1.1:1.3, grinding the raw materials with an agate mortar and pestle for 12 minutes to fully physically mix and obtain a mixed powder;
[0041] (2) transferring the mixed powder of step (1) into a crucible, and then placing the crucible into a high-temperature box furnace, melting it in an ambient atmosphere of 1450° C. for 45 min, performing high-temperature melting, and then pouring the melt onto a stainless steel plate preheated to 450° C., and then pressing it with a copper plate preheated to 450° C., and after cooling, removing the stainless steel plate and the copper plate to obtain a prefabricated precursor glass, and annealing the prefabricated precursor glass in a muffle furnace at 500° C. for 6 h to release thermal stress, thereby forming a precursor glass (PG);
[0042] (3) The precursor glass (PG) sample is processed into the required specifications by a diamond cutting machine, and then ground to a certain thickness on a polishing machine using a cast iron grinding wheel. Finally, it is polished on the polishing wheel using cerium oxide polishing liquid to obtain a microcrystalline glass sample of suitable size.
[0043] Example 3
[0044] A method for preparing fluorescent solar concentrating glass-ceramics, such as Figure 1 As shown, the specific steps are as follows:
[0045] (1) accurately weighing B2O3-SiO2-ZnO, all-inorganic boron halide perovskite, and copper-based halide perovskite in a molar ratio of B2O3-SiO2-ZnO: all-inorganic boron halide perovskite: copper-based halide perovskite of 1:1.2:1.5, grinding the raw materials with an agate mortar and pestle for 15 minutes to fully physically mix to obtain a mixed powder;
[0046] (2) transferring the mixed powder of step (1) into a crucible, and then placing the crucible into a high-temperature box furnace, melting it in an ambient atmosphere of 1500° C. for 50 min, performing high-temperature melting, and then pouring the melt onto a stainless steel plate preheated to 500° C., and then pressing it with a copper plate preheated to 500° C., and after cooling, removing the stainless steel plate and the copper plate to obtain a prefabricated precursor glass, and annealing the prefabricated precursor glass in a muffle furnace at 480° C. for 8 h to release thermal stress, thereby forming a precursor glass (PG);
[0047] (3) The precursor glass (PG) sample is processed into the required specifications by a diamond cutting machine, and then ground to a certain thickness on a polishing machine using a cast iron grinding wheel. Finally, it is polished on the polishing wheel using cerium oxide polishing liquid to obtain a focusing microcrystalline glass sample of suitable size.
[0048] like Figure 2 The photo shown is of the focusing microcrystalline glass obtained in Example 3. From the photo, it can be seen that when the light beam is irradiated to the glass surface, the material absorbs the light energy and then refracts it to the edge of the glass. Solar power generation strips are arranged on the edge of the glass to generate electricity.
[0049] The wavelength range of the light emitted by the light-concentrating micro-ceramics prepared in Example 3 was measured using a Hitachi U-4100 UV-visible-near-infrared spectrophotometer. Figure 3 As shown in the figure, it can be seen that the emitted light can be detected at 300nm-800nm, and the fluorescence quantum yield is more than 90%.
[0050] Take the concentrating microcrystalline glass sample prepared in Example 3, install solar thin-film cells around the concentrating microcrystalline glass, and assemble the concentrating microcrystalline glass and the solar thin-film cells into a new fluorescent solar concentrator (LSC) by gluing or crimping. After the assembly is completed, the concentrating microcrystalline glass reflects sunlight to the solar thin-film cells and converts it into electrical energy. The concentrating microcrystalline glass of the present invention concentrates light from a large area onto a solar thin-film cell with a small area. Unlike traditional solar concentrators, which need to track sunlight to match the angle, it can utilize sunlight more efficiently.
[0051] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A method for preparing fluorescent solar concentrating glass-ceramics, characterized in that: The specific steps are as follows: (1) Accurately weigh B2O3-SiO2-ZnO, all-inorganic boron halide perovskite, and copper-based halide perovskite, and grind the raw materials for 10-15 minutes to obtain a mixed powder; (2) melting the mixed powder of step (1) at high temperature, pouring the melt onto a preheated stainless steel plate, pressing a preheated copper plate onto the melt, cooling to obtain a prefabricated precursor glass, and annealing the prefabricated precursor glass to form a precursor glass; (3) Processing the precursor glass into the required specifications, and then grinding and polishing it to obtain focusing microcrystalline glass.
2. The method for preparing fluorescent solar concentrating glass-ceramics according to claim 1, characterized in that: Step (1) The molar ratio of B2O3-SiO2-ZnO, all-inorganic boron halide perovskite, and copper-based halide perovskite is 1:1-1.2:1-1.
5.
3. The method for preparing fluorescent solar concentrating glass-ceramics according to claim 1, characterized in that: The high temperature melting in step (2) is performed at 1400-1500° C. for 40-50 minutes.
4. The method for preparing fluorescent solar concentrating glass-ceramics according to claim 1, characterized in that: Step (2) Preheat the stainless steel plate and the copper plate to 350-500°C.
5. The method for preparing fluorescent solar concentrating glass-ceramics according to claim 1, characterized in that: Step (3) annealing at 450-500° C. for 6-9 hours.